Precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs (Volatile Organic Compounds) as well as preparation method and application of noble metal reduction catalyst
By using low silicon-to-aluminum ratio molecular sieves and macroporous alumina to support transition metals and rare earth metals in VOCs catalysts, the problem of catalyst deactivation due to silica coverage is solved, extending the service life and reducing costs.
Patent Information
- Application Number
- CN202410916374.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
AI Technical Summary
When dealing with existing VOCs catalysts containing organosilicon, they are easily deactivated due to silica crystal coverage, leading to pore blockage, and are complicated and costly to manufacture.
Low silicon to aluminum ratio molecular sieve and macroporous alumina are used as carriers to load transition metals, rare earth metals and precious metals through impregnation, avoiding pretreatment agents, using rare earth metal adsorption to decompose organic silicon, and capturing elemental silicon through macroporous alumina to extend Service life of precious metal catalysts.
It effectively avoids silica coverage, reduces the deactivation frequency of precious metal catalysts, extends the service life of the catalyst, reduces production costs, and improves the adsorption capacity of organic silicon.
Smart Images

Figure CN118719124A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of VOCs catalysts, and specifically relates to a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs, and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Volatile organic compounds (VOCs) are one of the main air pollutants, which can directly cause photochemical smog and aggravate haze pollution, endangering human health. In practical applications, VOCs catalysts are mainly precious metal catalysts. Then when organic silicon is contained in the actual working conditions, silicon dioxide crystals are often generated to cover the catalytic surface, block the pores, cover the silicon metal active sites, and accelerate the deactivation of the precious metal catalyst. In response to this phenomenon, there are a few coping methods, which are to set a pretreatment agent in front of the precious metal catalyst, for example: Patent CN 114100669 A discloses an extruded 400 mesh honeycomb silicon-containing VOCs pretreatment catalyst, including an aluminum-based carrier, an active component and other additives; Patent CN 115069277 A discloses an extruded spherical granular or spherical mesoporous through-granular VOCs pretreatment catalyst, including an aluminum-based carrier and an active component. Both of the above catalysts are used as pretreatment agents to selectively remove organic silicon from VOCs and protect the rear-end precious metal catalyst. However, its manufacturing is complex, the dosage of active ingredients is high, and the production cost is high, which greatly increases the cost of VOCs treatment.
[0004] Therefore, there is an urgent need to develop a catalyst that can effectively treat VOCs containing silicone to avoid the problem of silica crystals blocking the catalyst pores and causing its deactivation. Summary of the invention
[0005] In order to address the deficiencies of the prior art, the purpose of the present invention is to provide a precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs and its preparation method and application. When the catalyst provided by the present invention treats VOCs, there is no need to add front-end pretreatment agents or adsorbents and other materials.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] The first aspect of the present invention provides a method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs, comprising the following steps:
[0008] A low silicon-aluminum ratio molecular sieve with a silicon-aluminum ratio of 0.8-2 is prepared by using a silicon source and an aluminum source;
[0009] The noble metal oxide, the rare earth metal oxide, the transition metal oxide, the macroporous alumina and the binder are mixed in water and ground to obtain slurry A;
[0010] The low silicon-aluminum ratio molecular sieve and the binder are mixed in water and ground to obtain slurry B;
[0011] The slurry A is coated on the surface of the carrier by vacuum coating, and after drying, the slurry B is coated on the surface of the carrier by vacuum coating, dried, and calcined to obtain a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0012] The present invention provides a method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs, wherein a transition metal, a rare earth metal, a noble metal and a macroporous alumina are loaded on a carrier by an impregnation method, a low silicon-aluminum ratio molecular sieve (which is a low silicon-aluminum ratio MCM-41 molecular sieve) with a silicon-aluminum ratio of 0.8-2 is prepared by a simple process, and then the low silicon-aluminum ratio molecular sieve is loaded on the surface of the carrier by an impregnation method, and then dried and calcined. In actual working conditions, the catalyst for catalytic oxidation of silicon-containing VOCs is consistent with the use method of existing conventional catalysts, and there is no need to add materials such as front-end pretreatment agents or adsorbents. Rare earth metals adsorb and decompose organosilicon macromolecules in VOCs into elemental silicon or small molecule silicon, and the elemental silicon or small molecule silicon is preferentially captured by aluminum sites in macroporous alumina and molecular sieves, reducing their contact with internal noble metals, reducing the frequency of catalyst replacement, and extending the service life of noble metal catalysts. Moreover, the impregnation method loads transition metals, rare earth metals, and precious metals, thereby preventing them from being embedded in the matrix, reducing the amount of transition metals, rare earth metals, and precious metals used, and lowering costs.
[0013] Specifically, the macroporous alumina crystal structure is diverse, and it has the characteristics of interconnected mesoporous macropores, high specific surface area, and two-dimensional or three-dimensional spatial pore structure. On the one hand, it promotes the transmission of guest molecules to active sites in the mesoporous pores and reduces the transmission resistance; on the other hand, it also helps to increase the adsorption and separation efficiency and prolong the catalytic life. The present invention uses the aluminum affinity of silicon to adsorb and capture it, reduces the impact on precious metals, and greatly prolongs the service life of precious metal catalysts. At the same time, because the low silicon-aluminum ratio molecular sieve has a rich pore structure and a large specific surface area, the secondary loading of the low silicon-aluminum ratio molecular sieve further improves its adsorption of silicon. In general, molecular sieves with a low silicon-aluminum ratio have good adsorption capacity for macromolecules, but poor adsorption capacity for small molecules; while molecular sieves with a high silicon-aluminum ratio have good adsorption performance for small molecules, but poor adsorption capacity for macromolecules. When the silicon-aluminum ratio increases, the positive charge in the molecular sieve decreases, and the adsorption capacity also decreases. For molecular sieves with the same pore size and morphology, the lower the silicon-aluminum ratio, the stronger the adsorption performance. Using alumina as a substrate to load transition metals, rare earth metals, and precious metals can not only make the distribution of metal elements more uniform, but also improve the overall catalytic performance of the catalyst by adding a low silicon-aluminum ratio molecular sieve coating. It also makes it easier to capture silicon elements and increase the capture amount, thereby extending the service life of the precious metal catalyst, reducing the frequency of replacement by the company, and reducing the cost of use.
[0014] In some embodiments of the present invention, the method for preparing the low silicon-aluminum ratio molecular sieve comprises the following steps:
[0015] Prepare a water glass solution as solution C;
[0016] Sodium oxide and aluminum oxide are mixed in a molar ratio of 2.4-2.6:1 and added into water to obtain a solution D after reaction; a surfactant is added into the solution D and the pH is adjusted to 9-11;
[0017] The solution C is added dropwise to the solution D with adjusted pH, and the ratio of silicon in solution C to aluminum in solution D is controlled to be 0.8-2; after the addition is completed, the solution is heated in a water bath for crystallization, and after cooling, filtered, washed and dried to obtain a molecular sieve with a low silicon-aluminum ratio.
[0018] The water bath temperature is 28-32°C for 3-5 hours; the crystallization temperature is 88-92°C for 5-8 hours.
[0019] In some embodiments of the present invention, the slurry A is composed of: based on the mass percentage of each raw material, transition metal oxide 3%-20%, rare earth metal oxide 5%-20%, precious metal 0.01%-1%, macroporous alumina 40%-70%, and the rest is a binder.
[0020] In some embodiments of the present invention, the slurry B is composed of: based on the mass percentage of each raw material, 50%-90% of the low silicon-to-aluminum ratio molecular sieve, and the rest is a binder.
[0021] In some embodiments of the present invention, the specific surface area of the macroporous alumina is 178-182 m 2 / g, pore diameter of 8-12nm, pore volume of 0.58-0.62cm 3 / g.
[0022] In some embodiments of the present invention, the noble metal is at least one of platinum (Pt) and palladium (Pd); and the noble metal precursor is a salt of the noble metal.
[0023] Preferably, the platinum precursor is platinum nitrate.
[0024] Preferably, the palladium precursor is palladium nitrate.
[0025] In some embodiments of the present invention, the rare earth metal oxide is cerium oxide (CeO2), praseodymium oxide (Pr6O 11 ), at least one of lanthanum oxide (La2O3).
[0026] In some embodiments of the present invention, the transition metal oxide is at least one of manganese oxide (MnO2), cobalt oxide (Co3O4), and iron oxide (Fe2O3).
[0027] In some embodiments of the present invention, the binder is silica sol or alumina sol.
[0028] In some embodiments of the present invention, the grinding can be performed by a horizontal grinder. Specifically, the grinding temperature is 3°C-25°C, the grinding speed is 300r / min-1500r / min, the grinding time is 0.5h-5h, and the particle size D90 of the slurry obtained after grinding is 1μm-5μm, and the viscosity is 10mPa·S-200mPa·S.
[0029] In some embodiments of the present invention, the carrier is a cordierite honeycomb ceramic carrier. The cordierite honeycomb ceramic carrier is mainly composed of more than 90% cordierite crystals, has excellent compressive strength, thermal shock resistance and low thermal expansion coefficient, and can meet the application of most industrial VOCs catalytic combustion processes.
[0030] Preferably, the number of openings in the cross section of the cordierite honeycomb ceramic carrier is 100-600 meshes. In addition, in order to meet the requirements of the space design of engineering equipment during use, the cordierite honeycomb ceramic carrier structure is a cuboid, a cube or a cylinder. Specifically, when the carrier is a cuboid or a cube, its length, width and height can be 100mm-200mm, 100mm-200mm, 40mm-200mm, for example: the length, width and height are 100mm, 100mm, 50mm, etc.; when the cordierite honeycomb ceramic carrier is a cylinder, its diameter and height are 100mm-330mm, 100mm-200mm, for example, the diameter and height are 330mm and 150mm, respectively.
[0031] In some embodiments of the present invention, a bottom-feed vacuum coating device is used to coat the slurry on the surface of the cordierite honeycomb ceramic carrier.
[0032] Wherein, the vacuum degree of the lower feeding vacuum coating is 0.1MPa-0.5MPa, and the number of vacuum coating is 2-4 times.
[0033] In some embodiments of the present invention, the drying temperature is 80° C.-120° C. and the time is 0.1 h-0.5 h.
[0034] In some embodiments of the present invention, the calcination temperature is 450° C.-600° C. and the time is 1 h-5 h.
[0035] The second aspect of the present invention provides a precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs, which is prepared by the above-mentioned preparation method;
[0036] The catalyst for catalytic oxidation of silicon-containing VOCs consists of a carrier and a coating coated on the surface of the carrier, the coating loading is 80g / L-250g / L, and the noble metal loading is 200g / m 3 -700 g / m 3 The total coating loading of the two layers (coating mass g / carrier volume calculation L) is 80g / L-250g / L, and the precious metal loading (precious metal Pt, Pd total mass g / carrier volume calculation m 3 ) is 200g / m 3 -700g / m 3 The present invention increases the resistance to silicon-containing organic waste gas while maintaining a low coating shedding rate, thereby extending the service life of the catalyst and reducing the use cost of the enterprise.
[0037] The third aspect of the present invention provides an application of the above-mentioned precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs in VOCs treatment.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The present invention uses macroporous alumina as a matrix to load precious metals, rare earth metals and transition metals. It has a high specific surface area and rich pore structure, which is conducive to the dispersion of the active components of the catalyst and reduces the coverage of the active sites by silicon oxide formed after the oxidation of organosilicon; at the same time, it is conducive to the entry of VOCs molecules into the catalyst pores, increasing the contact area between VOCs molecules and the active sites, thereby effectively improving the activity of the catalyst and the resistance to organosilicon poisoning. After the present invention loads a layer of active components on the carrier, it is coated with a layer of low silicon-aluminum ratio molecular sieve, because it has a larger aluminum element ratio and specific surface area, it has excellent adsorption performance for organosilicon, can achieve the capture of organosilicon by the outer layer of the catalyst, and avoid the coverage of the active sites by silicon oxide formed after the oxidation of organosilicon; at the same time, the rich pore structure and large pore volume of the molecular sieve can allow VOCs molecules to normally enter the catalyst reaction layer to participate in the reaction, thereby extending the service life of the catalyst.
[0040] The present invention uses a conventional coating method for the preparation, grinding and coating of the slurry, which is easier to produce, reduces the use of substrates, and saves a lot of manpower and costs compared to extrusion or other forms of pre-pretreatment agents. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0042] Figure 1 is a catalytic activity decay diagram of the noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs prepared in Examples 1-6;
[0043] Figure 2 It is a catalytic activity decay diagram of the precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs prepared in Example 1 and Comparative Examples 1-3. DETAILED DESCRIPTION
[0044] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0045] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are explanations of the present invention rather than limitations. In the embodiments, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0046] In the following examples, the content of silica sol and aluminum sol is 25%. The concentration of platinum nitrate solution and palladium nitrate solution is 10%-20%, by mass percentage, and because the amount of both is relatively low, they are ignored in the calculation of solid content.
[0047] The solid content of the present invention is defined as the ratio of the mass of the solid obtained after the mixed slurry is calcined to the mass of the mixed slurry. The calculation formula of the solid content in the mixed slurry A is as follows:
[0048] Solid content = (m a +m b +m c +m d +m e ×25%) / 10000×100%
[0049] The total mass of macroporous alumina is denoted as m a ; The mass of the low silicon-aluminum ratio molecular sieve is denoted as m b ; The total mass of the transition metal oxide is denoted as m c ; The total mass of rare earth metal oxides is denoted as m d ; The mass of silica sol / alumina sol is recorded as m e .
[0050] The calculation formula of the solid content in the mixed slurry B is as follows:
[0051] Solid content = (m b +m e ×25%) / (m b +m e +m f )×100%
[0052] Among them, the mass of the low silicon-aluminum ratio molecular sieve is recorded as m b ; The mass of silica sol / alumina sol is recorded as m e , the mass of water is denoted as m f .
[0053] Example 1
[0054] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0055] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of macroporous alumina (specific surface area 180m 2 / g, pore diameter 10nm, pore volume 0.6cm 3 / g), 312.5g of cerium oxide, 300g of praseodymium oxide, 243.5g of manganese oxide, 245g of cobalt oxide, 124g of iron oxide, and 438g of aluminum sol were placed in 6227g of water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0056] Step 2: The mixed slurry A in step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 93.3 mPa·S.
[0057] Step 3: The slurry obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom-feed vacuum coating device, the coating vacuum is 0.3 MPa, and the coating frequency is 1 time. After coating, it is dried at 100° C. for 0.5 h to obtain a once-coated macroporous alumina precious metal catalyst.
[0058] Step 4: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution C; prepare aluminum hydroxide solution D according to n(Na2O) / n(AI2O3)=2.5. Mix hexadecyltrimethylammonium bromide and solution D in deionized water while stirring, adjust the pH value to 9, add solution C dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution C to aluminum in solution D to be 0.8. Place the obtained mixed solution in a water bath, age at 30°C for 4h, and crystallize at 90°C for 7h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).
[0059] Step 5: Take 300 g of the low silicon-aluminum ratio molecular sieve (silicon-aluminum ratio is 0.8) prepared in step 4 and 200 g of aluminum sol, place them in 670 g of deionized water and stir them thoroughly to obtain a mixed slurry B with a solid content of 30%.
[0060] Step 6: The slurry B obtained in step 5 is coated on the once-coated macroporous alumina noble metal catalyst obtained in step 3 by a bottom-feed vacuum coating device, the coating vacuum is 0.3Mpa, and the coating frequency is 1. After coating, it is dried at 100°C for 0.5h and calcined at 500°C for 5h to obtain a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0061] Example 2
[0062] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0063] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of conventional alumina (specific surface area 160m 2 / g, pore diameter 7nm, pore volume 0.42cm3 / g), 312.5g of cerium oxide, 300g of praseodymium oxide, 243.5g of manganese oxide, 245g of cobalt oxide, 124g of iron oxide, and 438g of aluminum sol were placed in 6227g of water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0064] Step 2: The mixed slurry A in step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 92.1 mPa·S.
[0065] Step 3: The slurry obtained in step 2 is coated on a 200 mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom feeding vacuum coating device, the coating vacuum is 0.3 MPa, and the coating frequency is 1 time. After coating, it is dried at 100°C for 0.5 h to obtain a single-coated conventional alumina noble metal catalyst.
[0066] Step 4: Dissolve a certain amount of water glass in deionized water and stir well to form solution C. Prepare aluminum hydroxide solution D according to n(Na2O) / n(AI2O3)=2.5. Mix hexadecyltrimethylammonium bromide and solution D in deionized water while stirring, adjust the pH value to 9, add solution C dropwise to the above solution and stir well, and control the ratio of silicon in solution C to aluminum in solution D to be 0.8. Place the obtained mixed solution in a water bath, age at 30°C for 4h, crystallize at 90°C for 7h, filter, wash and dry the reaction product after cooling to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).
[0067] Step 5: Take 300 g of the low silicon-aluminum ratio molecular sieve (silicon-aluminum ratio is 0.8) prepared in step 4 and 200 g of aluminum sol, place them in 670 g of deionized water and stir them thoroughly to obtain a mixed slurry B with a solid content of 30%.
[0068] Step 6: The slurry B obtained in step 5 is coated on the conventional alumina noble metal catalyst obtained in step 3 by a bottom feeding vacuum coating device, the coating vacuum is 0.3Mpa, and the coating number is 1. After coating, it is dried at 100°C for 0.5h and calcined at 500°C for 5h to prepare a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0069] Example 3
[0070] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0071] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of mesoporous alumina (specific surface area 160m 2 / g, pore diameter 9nm, pore volume 0.5cm3 / g), 312.5g of cerium oxide, 300g of praseodymium oxide, 243.5g of manganese oxide, 245g of cobalt oxide, 124g of iron oxide, and 438g of aluminum sol were placed in 6227g of water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0072] Step 2: The mixed slurry A in step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 92.1 mPa·S.
[0073] Step 3: The slurry obtained in step 2 is coated on a 200 mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom feeding vacuum coating device, the coating vacuum degree is 0.3 MPa, and the coating frequency is 1 time. After coating, it is dried at 100° C. for 0.5 h to obtain a single-coated mesoporous alumina noble metal catalyst.
[0074] Step 4: Dissolve a certain amount of water glass in deionized water and stir well to form solution C. Prepare aluminum hydroxide solution D according to n(Na2O) / n(AI2O3)=2.5. Mix hexadecyltrimethylammonium bromide and solution D in deionized water while stirring, adjust the pH value to 9, add solution C dropwise to the above solution and stir well, and control the ratio of silicon in solution C to aluminum in solution D to be 0.8. Place the obtained mixed solution in a water bath, age at 30°C for 4h, crystallize at 90°C for 7h, filter, wash and dry the reaction product after cooling to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).
[0075] Step 5: Take 300 g of the low silicon-aluminum ratio molecular sieve (silicon-aluminum ratio is 0.8) prepared in step 4 and 200 g of aluminum sol, place them in 670 g of deionized water and stir them thoroughly to obtain a mixed slurry B with a solid content of 30%.
[0076] Step 6: The slurry B obtained in step 5 is coated on the conventional alumina noble metal catalyst obtained in step 3 by a bottom feeding vacuum coating device, the coating vacuum is 0.3Mpa, and the coating number is 1. After coating, it is dried at 100°C for 0.5h and calcined at 500°C for 5h to prepare a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0077] Example 4
[0078] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0079] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of macroporous alumina (specific surface area 180m 2 / g, pore diameter 10nm, pore volume 0.6cm 3 / g), 312.5g of cerium oxide, 300g of praseodymium oxide, 243.5g of manganese oxide, 245g of cobalt oxide, 124g of iron oxide, and 438g of aluminum sol were placed in 6227g of water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0080] Step 2: The mixed slurry A in step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 90.7 mPa·S.
[0081] Step 3: The slurry obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom feeding vacuum coating device, the coating vacuum is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100° C. for 0.5 h and calcined at 500° C. for 5 h to prepare a precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0082] Example 5
[0083] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0084] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of mesoporous alumina (specific surface area 160m 2 / g, pore diameter 9nm, pore volume 0.5cm 3 / g), 312.5g of cerium oxide, 300g of praseodymium oxide, 243.5g of manganese oxide, 245g of cobalt oxide, 124g of iron oxide, and 438g of aluminum sol were placed in 6227g of water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0085] Step 2: The mixed slurry A of step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 90.7 mPa·S.
[0086] Step 3: The slurry obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom feeding vacuum coating device, the coating vacuum is 0.3 Mpa, and the coating frequency is 1 time. After coating, it is dried at 100° C. for 0.5 h and calcined at 500° C. for 5 h to prepare a precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0087] Example 6
[0088] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0089] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of conventional alumina (specific surface area 160m 2 / g, pore diameter 7nm, pore volume 0.42cm 3 / g), 312.5g of cerium oxide, 300g of praseodymium oxide, 243.5g of manganese oxide, 245g of cobalt oxide, 124g of iron oxide, and 438g of aluminum sol were placed in 6227g of water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0090] Step 2: The mixed slurry A in step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 90.7 mPa·S.
[0091] Step 3: The slurry A obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom feeding vacuum coating device, the coating vacuum is 0.3 MPa, and the coating frequency is 1 time. After coating, it is dried at 100° C. for 0.5 h and calcined at 500° C. for 5 h to prepare a precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0092] Comparative Example 1
[0093] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0094] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of macroporous alumina (specific surface area 180m 2 / g, pore diameter 10nm, pore volume 0.6cm 3 / g), 312.5g of cerium oxide, 300g of praseodymium oxide, 243.5g of manganese oxide, 245g of cobalt oxide, 124g of iron oxide, and 438g of aluminum sol were placed in 6227g of water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0095] Step 2: The mixed slurry A in step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 93.3 mPa·S.
[0096] Step 3: The slurry obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom-feed vacuum coating device, the coating vacuum is 0.3 MPa, and the coating frequency is 1 time. After coating, it is dried at 100° C. for 0.5 h to obtain a once-coated macroporous alumina precious metal catalyst.
[0097] Step 4: Take 300g of commercial molecular sieve ZSM-5 (silicon-aluminum ratio is 20) and 200g of aluminum sol, place them in 670g of deionized water and stir them thoroughly to obtain a mixed slurry B with a solid content of 30%.
[0098] Step 5: The slurry B obtained in step 4 is coated on the once-coated macroporous alumina noble metal catalyst obtained in step 3 by a bottom-feed vacuum coating device, the coating vacuum is 0.3Mpa, and the coating frequency is 1. After coating, it is dried at 100°C for 0.5h and calcined at 500°C for 5h to obtain a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0099] Comparative Example 2
[0100] A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs comprises the following steps:
[0101] Step 1: Take 15g of platinum nitrate solution, 15g of palladium nitrate solution, and 2100g of macroporous alumina (specific surface area 180m 2 / g, pore diameter 10nm, pore volume 0.6cm 3 / g), 556g cerium oxide, 345g cobalt oxide, 324g iron oxide, and 438g aluminum sol were placed in 6227g water and stirred to obtain a mixed slurry A with a solid content of 35%.
[0102] Step 2: The mixed slurry A in step 1 was transferred to a grinder and ground at 500 rpm for 1 h at a grinding temperature of 20° C. The obtained grinding slurry had a particle size D90 of 3 μm-5 μm and a viscosity of 93.3 mPa·S.
[0103] Step 3: The slurry obtained in step 2 is coated on a 200-mesh cordierite honeycomb ceramic carrier with a length, width and height of 100 mm, 100 mm and 50 mm respectively by a bottom-feed vacuum coating device, the coating vacuum is 0.3 MPa, and the coating frequency is 1 time. After coating, it is dried at 100° C. for 0.5 h to obtain a once-coated macroporous alumina precious metal catalyst.
[0104] Step 4: Dissolve a certain amount of water glass in deionized water and stir thoroughly to form solution C; prepare aluminum hydroxide solution D according to n(Na2O) / n(AI2O3)=2.5. Mix hexadecyltrimethylammonium bromide and solution D in deionized water while stirring, adjust the pH value to 9, add solution C dropwise to the above solution and stir thoroughly, and control the ratio of silicon in solution C to aluminum in solution D to be 0.8. Place the obtained mixed solution in a water bath, age at 30°C for 4h, and crystallize at 90°C for 7h. After cooling, filter, wash and dry the reaction product to obtain molecular sieve raw powder (silicon-aluminum ratio of 0.8).
[0105] Step 5: Take 300 g of the low silicon-aluminum ratio molecular sieve (silicon-aluminum ratio is 0.8) prepared in step 4 and 200 g of aluminum sol, place them in 670 g of deionized water and stir them thoroughly to obtain a mixed slurry B with a solid content of 30%.
[0106] Step 6: The slurry B obtained in step 5 is coated on the once-coated macroporous alumina noble metal catalyst obtained in step 3 by a bottom-feed vacuum coating device, the coating vacuum is 0.3Mpa, and the coating frequency is 1. After coating, it is dried at 100°C for 0.5h and calcined at 500°C for 5h to obtain a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
[0107] Comparative Example 3
[0108] The extruded catalyst was prepared by citing the preparation process in invention patent CN 115069277 A. The catalyst components included, by weight, 50 parts of activated alumina, 3 parts of cerium oxide, 3 parts of praseodymium oxide, 4 parts of manganese oxide, 3 parts of cobalt oxide, 2 parts of iron oxide, 14 parts of molecular sieve (silicon-aluminum ratio 0.8), 8 parts of glycerol, and 10 parts of silica sol.
[0109] The following steps are involved:
[0110] Step 1: Take activated alumina powder (macroporous alumina), add cerium oxide, praseodymium oxide, manganese oxide, cobalt oxide, iron oxide, and molecular sieve (silicon-aluminum ratio 0.8) powder in sequence and stir well, add water, platinum solution, palladium solution, glycerol, and aluminum sol to the mixed powder, stir into a mass at room temperature, extrude the obtained mixture in an extruder, set the extrusion temperature to 150°C, and inject the extruded material into a cylindrical mold to obtain columnar particles.
[0111] Step 2: Take the columnar particles and calcine them in two steps. First, calcine them at about 300°C for 2 hours, then increase the temperature to about 500°C and continue calcining for 4 hours. Finally, take out the calcined columnar particles and cool them for 24 hours to obtain a catalyst.
[0112] Performance Verification:
[0113] The precious metal reduction catalysts for catalytic combustion of silicon-containing VOCs prepared in Examples 1-6 were tested. Sample size of precious metal reduction catalysts for catalytic combustion of silicon-containing VOCs: The prepared sample volume was 100*100*50mm, and the drilled test sample size was a cylinder of Φ30*50mm.
[0114] Test conditions: ethyl acetate: 1000ppm, tetraethyl silicate: 300ppm, volume space velocity: 15000h -1 .
[0115] Figure 1 It is a catalytic activity decay diagram of the precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs prepared in Examples 1-6.
[0116] During the coating process, the sample loading amount was controlled to be kept within the same range, and the activity decay diagram of 6 groups of samples prepared in the experiment is shown in Figure 6. Judging from the test results, the activity decay rate of the sample of Example 4 coated with macroporous alumina in catalytic oxidation of 300ppm tetraethyl silicate and 1000ppm ethyl acetate was lower than that of Example 5 and Example 6, indicating that the anti-silicon poisoning performance of the sample prepared by macroporous alumina is better than that of mesoporous and conventional alumina.
[0117] Compared with Examples 4-6, it is found that Example 1 (macroporous alumina + low silicon-aluminum ratio coating), Example 2 (mesoporous alumina + low silicon-aluminum ratio coating), and Example 3 (conventional alumina + low silicon-aluminum ratio coating) significantly reduce the catalyst activity decay rate by coating the low silicon-aluminum ratio molecular sieve for the second time. Among them, Example 1 (macroporous alumina + low silicon-aluminum ratio coating) has the best effect. In the exhaust gas containing 300ppm of tetraethyl silicate, the catalyst activity decays to 90% in about 160 minutes, and the complete deactivation time is about 290 minutes, which greatly prolongs the catalyst activity decay time and shows excellent anti-silicon poisoning performance.
[0118] Comparison and verification:
[0119] The precious metal reduction catalysts for catalytic combustion of silicon-containing VOCs prepared in Comparative Examples 1-3 were tested. Sample size of precious metal reduction catalysts for catalytic combustion of silicon-containing VOCs: The sample volume prepared in Comparative Examples 1 and 2 was 100*100*50mm, and the drilled test sample size was a cylinder of Φ30*50mm. Comparative Example 3 was an extruded particle catalyst, and samples of the same volume were taken for testing.
[0120] Test conditions: ethyl acetate: 1000ppm, tetraethyl silicate: 300ppm, volume space velocity: 15000h -1 .
[0121] Figure 2This is a catalytic activity decay diagram of the precious metal reduction catalyst for catalytic combustion of silicon-containing VOCs prepared in Comparative Examples 1-3.
[0122] Compared with Example 1, it was found that in Example 1, ZSM-5 molecular sieve (silicon-aluminum ratio of 20) was used, and the activity of the catalyst sample decreased rapidly, and it was completely deactivated in only 110 minutes, indicating that the sample had poor resistance to silicon poisoning. In Example 2, only three transition metal oxides, cerium oxide, cobalt oxide, and iron oxide, were added. The catalyst was completely deactivated in about 200 minutes, which was about 100 minutes different from the complete deactivation of Example 1 to which praseodymium oxide and manganese oxide were added. The sample in Example 3 had an initial conversion efficiency of only 95%, which was lower than the 99% conversion efficiency of Example 1, and the amount of raw materials added was more, and the activity decayed slightly faster than that of the sample in Example 1. Compared with the three groups of comparative examples, Example 1 showed the best catalytic performance of silicon-containing VOCs.
[0123] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs, characterized in that: The steps include: A low silicon-aluminum ratio molecular sieve with a silicon-aluminum ratio of 0.8-2 is prepared by using a silicon source and an aluminum source; The noble metal precursor, rare earth metal oxide, transition metal oxide, macroporous alumina and binder are mixed in water and ground to obtain slurry A; The low silicon-aluminum ratio molecular sieve and the binder are mixed in water and ground to obtain slurry B; The slurry A is coated on the surface of the carrier by vacuum coating, and after drying, the slurry B is coated on the surface of the carrier by vacuum coating, dried, and calcined to obtain a noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs.
2. The preparation method according to claim 1, characterized in that The preparation method of the low silicon-aluminum ratio molecular sieve comprises the following steps: Prepare a water glass solution as solution C; Sodium oxide and aluminum oxide are mixed in a molar ratio of 2.4-2.6:1 and added into water to obtain a solution D after reaction; a surfactant is added into the solution D and the pH is adjusted to 9-11; The solution C is added dropwise to the solution D with adjusted pH, and the ratio of silicon in solution C to aluminum in solution D is controlled to be 0.8-2; after the addition is completed, the solution is heated in a water bath for crystallization, and after cooling, filtered, washed and dried to obtain a molecular sieve with a low silicon-aluminum ratio.
3. The preparation method according to claim 2, characterized in that: The water bath has a temperature of 28-32°C and a time of 3-5h; The crystallization temperature is 88-92°C and the time is 5-8h.
4. The preparation method according to claim 1, characterized in that: The solid composition of the slurry A is: based on the mass percentage of each raw material, 3%-20% of transition metal oxide, 5%-20% of rare earth metal oxide, 0.01%-1% of noble metal, 40%-70% of macroporous alumina, and the rest is a binder; the solid composition of the slurry B is: based on the mass percentage of each raw material, 50%-90% of low silicon-aluminum ratio molecular sieve, and the rest is a binder; The specific surface area of the macroporous alumina is 178-182 m 2 / g, pore diameter of 8-12nm, pore volume of 0.58-0.62cm 3 / g.
5. The preparation method according to claim 1 or 4, characterized in that: The noble metal is at least one of platinum and palladium; the noble metal precursor is a salt of the noble metal; The rare earth metal oxide is at least one of cerium oxide, praseodymium oxide and lanthanum oxide; The transition metal oxide is at least one of manganese oxide, cobalt oxide and iron oxide; The binder is silica sol or alumina sol.
6. The preparation method according to claim 1, characterized in that: The carrier is a cordierite honeycomb ceramic carrier.
7. The preparation method according to claim 1, characterized in that: The drying temperature is 80°C-120°C and the time is 0.1h-0.5h.
8. The preparation method according to claim 1, characterized in that: The calcination temperature is 450°C-600°C and the time is 1h-5h.
9. A noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 8; The transition metal-loaded low silicon-aluminum ratio molecular sieve coated catalyst for silicon-containing VOCs consists of a carrier and a coating coated on the surface of the carrier, the coating loading is 80g / L-250g / L, and the noble metal loading is 200g / m 3 -700 g / m 3 .
10. Use of the noble metal reduction catalyst for catalytic combustion of silicon-containing VOCs as claimed in claim 9 in VOCs treatment.
Citation Information
Cited By
Red mud-based VOCs (volatile organic compounds) pretreating agent as well as preparation method and application thereof
CN119076003A
Silicon poisoning resistant catalyst and preparation method thereof
CN119869550A
A silicon poisoning-resistant catalyst and its preparation method
CN119869550B
High-temperature-resistant sulfur-resistant VOCs catalyst suitable for RTO and preparation method and application thereof
CN120054469A
A high-temperature-resistant sulfur-resistant VOCs catalyst suitable for RTO, and a preparation method and application thereof
CN120054469B