Solar cell and preparation method thereof
By using a low-temperature process to form a base metal base layer on the silicon wafer and printing a silver-coated copper covering layer in TOPCon solar cells, the problems of silver shell shedding and copper ion migration caused by high-temperature sintering are solved, metallization costs are reduced, and battery efficiency is improved. reliability and efficiency.
Patent Information
- Application Number
- CN202410802386.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
The metallization cost of TOPCon solar cells is high. The existing silver-coated copper paste causes the silver shell to fall off and copper ions to migrate during the high-temperature sintering process, seriously reducing the performance and reliability of the battery and limiting its industrialization process.
By forming a patterned opening on the silicon wafer, a low-temperature process is used to prepare a base metal base layer in the opening, and a silver-coated copper covering layer is printed on it at low temperature to avoid high temperature damage to the silver shell and ensure the formation of the base metal and doped polysilicon layers. Ohmic contact, reducing silver content consumption and metallization costs.
It effectively reduces the silver content of the electrode, improves the reliability and efficiency of the battery, avoids copper ion migration, reduces metallization costs, and optimizes the thinning of the polysilicon layer on the back of the silicon wafer, improving the photoelectric performance of the battery.
Smart Images

Figure CN118738207A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a solar cell and a preparation method thereof. Background Art
[0002] Developing clean energy technology based on photovoltaic power generation is one of the important ways to solve the current energy supply problem and reduce greenhouse gas emissions. Crystalline silicon solar cells are still the mainstream products in the current commercial photovoltaic power generation field due to their excellent photovoltaic performance and relatively low manufacturing costs. In recent years, the iteration speed of crystalline silicon solar cell technology has accelerated, from the initial large-scale mass production of p-type Al-BSF cells to the PERC cells in the past few years, and then to the n-type TOPCon cells and HJT cells that have gradually dominated recently, the cell efficiency has been continuously improved.
[0003] Electrode metallization is one of the important processes of crystalline silicon solar cells. It is an important component of the manufacturing cost of the cell and a key factor affecting the photovoltaic performance of the cell. Since silver paste is used on both sides of the n-type cell, the silver paste consumption is significantly increased compared to PERC cells, and the metallization cost is high. In addition, due to the limitations of silver reserves and prices, the cost reduction space of the existing metallization technology is limited, which is one of the key factors restricting the acceleration of the industrialization of high-efficiency n-type cells. The metallization technology that uses base metal copper to replace silver is considered to be an ideal alternative technology for the future metallization of crystalline silicon cells.
[0004] At present, the metallization of n-type batteries in the industry is still mainly based on the preparation of silver electrodes by screen-printed silver paste. For n-type HJT batteries, screen-printed silver-coated copper paste technology has been used first, which can reduce the silver content in the electrode by 50% to 70%. Since TOPCon batteries are solar cells that need to form ohmic contacts through high-temperature sintering, if silver-coated copper paste is directly applied to TOPCon batteries, the silver shell will fall off during the high-temperature sintering process, and copper ions will migrate to the silicon substrate of the battery, seriously reducing the performance and reliability of the battery. Therefore, silver-coated copper paste cannot be directly applied to TOPCon batteries. At present, TOPCon batteries in the industry still use the method of double-sided screen printing of silver paste to prepare electrodes. The consumption of silver paste is large, resulting in high metallization costs for TOPCon batteries.
[0005] Therefore, in view of the above technical problems, it is necessary to provide a solar cell and a method for preparing the same. Summary of the invention
[0006] The object of the present invention is to provide a solar cell and a preparation method thereof, so as to reduce the metallization cost of a TOPCon cell.
[0007] In order to achieve the above purpose, the technical solution provided by an embodiment of the present invention is as follows:
[0008] A method for preparing a solar cell, the method comprising the following steps:
[0009] Providing a silicon wafer;
[0010] A tunneling layer and a doped polysilicon layer are sequentially stacked on the back side of the silicon wafer;
[0011] depositing a first dielectric layer on the doped polysilicon layer;
[0012] The first dielectric layer is patterned and opened by a laser process to form a first opening penetrating the doped polysilicon layer;
[0013] A first electrode in contact with the doped polysilicon layer is prepared at the first opening, including preparing a first base metal primer layer at the first opening by using an electroplating process or a chemical plating process; and printing a silver-coated copper slurry on the first base metal primer layer by using a screen printing process to form a first silver-coated copper covering layer after curing.
[0014] In one embodiment, the preparation method further comprises:
[0015] Prepare an emitter on the front side of the silicon wafer;
[0016] depositing a second dielectric layer on the emitter;
[0017] The second dielectric layer is patterned and opened by a laser process to form a second opening penetrating to the emitter;
[0018] A second electrode in contact with the emitter is prepared at the second opening, including preparing a second base metal primer layer at the second opening by electroplating or chemical plating; and printing a silver-coated copper slurry on the second base metal primer layer by screen printing to form a second silver-coated copper covering layer after curing.
[0019] In one embodiment, the curing temperature of the silver-coated copper slurry is 100° C. to 300° C., and the curing time is 1 min to 20 min.
[0020] In one embodiment, the electroplating process is a light-induced electroplating process or an electric field-induced electroplating process; wherein,
[0021] In the light-induced electroplating process, the wavelength of the light source is 300nm to 1100nm, and the cathode current density is 0.05A / dm 2 ~5A / dm 2 , the temperature range is 20℃~60℃, and the plating time is 1min~10min;
[0022] In the electric field induced plating process, the bath voltage is 0.5V~10V, and the cathode current density is 0.1A / dm 2 ~10A / dm 2, the temperature range is 20℃~60℃, and the plating time is 1min~10min.
[0023] In the chemical plating process, the chemical plating solution is a solution containing nickel sulfamate, with a pH value of 5 to 12, a temperature range of 60° C. to 90° C., and a reaction time of 2 min to 20 min.
[0024] In one embodiment, after preparing the first base metal primer layer, the process further comprises:
[0025] The first base metal bottom layer is annealed to form an ohmic contact between the first base metal bottom layer and the doped polysilicon layer; wherein the annealing temperature is 250°C to 450°C, the annealing time is 1 min to 20 min, the annealing atmosphere includes a protective gas and hydrogen, the protective gas includes nitrogen or an inert gas, the flow rate is 1 sccm to 10000 sccm, and the volume content of hydrogen is 1% to 50%.
[0026] In one embodiment, forming the first silver-clad copper covering layer further comprises:
[0027] Laser-assisted current injection is performed on the area where the first silver-clad copper covering layer is formed to form an ohmic contact between the first base metal base layer and the doped polysilicon layer; wherein the laser wavelength is 800nm~1200nm, the laser power is 5W~50W, the laser scanning speed is 10m / s~100m / s, and the bias voltage applied to the solar cell is 1V~20V.
[0028] In one embodiment, the first base metal primer layer fills the first opening and covers a portion of the surface of the first dielectric layer, and the width of the first silver-clad copper covering layer is less than or equal to the width of the first base metal primer layer.
[0029] In one embodiment, the first dielectric layer is AlO X Layer, SiN X Layer, SiO X N Y Layer, SiO X The thickness of the first opening is 1 μm to 40 μm or 40 μm to 400 μm, the thickness of the first base metal primer layer is 0.1 μm to 1 μm, and the thickness of the first silver-clad copper covering layer is 2 μm to 20 μm.
[0030] In one embodiment, the width of the first base metal primer layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or,
[0031] The width of the first silver-clad copper covering layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or,
[0032] The base metal in the first base metal primer layer is nickel or titanium.
[0033] In one embodiment, the second base metal primer layer fills the second opening and covers a portion of the second dielectric layer surface, and the width of the second silver-clad copper covering layer is less than or equal to the width of the second base metal primer layer.
[0034] In one embodiment, the second dielectric layer is AlO X Layer, SiN X Layer, SiO X N Y Layer, SiO X The thickness of the second opening is 1 μm to 40 μm or 40 μm to 400 μm, the thickness of the second base metal primer layer is 0.1 μm to 1 μm, and the thickness of the second silver-clad copper covering layer is 2 μm to 20 μm.
[0035] In one embodiment, the width of the second base metal primer layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or,
[0036] The width of the second silver-clad copper covering layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or,
[0037] The base metal in the second base metal primer layer is nickel or titanium.
[0038] In one embodiment, the preparation method further comprises:
[0039] Prepare an emitter on the front side of the silicon wafer;
[0040] depositing a second dielectric layer on the emitter;
[0041] The conductive paste is printed on the second dielectric layer by a screen printing process, and the front electrode is prepared by high-temperature sintering at a temperature of 700° C. to 850° C.
[0042] The technical solution provided by an embodiment of the present invention is as follows:
[0043] A solar cell is prepared by the above-mentioned preparation method.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The present invention forms a patterned opening through a dielectric layer, first prepares a base metal base layer in the opening, and then prints a silver-clad copper covering layer at a low temperature. By optimizing the structure and material of the dielectric layer and the electrode, the silver content of the electrode can be greatly reduced, thereby reducing the metallization cost.
[0046] The metallization process uses a low-temperature process to avoid the destruction and detachment of the silver shell on the surface of the silver-clad copper conductive phase caused by high temperature. The base metal base layer and the doped polysilicon layer are in ohmic contact, which can avoid the subsequent migration of copper ions into the silicon and improve the reliability of the battery. The low-temperature process is also conducive to the thinning of the polysilicon layer on the back of the silicon wafer, which can ensure the back passivation performance and improve the battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0048] Figures 1a to 1g is a process flow chart of the method for preparing a solar cell in Example 1 of the present invention;
[0049] Figure 2a is a schematic structural diagram of the first electrode in Example 1 of the present invention;
[0050] Figure 2b is a schematic structural diagram of the second electrode in Example 1 of the present invention;
[0051] Figure 3 Schematic diagram of the structure of the solar cell in Example 3 of the present invention. DETAILED DESCRIPTION
[0052] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0053] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0054] The present invention discloses a method for preparing a solar cell, comprising the following steps:
[0055] Providing a silicon wafer;
[0056] A tunneling layer and a doped polysilicon layer are sequentially stacked on the back side of the silicon wafer;
[0057] depositing a first dielectric layer on the doped polysilicon layer;
[0058] The first dielectric layer is patterned and opened by a laser process to form a first opening penetrating the doped polysilicon layer;
[0059] A first electrode in contact with the doped polysilicon layer is prepared at the first opening, including preparing a first base metal primer layer at the first opening by using an electroplating process or a chemical plating process; and printing a silver-coated copper slurry on the first base metal primer layer by using a screen printing process to form a first silver-coated copper covering layer after curing.
[0060] In the present invention, a patterned opening is formed through a dielectric layer, a base metal primer layer is first prepared in the opening, and then a silver-clad copper covering layer is printed at low temperature. The metallization process adopts a low-temperature process, which can avoid the destruction and detachment of the silver shell on the surface of the silver-clad copper conductive phase caused by high temperature. The base metal primer layer is in ohmic contact with the doped polysilicon layer, which can avoid the subsequent migration of copper ions into silicon, thereby improving the reliability of the battery.
[0061] The present invention is described in detail below in conjunction with specific implementations.
[0062] Embodiment 1:
[0063] The solar cell in this embodiment is a TOPCon cell, and the preparation method includes the following steps:
[0064] 1. Ginseng Figure 1a As shown, a silicon wafer 10 is provided and double-sided texturing is performed.
[0065] The silicon wafer 10 in this embodiment is an N-type single crystal silicon wafer. The front and back sides of the silicon wafer are textured and cleaned by alkaline solution to form a pyramid texture structure (not shown) on the surface of the silicon wafer 10.
[0066] Exemplarily, the alkali solution may contain an alkaline solution of sodium hydroxide or potassium hydroxide, the mass concentration of NaOH or KOH is 0.5% to 2%, the texturing temperature is 60° C. to 90° C., and the texturing time is 240s to 480s.
[0067] 2. Ginseng Figure 1b As shown, an emitter 14 is prepared on the front side of the silicon wafer 10 .
[0068] The textured silicon wafer is placed in a high-temperature diffusion furnace for front boron diffusion to prepare a front p+ emitter.
[0069] For example, in this embodiment, the temperature of high temperature diffusion is 800°C to 1200°C, the depth of the prepared p+ emitter is 0.6μm to 1.5μm, the square resistance is 60Ω / □ to 600Ω / □, and the surface boron doping concentration is 1E18atoms / cm 3 ~1E20atoms / cm 3 .
[0070] 3. The back side of the silicon wafer 10 is polished and etched.
[0071] First, the BSG layer on the back of the silicon wafer is removed, and then the silicon wafer is placed in an alkali solution for back polishing. In this embodiment, the alkali solution is an alkaline solution containing sodium hydroxide or potassium hydroxide, the mass concentration of NaOH or KOH is 1% to 5%, the polishing temperature is 50° C. to 80° C., and the polishing time is 100s to 300s.
[0072] 4. Ginseng Figure 1c As shown, a tunneling layer 11 and a doped polysilicon layer 12 are sequentially stacked on the back of a silicon wafer 10 .
[0073] The tunneling layer 11 is a SiO2 layer with a thickness of 1nm to 3nm; the doped polysilicon layer 12 is a phosphorus-doped polysilicon layer with a thickness of 10nm to 150nm, preferably 10nm to 110nm. In this embodiment, 100nm is used as an example for explanation. The square resistance is 20Ω / □ to 200Ω / □, and the phosphorus doping concentration is 1E20 atoms / cm 3 ~1E21atoms / cm 3 .
[0074] Specifically, a 1nm to 3nm thick tunnel oxide layer and a 10nm to 150nm thick phosphorus-doped amorphous silicon layer are sequentially deposited on the back of the silicon wafer using tubular PECVD, and then crystallized at 800°C to 900°C in a high-temperature annealing furnace for 10min to 100min to form a phosphorus-doped polycrystalline silicon layer.
[0075] 5. Etch the front side to remove the plating.
[0076] First, remove the PSG layer on the front side, and then put the silicon wafer into an alkaline solution to etch and remove the polysilicon layer. In this embodiment, the alkaline solution is an alkaline solution containing sodium hydroxide or potassium hydroxide, the mass concentration of NaOH or KOH is 1% to 5%, the temperature of the de-plating etching is 50°C to 80°C, and the etching time is 50s to 200s.
[0077] 6. Ginseng Figure 1d As shown, a second dielectric layer is deposited on the front side of the silicon wafer 10 .
[0078] Among them, the second dielectric layer is AlOX Layer, SiN X Layer, SiO X N Y Layer, SiO X The second dielectric layer comprises a passivation layer 15 and an anti-reflection layer 16 which are sequentially stacked on the emitter 14. The passivation layer is SiO X 、AlO X A combination of one or more of the above, preferably an Al2O3 layer with a thickness of 1nm to 10nm, and an anti-reflection layer of SiN X 、SiO X N Y 、SiO X One or more combinations thereof, preferably SiN X Layer with a thickness of 60nm to 80nm.
[0079] For example, the passivation layer 15 and the anti-reflection layer 16 in this embodiment are deposited in sequence by ALD and PECVD processes, respectively. X layer.
[0080] 7. Ginseng Figure 1e As shown, a first dielectric layer 13 is deposited on the back side of the silicon wafer.
[0081] The first dielectric layer 13 is AlO X Layer, SiN X Layer, SiO X N Y Layer, SiO X A combination of one or more layers, preferably SiN X The layer has a thickness of 60 nm to 100 nm, preferably 60 nm to 80 nm.
[0082] Exemplarily, the first dielectric layer 13 in this embodiment is deposited on the back side of the silicon wafer by using a PECVD process.
[0083] 8. Ginseng Figure 1f As shown, the first dielectric layer and the second dielectric layer are patterned and opened respectively by laser technology to form a first opening 131 penetrating the doped polysilicon layer 12 and a second opening 161 penetrating the emitter 14 .
[0084] Exemplarily, in this embodiment, an ultraviolet picosecond laser is used to perform patterned film opening, and the opening width and depth of the first opening 131 and the second opening 161 are controlled by laser parameters.
[0085] Specifically, the width of the first opening is 1 μm to 40 μm or 40 μm to 400 μm, specifically, the width of the first opening corresponding to the fine grid line is 1 μm to 40 μm, and the width of the first opening corresponding to the main grid line or the welding pad point is 40 μm to 400 μm. The width of the second opening is 1 μm to 40 μm or 40 μm to 400 μm, specifically, the width of the second opening corresponding to the fine grid line is 1 μm to 40 μm, and the width of the second opening corresponding to the main grid line or the welding pad point is 40 μm to 400 μm.
[0086] 9. Ginseng Figure 1g As shown, a first electrode 17 and a second electrode 18 are respectively provided on the back side and the front side of the silicon wafer.
[0087] Ginseng Figure 1g Combined with Figure 2a , 2b As described above, the first electrode 17 in this embodiment includes a first base metal bottom layer 171 and a first silver-clad copper covering layer 172 . The first base metal bottom layer 171 fills the first opening and is in ohmic contact with the doped polysilicon layer 12 . The first silver-clad copper covering layer 172 is stacked on the surface of the first base metal bottom layer 171 .
[0088] Preferably, the first base metal bottom layer 171 is filled in the first opening and covers a portion of the surface of the first dielectric layer 13, and the width of the first silver-clad copper covering layer 172 is smaller than the width of the first base metal bottom layer 171, which can ensure the positioning accuracy during the printing process and avoid printing deviation of the silver-clad copper slurry, thereby ensuring the conduction performance of carriers between the first silver-clad copper covering layer 172 and the first base metal bottom layer 171, thereby improving battery efficiency.
[0089] Exemplarily, in this embodiment, the thickness of the first base metal coating layer 171 is 0.1μm to 1μm, and the widths of the first base metal coating layer 171 are 5μm to 50μm and 50μm to 500μm for the fine gate lines and the main gate lines, respectively; the thickness of the first silver-clad copper covering layer 172 is 2μm to 20μm, and the widths of the first silver-clad copper covering layer 172 are 5μm to 50μm and 50μm to 500μm for the fine gate lines and the main gate lines, respectively.
[0090] Furthermore, the first base metal coating layer 171 is a base metal electrode, and the base metal is any one or more of nickel and titanium. For example, the first base metal coating layer in this embodiment is a nickel electrode.
[0091] The second electrode 18 in this embodiment includes a second base metal bottom layer 181 and a second silver-coated copper covering layer 182. The second base metal bottom layer 181 fills the second opening and is in ohmic contact with the emitter 14. The second silver-coated copper covering layer 182 is stacked on the surface of the second base metal bottom layer 181. The specific structure of the second electrode 18 in this embodiment is completely the same as that of the first electrode 17, and will not be described again here.
[0092] Specifically, taking the preparation of the first back electrode 17 as an example, the specific preparation process is as follows:
[0093] First, a first base metal bottom layer 171 is prepared at the first opening 131 by an electroplating process or a chemical plating process. The electroplating process is a light-induced electroplating process or an electric field-induced electroplating process. Taking the light-induced electroplating process as an example, the first base metal bottom layer 171 is a nickel (Ni) metal layer, the light source has a wavelength of 300nm to 1100nm, and the cathode current density is 0.05A / dm 2 ~5A / dm 2 , the temperature range is 20℃~60℃, and the plating time is 1min~10min. Preferably, the light wavelength of the light source in this embodiment is 700nm, and the cathode current density is 2.5A / dm 2 , the temperature range is 40℃ and the plating time is 5min.
[0094] Then, the first base metal bottom layer is annealed to form Ni-Si ohmic contact between the first base metal bottom layer and the doped polysilicon layer, the annealing temperature is 250°C to 450°C, the annealing time is 1min to 20min, the annealing atmosphere includes protective gas and hydrogen, the protective gas includes nitrogen or inert gas, the flow rate is 1sccm to 10000sccm, and the volume content of hydrogen is 1% to 50%. Preferably, the annealing temperature in this embodiment is 350°C, the annealing time is 10min, the annealing atmosphere includes argon and hydrogen, the flow rate is 5000sccm, and the volume content of hydrogen is 25%.
[0095] Finally, a silver-coated copper paste is printed on the first base metal base layer 171 by screen printing, and after curing, a first silver-coated copper covering layer 172 is formed, and the curing temperature is 100° C. to 300° C. and the curing time is 1 min to 20 min. Preferably, in this embodiment, the curing temperature is 200° C. and the curing time is 10 min.
[0096] In this embodiment, the first electrode 17 and the second electrode 18 are both gate line electrodes, which at least include a plurality of main gate lines and fine gate lines, the main gate lines and the fine gate lines are vertically distributed, and the patterns of the first opening and the second opening correspond to the first electrode and the second electrode respectively.
[0097] In other embodiments, the first base metal bottom layer can also be prepared by an electric field induced electroplating process or a chemical plating process. Specifically, in the electric field induced electroplating process, the cell voltage is 0.5V to 10V, and the cathode current density is 0.1A / dm 2 ~10A / dm 2 , the temperature range is 20℃~60℃, and the plating time is 1min~10min; in the chemical plating process, the chemical plating solution is a solution containing nickel sulfamate, the pH value is 5~12, the temperature range is 60℃~90℃, and the reaction time is 2min~20min.
[0098] Embodiment 2:
[0099] The solar cell in this embodiment is a TOPCon cell, and its structure is substantially the same as that in Embodiment 1, except that in this embodiment, no annealing process is used to form the Ni-Si ohmic contact. Instead, laser-assisted current injection is performed on the region of the first silver-clad copper covering layer after the first silver-clad copper covering layer is formed.
[0100] Specifically, in the laser-assisted current injection process, the laser wavelength is 800nm to 1200nm, the laser power is 5W to 50W, the laser scanning speed is 10m / s to 100m / s, and the bias voltage applied to the solar cell is 1V to 20V. Preferably, in this embodiment, the laser wavelength is 1000nm, the laser power is 25W, the laser scanning speed is 50m / s, and the bias voltage applied to the solar cell is 10V.
[0101] Embodiment 3:
[0102] Ginseng Figure 3 As shown, the solar cell in this embodiment is a TOPCon cell, and its structure is substantially the same as that in Embodiment 1, except that the second electrode 18' on the front side of the silicon wafer is different in structure and preparation process from the second electrode 18 in Embodiment 1, while the first electrode 17 on the back side of the silicon wafer is exactly the same in structure and preparation process as the first electrode 17 in Embodiment 1.
[0103] Specifically, in the preparation method of the solar cell in this embodiment, after the second dielectric layer is deposited on the front side of the silicon wafer, there is no need to use a laser process to pattern the second dielectric layer. The existing screen printing process is used to directly print silver paste or silver aluminum paste on the second dielectric layer, and high-temperature sintering (sintering temperature 750°C ~ 850°C) or high-temperature sintering (sintering temperature 700°C ~ 800°C) combined with a laser-assisted current injection process is used to form a metal-silicon ohmic contact on the front emitter, thereby obtaining a front electrode.
[0104] Comparative Example 1:
[0105] The solar cell in this comparative example is a TOPCon cell, and its preparation method is the same as that in Example 1, steps 1 to 7 are exactly the same, and the metallization process after the front and back dielectric layers are deposited is specifically as follows:
[0106] The existing screen printing process is used to print silver paste on the first dielectric layer, and silver paste or silver aluminum paste is printed on the second dielectric layer. Through high-temperature sintering (sintering temperature 750°C ~ 850°C), or through high-temperature sintering (sintering temperature 700°C ~ 800°C) combined with laser-assisted current injection process, metal-silicon ohmic contact is formed on the front emitter and the back doped polysilicon layer, thereby obtaining the front and back electrodes.
[0107] After comparison, the electrical performance data of the solar cells in Examples 1 and 2 and Comparative Example 1 are as follows:
[0108] Group <![CDATA[V oc (mV)]]> <![CDATA[J sc (mA / cm 2 )]]> FF(%) <![CDATA[R s (mΩ)]]> <![CDATA[R sh (Oh)]]> Eff(%) Comparative Example 1 734.4 41.81 84.81 0.67 2254 26.04 Example 1 736.2 41.80 84.61 0.71 3618 26.04 Example 2 736.7 41.81 84.80 0.68 2801 26.12
[0109] Since the metallization process uses a low-temperature process, it can avoid the destruction and detachment of the silver shell on the surface of the silver-clad copper conductive phase caused by high temperature. Through the annealing process, the base metal base layer and the doped polysilicon layer form Ni-Si ohmic contact, which can avoid the subsequent migration of copper ions into silicon and improve the reliability of the battery. The low-temperature process is also conducive to the thinning of the polysilicon layer on the back of the silicon wafer, which can ensure the back passivation performance and improve the efficiency of the battery.
[0110] In addition, by optimizing the structure and materials of the dielectric layer and the electrode, the silver content of the electrode can be greatly reduced and the metallization cost can be reduced.
[0111] Compared with Comparative Example 1, the open circuit voltage V OC There is a significant improvement, and the final battery efficiency Eff can be on par with that of pure silver electrodes.
[0112] In Example 2, a laser-assisted current injection process is used to form a Ni-Si ohmic contact. Compared with the annealing process in Example 1, the contact resistance can be further improved and the metal-induced recombination in the solar cell can be reduced, thereby further improving the cell efficiency Eff by about 0.08%.
[0113] In the above-mentioned Examples 1, 2 and Comparative Example 1, the thickness of the doped polysilicon layer on the back of the silicon wafer is described by taking 90nm to 110nm as an example. In Comparative Example 1, due to the limitation of the high-temperature sintering process of the existing electrode, the thickness of the doped polysilicon layer in the metal area cannot be thinned, and thinning the doped polysilicon layer in the non-metallic area requires additional etching / photolithography processes, which increases the process cost.
[0114] In Examples 1 and 2 of the present invention, since the electrodes are made using a low-temperature process, the thickness of the doped polysilicon layer (including the metal area and the non-metal area) on the back of the silicon wafer can be reduced to 20nm to 80nm, preferably 40nm to 60nm. This can further reduce the optical absorption on the back side and obtain better photoelectric performance, thereby further improving the battery efficiency on the basis of Examples 1 and 2 without increasing the process steps and reducing the process cost.
[0115] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0116] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a solar cell, characterized in that: The preparation method comprises the following steps: Providing a silicon wafer; A tunneling layer and a doped polysilicon layer are sequentially stacked on the back side of the silicon wafer; depositing a first dielectric layer on the doped polysilicon layer; The first dielectric layer is patterned and opened by a laser process to form a first opening penetrating the doped polysilicon layer; A first electrode in contact with the doped polysilicon layer is prepared at the first opening, including preparing a first base metal primer layer at the first opening by using an electroplating process or a chemical plating process; and printing a silver-coated copper slurry on the first base metal primer layer by using a screen printing process to form a first silver-coated copper covering layer after curing.
2. The preparation method according to claim 1, characterized in that: The preparation method further comprises: Prepare an emitter on the front side of the silicon wafer; depositing a second dielectric layer on the emitter; The second dielectric layer is patterned and opened by a laser process to form a second opening penetrating to the emitter; A second electrode in contact with the emitter is prepared at the second opening, including preparing a second base metal primer layer at the second opening by electroplating or chemical plating; and printing a silver-coated copper slurry on the second base metal primer layer by screen printing to form a second silver-coated copper covering layer after curing.
3. The preparation method according to claim 1 or 2, characterized in that: The curing temperature of the silver-coated copper slurry is 100° C. to 300° C., and the curing time is 1 min to 20 min.
4. The preparation method according to claim 1 or 2, characterized in that: The electroplating process is a light-induced electroplating process or an electric field-induced electroplating process; wherein, In the light-induced electroplating process, the wavelength of the light source is 300nm to 1100nm, and the cathode current density is 0.05A / dm 2 ~5A / dm 2 , the temperature range is 20℃~60℃, and the plating time is 1min~10min; In the electric field induced electroplating process, the bath voltage is 0.5V~10V and the cathode current density is 0.1A / dm 2 ~10A / dm 2 , the temperature range is 20℃~60℃, and the plating time is 1min~10min. In the chemical plating process, the chemical plating solution is a solution containing nickel sulfamate, with a pH value of 5 to 12, a temperature range of 60° C. to 90° C., and a reaction time of 2 min to 20 min.
5. The preparation method according to claim 1, characterized in that: After preparing the first base metal primer layer, the method further comprises: The first base metal bottom layer is annealed to form an ohmic contact between the first base metal bottom layer and the doped polysilicon layer; wherein the annealing temperature is 250°C to 450°C, the annealing time is 1 min to 20 min, the annealing atmosphere includes a protective gas and hydrogen, the protective gas includes nitrogen or an inert gas, the flow rate is 1 sccm to 10000 sccm, and the volume content of hydrogen is 1% to 50%.
6. The preparation method according to claim 1, characterized in that: Forming the first silver-clad copper covering layer also includes: Laser-assisted current injection is performed on the area where the first silver-clad copper covering layer is formed to form an ohmic contact between the first base metal base layer and the doped polysilicon layer; wherein the laser wavelength is 800nm~1200nm, the laser power is 5W~50W, the laser scanning speed is 10m / s~100m / s, and the bias voltage applied to the solar cell is 1V~20V.
7. The preparation method according to claim 1, characterized in that: The first base metal bottom layer is filled in the first opening and covers a portion of the surface of the first dielectric layer. The width of the first silver-clad copper covering layer is less than or equal to the width of the first base metal bottom layer.
8. The preparation method according to claim 7, characterized in that: The first dielectric layer is AlO X Layer, SiN X Layer, SiO X N Y Layer, SiO X The thickness of the first opening is 1 μm to 40 μm or 40 μm to 400 μm, the thickness of the first base metal primer layer is 0.1 μm to 1 μm, and the thickness of the first silver-clad copper covering layer is 2 μm to 20 μm.
9. The preparation method according to claim 7, characterized in that: The width of the first base metal primer layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or, The width of the first silver-clad copper covering layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or, The base metal in the first base metal primer layer is nickel or titanium.
10. The preparation method according to claim 2, characterized in that: The second base metal primer layer is filled in the second opening and covers a portion of the second dielectric layer surface. The width of the second silver-clad copper covering layer is less than or equal to the width of the second base metal primer layer.
11. The preparation method according to claim 10, characterized in that: The second dielectric layer is AlO X Layer, SiN X Layer, SiO X N Y Layer, SiO X The thickness of the second opening is 1 μm to 40 μm or 40 μm to 400 μm, the thickness of the second base metal primer layer is 0.1 μm to 1 μm, and the thickness of the second silver-clad copper covering layer is 2 μm to 20 μm.
12. The preparation method according to claim 10, characterized in that: The width of the second base metal primer layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or, The width of the second silver-clad copper covering layer is 5 μm to 50 μm or 50 μm to 500 μm; and / or, The base metal in the second base metal primer layer is nickel or titanium.
13. The preparation method according to claim 1, characterized in that: The preparation method further comprises: Prepare an emitter on the front side of the silicon wafer; depositing a second dielectric layer on the emitter; The conductive paste is printed on the second dielectric layer by a screen printing process, and the front electrode is prepared by high-temperature sintering at a temperature of 700° C. to 850° C.
14. A solar cell, characterized in that: The solar cell is prepared by the preparation method according to any one of claims 1 to 13.
Citation Information
Cited By
TOPCon battery metallization method
CN119545950A
Solar cell and photovoltaic module
CN120583790A
TOPCon battery structure and preparation method and splitting method thereof
CN120640838A