Flame retardant for environment-friendly paint and preparation method thereof
The environmentally friendly paint flame retardant prepared by mixing phosphorus and nitrogen flame retardants in a specific proportion and adding a coupling agent solves the problem of poor flame retardant effect in the existing technology and achieves efficient flame retardant effect and Thermal stability is improved.
Patent Information
- Application Number
- CN202410849763.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing flame retardants for wall paint have a single flame retardant component, poor flame retardant effect, and cannot effectively prevent the spread of flames.
An environmentally friendly flame retardant for paint is used, which is prepared by mixing phosphorus flame retardants and nitrogen flame retardants in a specific ratio, and adding a coupling agent for stirring, including phosphorus flame retardants such as phosphorus dioxide, trimer Phosphate esters and cyclophosphamide, as well as nitrogen-based flame retardants such as melamine and carbamide peroxide, form highly effective flame retardant compositions.
It has achieved a significant reduction in the amount of flame retardant added, reaching the UL94V-0 flame retardant grade, and improved thermal stability and flame retardant effects.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of flame retardants, and more specifically to a flame retardant for environmentally friendly paint and a preparation method thereof. Background Art
[0002] Flame retardants are chemicals that slow or stop the burning process of a material. Flame retardants generally work in the following ways: Gas phase inhibition: Flame retardants decompose at high temperatures to release gases that dilute the oxygen in the combustion zone, thereby inhibiting the combustion reaction. Reduction of heat release: Flame retardants can absorb heat and reduce the burning temperature of the material, reducing the generation and spread of flames. Formation of an inert shell: Some flame retardants form a layer of char on the surface of the material, which hinders the transmission of combustion gases and heat to the inside, thereby delaying the spread of fire. Catalytic reduction: The chemical components in flame retardants can catalyze specific reactions during the combustion process, reducing the reaction rate between fuel and oxygen.
[0003] Flame retardants in wall paint are mainly used to improve the fire resistance of the paint and reduce the flame spread rate and smoke generation in the event of a fire. Commonly used wall paint flame retardants can be inorganic flame retardants or organic flame retardants, depending on the formulation of the paint and the required fire protection level. Phosphorus flame retardants: Phosphorus flame retardants are common inorganic flame retardants that can form phosphides or phosphates at high temperatures, effectively slowing down the spread of flames and reducing the amount of harmful gases produced in fires. Nitrogen flame retardants: Nitrogen flame retardants can release inert gases at high temperatures, dilute the surrounding oxygen, and thus inhibit the combustion process. Fluorine-containing flame retardants: Fluorine-containing compounds can form a flame retardant layer on the surface of the material, reducing the spread of flames. Nano flame retardants: Nano materials such as nano alumina or nano silicon can form a barrier on the surface of the material to hinder the spread of combustion gases and heat.
[0004] However, the existing flame retardants for wall paints have a single flame retardant component and poor flame retardant effect. When a fire occurs, it cannot achieve effective flame retardancy. Therefore, research on flame retardants is very necessary. Summary of the invention
[0005] The purpose of the present invention is to provide a flame retardant for environmentally friendly paint to solve the technical problems existing in the above-mentioned background technology.
[0006] The technical solution of the present invention provides a flame retardant for environmentally friendly paint, comprising a phosphorus flame retardant and a nitrogen flame retardant, wherein the phosphorus flame retardant comprises the following components in parts by weight: 10-15 parts of phosphorus dioxide, 6-10 parts of tripolyphosphate, 3-7 parts of hexametaphosphate, 7-11 parts of cyclophosphamide, and 6-14 parts of phosphoric acid;
[0007] The nitrogen-based flame retardant comprises the following components in parts by weight: 9-15 parts of melamine, 2-5 parts of tripolyphosphonate, 2-7 parts of urea peroxide, 1-3 parts of hydantoin and 1-8 parts of polyamide.
[0008] In a preferred embodiment, the phosphorus-based flame retardant includes the following components in parts by weight: 10 parts of phosphorus dioxide, 6 parts of tripolyphosphate, 3 parts of hexametaphosphate, 7 parts of cyclophosphamide, and 6 parts of phosphoric acid; the nitrogen-based flame retardant includes the following components in parts by weight: 9 parts of melamine, 2 parts of tripolyphosphonate, 2 parts of urea peroxide, 1 part of hydantoin, and 1 part of polyamide.
[0009] In a preferred embodiment, the phosphorus-based flame retardant includes the following components in parts by weight: 12 parts of phosphorus dioxide, 8 parts of tripolyphosphate, 5 parts of hexametaphosphate, 8 parts of cyclophosphamide, and 10 parts of phosphoric acid; the nitrogen-based flame retardant includes the following components in parts by weight: 11 parts of melamine, 4 parts of tripolyphosphonate, 6 parts of urea peroxide, 2 parts of hydantoin, and 5 parts of polyamide.
[0010] In a preferred embodiment, a coupling agent is further included, and the weight proportion of the silane coupling agent is 5-9 parts.
[0011] In a preferred embodiment, the coupling agent is one of γ-aminopropyltriethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane and N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane.
[0012] A method for preparing a flame retardant for environmentally friendly paint comprises the following steps: adding a phosphorus flame retardant and a nitrogen flame retardant into a reactor together, mixing and stirring for 10-20 minutes at a rotation speed of 200-400 r / min, then adding a coupling agent, and continuously stirring for 5-12 minutes to obtain a flame retardant.
[0013] The beneficial effects of the technical solution of the present invention are:
[0014] This solution mixes phosphorus flame retardants and nitrogen flame retardants and controls the ratio within a certain range. From the experimental results, it can be seen that when the flame retardant of the present invention is added in an amount of 10 parts by weight, the flame retardant grade can reach UL94V-0. Compared with the existing flame retardants on the market, the addition amount is significantly reduced, the thermal stability is improved, and the flame retardant effect is improved. DETAILED DESCRIPTION
[0015] The present invention is further described in detail below. The embodiments of the present invention are provided for the purpose of illustration and description, and are not intended to be exhaustive or to limit the present invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described to better illustrate the principles and practical applications of the present invention, and to enable those of ordinary skill in the art to understand the present invention and design various embodiments with various modifications suitable for specific uses.
[0016] Example 1
[0017] The technical solution of the present invention provides a flame retardant for environmentally friendly paint, comprising a phosphorus flame retardant and a nitrogen flame retardant, wherein the phosphorus flame retardant comprises the following components in parts by weight: 10 parts of phosphorus dioxide, 6 parts of tripolyphosphate, 3 parts of hexametaphosphate, 7 parts of cyclophosphamide, and 6 parts of phosphoric acid; the nitrogen flame retardant comprises the following components in parts by weight: 9 parts of melamine, 2 parts of tripolyphosphonate, 2 parts of urea peroxide, 1 part of hydantoin, and 1 part of polyamide.
[0018] The invention also comprises a coupling agent, wherein the weight proportion of the silane coupling agent is 5 parts. The coupling agent is γ-aminopropyltriethoxysilane.
[0019] A method for preparing a flame retardant for environmentally friendly paint comprises the following steps: adding a phosphorus flame retardant and a nitrogen flame retardant into a reactor together, mixing and stirring for 100 minutes at a speed of 200 r / min, then adding a coupling agent, and continuously stirring for 5 minutes to obtain a flame retardant.
[0020] At the same time, the flame retardant is used to prepare latex paint, and the flame retardant is added into the latex paint in an amount of 10 parts.
[0021] Example 2
[0022] The technical solution of the present invention provides a flame retardant for environmentally friendly paint, comprising a phosphorus flame retardant and a nitrogen flame retardant, wherein the phosphorus flame retardant comprises the following components in parts by weight: 12 parts of phosphorus dioxide, 8 parts of tripolyphosphate, 5 parts of hexametaphosphate, 8 parts of cyclophosphamide, and 10 parts of phosphoric acid; the nitrogen flame retardant comprises the following components in parts by weight: 11 parts of melamine, 4 parts of tripolyphosphonate, 6 parts of urea peroxide, 2 parts of hydantoin, and 5 parts of polyamide.
[0023] The invention also comprises a coupling agent, wherein the weight proportion of the silane coupling agent is 9 parts. The coupling agent is N-β-aminoethyl-γ-aminopropyltrimethoxysilane.
[0024] A method for preparing a flame retardant for environmentally friendly paint comprises the following steps: adding a phosphorus flame retardant and a nitrogen flame retardant into a reactor together, mixing and stirring for 20 minutes at a speed of 400 r / min, then adding a coupling agent, and continuously stirring for 12 minutes to obtain a flame retardant.
[0025] At the same time, the flame retardant is used to prepare latex paint, and the flame retardant is added into the latex paint in an amount of 10 parts.
[0026] Example 3
[0027] The technical solution of the present invention provides a flame retardant for environmentally friendly paint, comprising a phosphorus flame retardant and a nitrogen flame retardant, wherein the phosphorus flame retardant comprises the following components in parts by weight: 15 parts of phosphorus dioxide, 10 parts of tripolyphosphate, 7 parts of hexametaphosphate, 11 parts of cyclophosphamide, and 14 parts of phosphoric acid;
[0028] The nitrogen-based flame retardant comprises the following components in parts by weight: 15 parts of melamine, 5 parts of tripolyphosphonate, 7 parts of urea peroxide, 1-3 parts of hydantoin, and 8 parts of polyamide.
[0029] The invention also comprises a coupling agent, wherein the weight proportion of the silane coupling agent is parts. The coupling agent is N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane.
[0030] A method for preparing a flame retardant for environmentally friendly paint comprises the following steps: adding a phosphorus flame retardant and a nitrogen flame retardant into a reactor together, mixing and stirring for 20 minutes at a speed of 200 r / min, then adding a coupling agent, and continuously stirring for 8 minutes to obtain a flame retardant.
[0031] At the same time, the flame retardant is used to prepare latex paint, and the flame retardant is added into the latex paint in an amount of 10 parts.
[0032] Comparative Example 1
[0033] The flame retardant disclosed in application number 201410286058.7 was added into the latex paint in an amount of 10 parts.
[0034] Comparative Example 2
[0035] The flame retardant disclosed in application number 202110515750.2 is added to the latex paint in an amount of 10 parts.
[0036] The flame retardant properties of the latex paints prepared in Examples 1-5 were tested, and the results are shown in Table 1 below:
[0037] Table 1: Flame retardant test results of Examples 1-5 and Comparative Examples 1-2
[0038] project Added amount (portion) Flame retardant grade Added amount (portion) Flame retardant grade Example 1 10 UL94V-0 10 UL94V-0 Example 2 10 UL94V-0 10 UL94V-0 Example 3 10 UL94V-0 10 UL94V-0 Comparative Example 1 10 UL94V-2 30 UL94V-0 Comparative Example 2 10 UL94V-2 40 UL94V-0
[0039] It can be seen that when the addition amount of the flame retardant of the present invention is 10 parts by weight, the flame retardant grade can reach UL94V-0. Compared with the existing flame retardants on the market, the addition amount is significantly reduced, the thermal stability is improved, and the flame retardant effect is good.
[0040] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field and related fields without creative work should fall within the scope of protection of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention are implemented according to the conventional means in the field unless otherwise specified and limited.
Claims
1. A flame retardant for environmentally friendly paint, characterized in that: It includes phosphorus flame retardant and nitrogen flame retardant, wherein the phosphorus flame retardant includes the following components in parts by weight: 10-15 parts of phosphorus dioxide, 6-10 parts of tripolyphosphate, 3-7 parts of hexametaphosphate, 7-11 parts of cyclophosphamide, and 6-14 parts of phosphoric acid; The nitrogen-based flame retardant comprises the following components in parts by weight: 9-15 parts of melamine, 2-5 parts of tripolyphosphonate, 2-7 parts of urea peroxide, 1-3 parts of hydantoin and 1-8 parts of polyamide.
2. The flame retardant for environmentally friendly paint according to claim 1, characterized in that: The phosphorus-based flame retardant includes the following components in parts by weight: 10 parts of phosphorus dioxide, 6 parts of tripolyphosphate, 3 parts of hexametaphosphate, 7 parts of cyclophosphamide, and 6 parts of phosphoric acid; the nitrogen-based flame retardant includes the following components in parts by weight: 9 parts of melamine, 2 parts of tripolyphosphonate, 2 parts of urea peroxide, 1 part of hydantoin, and 1 part of polyamide.
3. The flame retardant for environmentally friendly paint according to claim 1, characterized in that: The phosphorus-based flame retardant includes the following components in parts by weight: 12 parts of phosphorus dioxide, 8 parts of tripolyphosphate, 5 parts of hexametaphosphate, 8 parts of cyclophosphamide, and 10 parts of phosphoric acid; the nitrogen-based flame retardant includes the following components in parts by weight: 11 parts of melamine, 4 parts of tripolyphosphonate, 6 parts of urea peroxide, 2 parts of hydantoin, and 5 parts of polyamide.
4. The flame retardant for environmentally friendly paint according to claim 1, characterized in that: The invention also comprises a coupling agent, wherein the weight proportion of the silane coupling agent is 5-9 parts.
5. The flame retardant for environmentally friendly paint according to claim 1, characterized in that: The coupling agent is one of γ-aminopropyltriethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane and N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane.
6. The method for preparing a flame retardant for environmentally friendly paint according to any one of claims 1 to 5, characterized in that: The steps include: Add the phosphorus flame retardant and the nitrogen flame retardant into the reactor together, mix and stir for 10-20 minutes at a speed of 200-400r / min, then add the coupling agent, continue stirring for 5-12 minutes, and then obtain the flame retardant.