High-temperature-resistant deeply-cured ultraviolet curing adhesive and preparation method thereof

By using epoxy resin, silicone-modified acrylate and other materials in UV-curable adhesives, combined with the dark reaction characteristics of cationic photoinitiators, a high cross-linking network structure is formed, which solves the problem of high-temperature adhesion in the existing technology. It solves the problems of reduced contact performance and insufficient curing depth, and achieves the effects of high temperature resistance and deep curing.

CN118725795AInactive Publication Date: 2024-10-01SHENZHEN NO 1 FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410963574.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The bonding performance of existing UV-curable adhesives decreases under high temperature conditions, the curing depth is insufficient, and the curing is limited to the illuminated area, making it difficult to effectively cure in dark or weak light areas.

Method used

Using a combination of epoxy resin, silicone-modified acrylate, polyurethane acrylate prepolymer, reactive diluent, cationic photoinitiator and silane coupling agent, a UV-curable adhesive preparation method is used to form a highly cross-linked The high degree of three-dimensional network structure uses the dark reaction characteristics of the cationic photoinitiator to extend the curing time, improve thermal stability and curing depth.

Benefits of technology

It achieves deep curing and good mechanical properties under high temperature conditions, maintains adhesion and flexibility, extends the curing time, and improves shear strength and thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004951050360000071
    Figure BDA0004951050360000071
  • Figure BDA0004951050360000081
    Figure BDA0004951050360000081
Patent Text Reader

Abstract

The invention belongs to the technical field of adhesives, and provides a high-temperature-resistant deeply-cured ultraviolet curing adhesive and a preparation method thereof. The ultraviolet curing adhesive is prepared from epoxy resin, organic silicon modified acrylate, a polyurethane acrylate prepolymer, a reactive diluent, a photoinitiator, a thixotropic agent and a silane coupling agent in specific parts by mass. The epoxy resin, the organic silicon modified acrylate, the polyurethane acrylate prepolymer and the reactive diluent are cured under the action of the cationic photoinitiator, so that the thermal stability of a cured product can be effectively enhanced, the curing shrinkage rate is reduced, the shear strength is improved, and the curing time is shortened; the ultraviolet curing adhesive has relatively high rigidity, high hardness, no surface crack and good mechanical property; the high-temperature-resistant adhesive has the advantages that excellent adhesion to plastics is maintained, the adhesive flexibility after curing is realized, the high-temperature-resistant effect is achieved, and the high-temperature-resistant adhesive still has excellent shear strength after high-temperature aging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and in particular to a high temperature resistant deep curing ultraviolet light curing adhesive and a preparation method thereof. Background Art

[0002] UV-curing adhesives are widely used in various fields due to their high efficiency and environmental protection. UV-curing adhesives are usually composed of photosensitive resins, crosslinking agents, diluents, photosensitizers, and modifiers. They achieve the purpose of bonding by undergoing a curing reaction under ultraviolet light irradiation. At present, the photosensitive resin of UV-curing adhesives is generally epoxy resin, which can shorten the time for rapid bonding and has good mechanical properties, chemical stability, weather resistance, etc.

[0003] According to different triggering mechanisms, photocuring systems are divided into free radical photocuring systems and cationic photocuring systems. Compared with free radical photocuring systems, cationic photocuring systems have the following advantages: small volume shrinkage during curing and strong adhesion; not inhibited by oxygen, rapid and complete curing can be achieved in air atmosphere; curing reaction is not easy to terminate, suitable for curing thick films and paints, etc.

[0004] Conventional UV-curing adhesives currently available have obvious limitations in high-temperature applications. Most adhesives will soften quickly under high-temperature conditions after curing, resulting in decreased bonding performance. As the ambient temperature rises, some adhesive molecular chains will experience relative slippage, and the mechanical properties of the material will decrease; some adhesives will further produce cross-links in the already cured colloids, which will become harder and more brittle, and their impact resistance will decrease. At the same time, the curing of UV-curing adhesives in the prior art is limited to the illuminated areas. It is difficult to effectively cure in areas that are not exposed to UV light or where the light is very weak, and the curing depth is insufficient.

[0005] Therefore, it is of great significance to provide a UV-curable adhesive that is resistant to high temperatures and has good mechanical properties and can be deeply cured. Summary of the invention

[0006] The object of the present invention is to provide a high temperature resistant deep curing ultraviolet light curing adhesive and a preparation method thereof in view of the deficiencies in the prior art.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a high temperature resistant deep curing UV curing adhesive, comprising the following raw materials in parts by weight:

[0009] 30-40 parts of epoxy resin, 10-20 parts of silicone modified acrylate, 10-20 parts of polyurethane acrylate prepolymer, 8-15 parts of reactive diluent, 3-10 parts of photoinitiator, 1-5 parts of thixotropic agent, and 1-5 parts of silane coupling agent.

[0010] Preferably, the epoxy resin comprises one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin and alicyclic epoxy resin.

[0011] Preferably, the organosilicon-modified acrylate comprises one or more of hydroxyl organosilicon-modified acrylate, amino organosilicon-modified acrylate, alkoxy organosilicon-modified acrylate and epoxy organosilicon-modified acrylate.

[0012] Preferably, the active diluent comprises one or more of butyl glycidyl ether, 3-ethyl-3-hydroxymethyloxetane, 3,3-(oxybismethylene)-bis-(3-ethyl)oxetane, vinyl cyclohexyl ether, glycerol triglycidyl ether, trimethylolpropane triacrylate and tetrahydrofuran acrylate.

[0013] Preferably, the photoinitiator is a cationic photoinitiator, and the photoinitiator comprises one or more of an aromatic diazonium salt, a triarylsulfonium salt, an iron arene salt and a sulfonyloxy ketone.

[0014] Preferably, the thixotropic agent comprises one or more of silicon micropowder, fumed silica and organic bentonite, and the particle size of the thixotropic agent is 1 to 15 μm.

[0015] Preferably, the silane coupling agent comprises one or more of 3-glycidyloxypropyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane and 3-aminopropyltriethoxysilane.

[0016] The present invention also provides a method for preparing the high temperature resistant deep curing UV curing adhesive, comprising the following steps:

[0017] 1) mixing epoxy resin, silicone-modified acrylate, polyurethane acrylate prepolymer and reactive diluent to obtain a mixed prepolymer;

[0018] 2) Mixing the mixed prepolymer, the photoinitiator, the thixotropic agent and the silane coupling agent to obtain a UV-curable adhesive.

[0019] Preferably, the mixing speed in step 1) is 1000-2000 r / min, the mixing temperature is 20-40°C, and the mixing time is 10-20 min; the mixing speed in step 2) is 800-1500 r / min, the mixing temperature is 25-45°C, and the mixing time is 5-10 min.

[0020] The beneficial effects of the present invention include the following:

[0021] 1) When the curing adhesive of the present invention is irradiated with ultraviolet light, the cationic photoinitiator decomposes to generate cationic groups that initiate the ring-opening polymerization of epoxy groups, thereby retaining the advantage of instant curing of ultraviolet light curing technology; the cationic groups have a long active induction period, and can still initiate the ring-opening polymerization reaction of epoxy groups under low energy or after the ultraviolet light is withdrawn, delaying the curing time for a long time, and utilizing the unique "dark reaction" characteristics of the cationic system to complete the post-curing.

[0022] 2) The present invention uses acrylate and silicone groups in silicone-modified acrylate resin for condensation to form random, grafted and interpenetrating network copolymers. After UV curing, a firmly cross-linked three-dimensional network structure is formed between polymer molecules and between the polymer and the substrate. The cured product of this structure has many cross-linking points between molecules, a denser three-dimensional network structure, a high degree of cross-linking, and good high temperature resistance.

[0023] 3) The epoxy resin, silicone-modified acrylate, polyurethane acrylate prepolymer and reactive diluent of the present invention are cured under a cationic photoinitiator, which can effectively enhance the thermal stability of the cured product, reduce the curing shrinkage, improve the shear strength and shorten the curing time; the UV-curing adhesive of the present invention has high rigidity, high hardness, no surface cracks and good mechanical properties; while maintaining excellent adhesion to plastics and colloid flexibility after curing, it achieves high temperature resistance and still has excellent shear strength after high temperature aging. DETAILED DESCRIPTION

[0024] The present invention provides a high temperature resistant deep curing UV curing adhesive, comprising the following raw materials in parts by weight:

[0025] 30-40 parts of epoxy resin, 10-20 parts of silicone modified acrylate, 10-20 parts of polyurethane acrylate prepolymer, 8-15 parts of reactive diluent, 3-10 parts of photoinitiator, 1-5 parts of thixotropic agent, and 1-5 parts of silane coupling agent.

[0026] The raw materials for preparing the UV-curable adhesive of the present invention include 30 to 40 parts of epoxy resin, preferably 32 to 38 parts, more preferably 34 to 36 parts, and more preferably 35 parts.

[0027] In the present invention, the epoxy resin preferably comprises one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin and alicyclic epoxy resin.

[0028] The raw materials for preparing the UV-curable adhesive of the present invention include 10 to 20 parts of silicone-modified acrylate, preferably 12 to 18 parts, more preferably 14 to 16 parts, and more preferably 15 parts.

[0029] In the present invention, the organosilicon-modified acrylate preferably comprises one or more of hydroxyl organosilicon-modified acrylate, amino organosilicon-modified acrylate, alkoxy organosilicon-modified acrylate and epoxy organosilicon-modified acrylate.

[0030] The raw materials for preparing the UV-curable adhesive of the present invention include 10 to 20 parts of polyurethane acrylate prepolymer, preferably 12 to 18 parts, more preferably 14 to 16 parts, and more preferably 15 parts.

[0031] In the present invention, the polyurethane acrylate prepolymer is preferably one or more of Sartomer CN9001NS, Sartomer CN972, Cytec EB210 and BASF UA9030A.

[0032] The raw materials for preparing the UV-curable adhesive of the present invention contain 8 to 15 parts of reactive diluent, preferably 10 to 13 parts, and more preferably 11 to 12 parts.

[0033] In the present invention, the reactive diluent preferably comprises one or more of butyl glycidyl ether, 3-ethyl-3-hydroxymethyloxetane, 3,3-(oxybismethylene)-bis-(3-ethyl)oxetane, vinyl cyclohexyl ether, glycerol triglycidyl ether, trimethylolpropane triacrylate and tetrahydrofuran acrylate.

[0034] The main function of active diluent is to adjust viscosity and participate in polymerization reaction, which can not only increase the speed of photocuring, but also improve the toughness of adhesive. If the reaction activity of diluent and prepolymer is very different, the diluent will undergo homopolymerization or addition reaction with photoinitiator and will not participate in cross-linking of prepolymer. Active diluent can significantly shorten curing time and enhance the bonding performance of adhesive. If the addition amount is too large, it will lead to decreased bonding strength and water resistance.

[0035] The raw materials for preparing the UV-curable adhesive of the present invention contain 3 to 10 parts of photoinitiator, preferably 4 to 8 parts, and more preferably 6 to 7 parts.

[0036] In the present invention, the photoinitiator is a cationic photoinitiator, and the photoinitiator preferably comprises one or more of an aromatic diazonium salt, a triarylsulfonium salt, an iron arene salt and a sulfonyloxy ketone; the triarylsulfonium salt is preferably triarylsulfonium hexafluoroantimonate (UV-6976), and the iron arene salt is preferably η6-isopropylphenylferrocenium hexafluorophosphate (Irgacure 261); the sulfonyloxy ketone is preferably 2-toluenesulfonyloxy-2,4,6-cycloheptatriene-1-one.

[0037] In the present invention, after the photoinitiator is irradiated with ultraviolet light, it absorbs the energy of light and splits into active free radicals, causing the adhesive to cross-link and solidify to form a network structure; if the amount of initiator added is too little, the polymerization speed is too slow and the polymerization is insufficient, thereby reducing the bonding strength of the adhesive; if the amount of initiator used is too much, it will remain in the system, causing color change and affecting the optical properties.

[0038] The raw materials for preparing the UV-curable adhesive of the present invention contain 1 to 5 parts of a thixotropic agent, preferably 2 to 4 parts, and more preferably 3 parts.

[0039] In the present invention, the thixotropic agent preferably comprises one or more of silicon powder, fumed silica and organic bentonite; the particle size of the thixotropic agent is preferably 1 to 15 μm, more preferably 3 to 12 μm, and more preferably 5 to 10 μm.

[0040] The raw materials for preparing the UV-curable adhesive of the present invention contain 1 to 5 parts of silane coupling agent, preferably 2 to 4 parts, and more preferably 3 parts.

[0041] In the present invention, the silane coupling agent preferably comprises one or more of 3-glycidyloxypropyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane and 3-aminopropyltriethoxysilane.

[0042] In the present invention, the silane coupling agent can significantly increase the compatibility between the resin and the substrate, and improve the adhesion of the adhesive to the substrate.

[0043] The present invention also provides a method for preparing the high temperature resistant deep curing UV curing adhesive, comprising the following steps:

[0044] 1) mixing epoxy resin, silicone-modified acrylate, polyurethane acrylate prepolymer and reactive diluent to obtain a mixed prepolymer;

[0045] 2) Mixing the mixed prepolymer, the photoinitiator, the thixotropic agent and the silane coupling agent to obtain a UV-curable adhesive.

[0046] In the present invention, the mixing speed in step 1) is preferably 1000-2000 r / min, more preferably 1200-1800 r / min, and more preferably 1400-1500 r / min; the mixing temperature is preferably 20-40°C, more preferably 25-35°C, and more preferably 30°C; the mixing time is preferably 10-20 min, more preferably 12-18 min, and more preferably 14-15 min.

[0047] In the present invention, the mixing speed in step 2) is preferably 800-1500 r / min, more preferably 1000-1300 r / min, and more preferably 1100-1200 r / min; the mixing temperature is preferably 25-45°C, more preferably 30-40°C, and more preferably 35-36°C; the mixing time is preferably 5-10 min, more preferably 6-9 min, and more preferably 7-8 min.

[0048] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0049] In the embodiment, the hydroxy silicone modified acrylate is Qingrun QR630, the epoxy silicone modified acrylate is Xiano RB-237; the alkoxy silicone modified acrylate is Miki SM1046; the triarylsulfonium hexafluoroantimonate is UV-6976, the η6-isopropylphenylferrocenium hexafluorophosphate is Irgacure 261; the phenolic epoxy resin is F51; and the particle size of the thixotropic agent is 10 μm.

[0050] Example 1

[0051] The UV-curing adhesive was prepared from the following raw materials in parts by mass: 35 parts of bisphenol A epoxy resin, 15 parts of epoxy silicone-modified acrylate, 15 parts of polyurethane acrylate prepolymer (Sartomer CN9001NS), 6 parts of 3-ethyl-3-hydroxymethyloxetane, 6 parts of glycerol triglycidyl ether, 6 parts of η6-isopropylferrocenium hexafluorophosphate, 3 parts of fumed silica, and 3 parts of 3-glycidyloxypropyltrimethoxysilane.

[0052] Bisphenol A epoxy resin, epoxy silicone modified acrylate, polyurethane acrylate prepolymer, 3-ethyl-3-hydroxymethyloxetane and propylene glycol triglycidyl ether were mixed at a speed of 1500 r / min and 30°C for 15 minutes to obtain a uniformly mixed prepolymer; the prepolymer, η6-isopropylferrocenium hexafluorophosphate, fumed silica and 3-glycidyloxypropyltrimethoxysilane were mixed at a speed of 1200 r / min and 35°C for 8 minutes, and finally centrifuged and degassed at a speed of 3000 r / min to obtain a UV-curable adhesive.

[0053] Example 2

[0054] The UV-curing adhesive was prepared from the following raw materials in parts by mass: 32 parts of bisphenol F epoxy resin, 18 parts of hydroxy silicone-modified acrylate, 12 parts of polyurethane acrylate prepolymer (Cyanote EB210), 10 parts of butyl glycidyl ether, 4 parts of triarylsulfonium hexafluoroantimonate, 1 part of silicon powder, and 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0055] Bisphenol F epoxy resin, hydroxy silicone modified acrylate, polyurethane acrylate prepolymer and butyl glycidyl ether were mixed at a speed of 1200 r / min and 25°C for 18 minutes to obtain a uniformly mixed prepolymer; the prepolymer, triarylsulfonium hexafluoroantimonate, silicon powder and γ-(2,3-epoxypropoxy)propyltrimethoxysilane were mixed at a speed of 1000 r / min and 30°C for 10 minutes, and finally centrifuged and degassed at a speed of 2500 r / min to obtain a UV-curable adhesive.

[0056] Example 3

[0057] The UV-curable adhesive was prepared from the following raw materials in parts by mass: 38 parts of phenolic epoxy resin, 12 parts of alkoxy silicone-modified acrylate, 18 parts of polyurethane acrylate prepolymer (BASF UA9030A), 13 parts of 3,3-(oxybis(methylene))-bis-(3-ethyl)oxetane, 8 parts of η6-isopropylferrocenium hexafluorophosphate, 4 parts of organic bentonite, and 5 parts of 3-aminopropyltriethoxysilane.

[0058] The phenolic epoxy resin, alkoxy silicone modified acrylate, polyurethane acrylate prepolymer and 3,3-(oxybismethylene)-bis-(3-ethyl)oxetane were mixed at a speed of 1800 r / min and 35°C for 12 minutes to obtain a uniformly mixed prepolymer; the prepolymer, η6-isopropylferrocenium hexafluorophosphate, organic bentonite and 3-aminopropyltriethoxysilane were mixed at a speed of 1500 r / min and 40°C for 5 minutes, and finally centrifuged and degassed at a speed of 2800 r / min to obtain a UV-curable adhesive.

[0059] Comparative Example 1

[0060] The epoxy silicone modified acrylate and 3-glycidyloxypropyltrimethoxysilane in Example 1 were omitted, and η6-isopropylferrocenium hexafluorophosphate was replaced by benzoin dimethyl ether. Other conditions were the same as in Example 1.

[0061] Comparative Example 2

[0062] The polyurethane acrylate prepolymer and 3-ethyl-3-hydroxymethyloxetane of Example 1 were omitted, glycerol triglycidyl ether was replaced with isobornyl (meth)acrylate, and bisphenol A type epoxy resin was changed to 50 parts. Other conditions were the same as in Example 1.

[0063] The UV-curable adhesives of Examples 1 to 3 and Comparative Examples 1 to 2 were tested for properties such as curing time, shear strength, and high-temperature aging shear strength. The test results are shown in Table 1.

[0064] Curing time test: at light intensity 200mW / cm 2 , irradiate under ultraviolet light with a wavelength of 365nm and test the curing time.

[0065] Shear strength test: With transparent polycarbonate (PC) as the substrate, the sample was prepared according to the standard of GB / T 7124-2008. 2 , irradiate under ultraviolet light with a wavelength of 365nm for 50s, and test the high temperature aging shear strength.

[0066] High temperature aging shear strength test: transparent polycarbonate (PC) was used to prepare samples according to the standard of GB / T 7124-2008. 2 , irradiated under ultraviolet light with a wavelength of 365nm for 50s, the cured sample was placed at room temperature for 2h, and then baked in a 150℃ forced air oven for 20h for aging. The aged sample was placed at room temperature for 24h to test the high temperature aging shear strength.

[0067] Table 1 Test results of UV-curable adhesives of Examples and Comparative Examples

[0068]

[0069]

[0070] The present invention reasonably selects the types of prepolymer, photoinitiator and active diluent, and controls the specific amount of each raw material, so that the curing time of the obtained UV-curable adhesive is significantly shortened, and the curing speed is improved; the high temperature resistance is good, and it has excellent shear strength at both room temperature and high temperature; the cationic photoinitiator of the present invention has a long active induction period, which can trigger the prepolymer to undergo polymerization reaction for a long time, increase the curing depth and effectively cure. It can be seen from the embodiments, comparative examples and Table 1 that the types and amounts of the raw materials of the present invention are closely related. Changing any type or amount of the raw materials will prolong the curing time of the UV-curable adhesive and reduce its shear strength and high temperature resistance.

[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A high temperature resistant deep curing UV curing adhesive, characterized in that: Contains the following raw materials by mass: 30-40 parts of epoxy resin, 10-20 parts of silicone modified acrylate, 10-20 parts of polyurethane acrylate prepolymer, 8-15 parts of reactive diluent, 3-10 parts of photoinitiator, 1-5 parts of thixotropic agent, and 1-5 parts of silane coupling agent.

2. The UV curing adhesive according to claim 1, characterized in that: The epoxy resin comprises one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin and alicyclic epoxy resin.

3. The UV curing adhesive according to claim 1 or 2, characterized in that: The organosilicon-modified acrylate includes one or more of hydroxyl organosilicon-modified acrylate, amino organosilicon-modified acrylate, alkoxy organosilicon-modified acrylate and epoxy organosilicon-modified acrylate.

4. The UV-curable adhesive according to claim 3, characterized in that: The active diluent comprises one or more of butyl glycidyl ether, 3-ethyl-3-hydroxymethyloxetane, 3,3-(oxybismethylene)-bis-(3-ethyl)oxetane, vinyl cyclohexyl ether, glycerol triglycidyl ether, trimethylolpropane triacrylate and tetrahydrofuran acrylate.

5. The UV curing adhesive according to claim 3, characterized in that: The photoinitiator is a cationic photoinitiator, and the photoinitiator comprises one or more of aromatic diazonium salts, triarylsulfonium salts, iron aromatic salts and sulfonyloxy ketones.

6. The UV-curable adhesive according to claim 4 or 5, characterized in that: The thixotropic agent comprises one or more of silicon micropowder, fumed silica and organic bentonite, and the particle size of the thixotropic agent is 1 to 15 μm.

7. The UV-curable adhesive according to claim 6, characterized in that: The silane coupling agent comprises one or more of 3-glycidyloxypropyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane and 3-aminopropyltriethoxysilane.

8. The method for preparing the high temperature resistant deep curing UV curing adhesive according to any one of claims 1 to 7, characterized in that: The following steps are included: 1) mixing epoxy resin, silicone-modified acrylate, polyurethane acrylate prepolymer and reactive diluent to obtain a mixed prepolymer; 2) Mixing the mixed prepolymer, the photoinitiator, the thixotropic agent and the silane coupling agent to obtain a UV-curable adhesive.

9. The preparation method according to claim 8, characterized in that: The mixing speed of step 1) is 1000-2000 r / min, the mixing temperature is 20-40° C., and the mixing time is 10-20 min; the mixing speed of step 2) is 800-1500 r / min, the mixing temperature is 25-45° C., and the mixing time is 5-10 min.