A preparation process of activated carbon with high adsorption and degradation performance

By combining activated carbon surface treatment with modified titanium dioxide, the problem of weak bonding between activated carbon and titanium dioxide was solved, achieving improved high-efficiency adsorption and photocatalytic degradation performance with long-lasting effects.

CN118767892BActive Publication Date: 2024-11-29福建韩研环保科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411255911.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-29
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

When activated carbon adsorbs and photocatalytically degrades pollutants, the binding force between titanium dioxide and activated carbon is weak, making it easy to detach, and the photocatalytic efficiency is low, making it difficult to achieve long-term binding.

Method used

Wood chips are activated using a mixture of phosphoric acid solution and boric acid, treated with hydrogen peroxide, and then the surface double bonds are modified with vinyltrimethoxysilane and methacrylic acid. Polymers are grafted onto the chips, and then crosslinked with modified titanium dioxide through ethylenediamine to form a strongly bonded composite material.

Benefits of technology

It achieves efficient photocatalytic degradation of pollutants while maintaining the adsorption performance of activated carbon. The photocatalyst and activated carbon have a strong binding force, are not easy to separate, and have a long-lasting effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to a preparation process of activated carbon with high adsorption and high degradation performance, and belongs to the technical field of activated carbon. The present invention first uses a mixture of phosphoric acid solution and boric acid as an activator and sawdust as a raw material to prepare a precursor, then adds hydrogen peroxide for surface treatment to enrich the surface hydroxyl groups, then adds vinyl trimethoxy silane, modifies the double bonds through the action of methoxy and hydroxyl groups, and methacrylic acid is used as a monomer to polymerize the double bonds, thereby grafting the polymer, and finally adds modified titanium dioxide that is also sequentially modified by vinyl trimethoxy silane, grafted by methacrylic acid polymerization, and then in-situ polymerized by aniline, and uses ethylenediamine as a cross-linking agent to achieve the compounding of a photocatalyst, and prepare an activated carbon, which has excellent adsorption performance on the one hand when actually used, and can also efficiently degrade pollutants on the other hand, and the photocatalyst and the activated carbon have a strong binding force and are not easy to separate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of activated carbon, and in particular relates to a preparation process of activated carbon with high adsorption and high degradation performance. Background Art

[0002] Activated carbon is an adsorbent material made from carbon-rich materials such as coal, petroleum asphalt, wood, olivine, nut shells, coconut shells, etc. through a carbonization and activation process. It is usually in powder or granular form, has a very developed pore structure and rich surface chemical groups, and is widely used in air purification, sewage treatment and other fields in daily life. For example, houses that have just been renovated often use activated carbon to adsorb and remove volatile organic pollutants such as formaldehyde. However, since activated carbon itself only has adsorption function but no degradation function, this greatly limits the practical application of activated carbon. In order to solve this technical defect, many existing technologies use the method of composite titanium dioxide to give activated carbon the ability to degrade. The ability to photocatalytically degrade pollutants, but this technology still has many disadvantages that limit its effectiveness. This is because, on the one hand, titanium dioxide has a wide band gap and low quantum efficiency, and absorbs and utilizes less visible light, so it cannot degrade very efficiently. On the other hand, titanium dioxide is simply compounded with activated carbon in the form of physical blending, and the binding force between the two is not strong. In the actual preparation and / or use process, titanium dioxide is very easy to fall off, which directly causes the loss of photocatalyst and greatly reduces the degradation performance. If it is compounded in the form of chemical bonds, it is difficult to ensure long-term effectiveness. The various free radicals generated by titanium dioxide when it is photocatalyzed will also attack the compound chemical bonds, and thus the two cannot form an effective combination. Summary of the invention

[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide a preparation process of activated carbon with high adsorption and high degradation performance. The present invention first uses a mixture of phosphoric acid solution and boric acid as an activator and sawdust as a raw material to prepare a precursor, then adds hydrogen peroxide for surface treatment to enrich the surface hydroxyl groups, then adds vinyltrimethoxysilane to modify the double bonds through the action of methoxy and hydroxyl groups, and methacrylic acid is used as a monomer to polymerize the double bonds, thereby grafting the polymer, and finally adds modified titanium dioxide which is also sequentially modified by vinyltrimethoxysilane, grafted by methacrylic acid polymerization, and then in-situ polymerized by aniline, and ethylenediamine is used as a cross-linking agent to realize the compounding of a photocatalyst, so as to prepare an activated carbon, which has excellent adsorption performance when actually used, and can also efficiently degrade pollutants, and the photocatalyst and the activated carbon have a strong binding force and are not easy to separate.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A preparation process of activated carbon with high adsorption and high degradation performance, the preparation process comprising the following steps:

[0006] (1) 50-60 parts by weight of sawdust were washed with deionized water, then vacuum dried at 50-60° C. until constant weight was achieved, and crushed to a particle size of 1-2 mm to obtain material A;

[0007] (2) adding 50-80 parts by weight of phosphoric acid solution and 4-6 parts by weight of boric acid to the material A, stirring for 5-10 minutes at room temperature, then immersing at 70-80° C. for 3-4 hours, filtering, removing the filtrate, and obtaining material B;

[0008] (3) carbonizing the material B under a nitrogen atmosphere, cooling it naturally to room temperature, then activating it under a carbon dioxide atmosphere, cooling it naturally to room temperature, washing it with deionized water, and finally vacuum drying it at 50-60° C. until constant weight is obtained to obtain material C;

[0009] (4) Add 150-200 parts by weight of hydrogen peroxide to the material C, stir for 5-10 minutes at room temperature, then soak at 50-60°C for 2-3 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60°C until constant weight, to obtain material D;

[0010] (5) Add 200-250 parts by weight of anhydrous ethanol, 0.5-1 parts by weight of deionized water and 3-4 parts by weight of vinyltrimethoxysilane to the material D, and then stir at 60-70° C. for 20-24 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60° C. until constant weight, to obtain material E;

[0011] (6) Add 200-250 parts by weight of deionized water, 12-14 parts by weight of methacrylic acid and 0.5-1 parts by weight of potassium persulfate to the material E, then stir at 80-85° C. for 2-3 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60° C. until constant weight, to obtain material F;

[0012] (7) Add 200-250 parts by weight of anhydrous ethanol, 8-10 parts by weight of modified titanium dioxide and 2-3 parts by weight of ethylenediamine to the material F, stir and mix at room temperature for 5-10 minutes, adjust the pH to 4 with concentrated sulfuric acid, and then stir at 50-60°C for 2-3 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60°C until constant weight, and the preparation is completed.

[0013] As a preferred technical solution of the present invention, the mass fraction of the phosphoric acid solution in step (2) is 45-50%.

[0014] As a preferred technical solution of the present invention, the carbonization in step (3) refers to heating the temperature to 350-400°C at a heating rate of 10-15°C / min and then maintaining the temperature for 1-2 hours; the activation refers to heating the temperature to 500-600°C at a heating rate of 10-15°C / min and then maintaining the temperature for 1-1.5 hours.

[0015] As a preferred technical solution of the present invention, the concentration of the hydrogen peroxide in step (4) is 1-1.5 mol / L.

[0016] As a preferred technical solution of the present invention, the modified titanium dioxide in step (7) is prepared by the following steps:

[0017] Step A: adding 80-100 parts by weight of anhydrous ethanol, 0.5-1 parts by weight of deionized water and 1 part by weight of vinyltrimethoxysilane to 5-7 parts by weight of nano titanium dioxide, stirring at 60-70° C. for 20-24 hours, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 60-70° C. until constant weight, to obtain material a;

[0018] Step B: adding 80-100 parts by weight of deionized water, 2 parts by weight of methacrylic acid and 0.3-0.5 parts by weight of potassium persulfate to the material a, stirring at 70-80° C. for 4-6 hours, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 60-70° C. until constant weight, to obtain material b;

[0019] Step C: add 80-100 parts by weight of dilute hydrochloric acid solution and 4-5 parts by weight of aniline to the material b, then add 30-40 parts by weight of ammonium persulfate solution dropwise while stirring at 2-4°C, continue stirring at a constant temperature for 5-6 hours after the addition is completed, let stand for 2-3 hours, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 60-70°C until constant weight, and the preparation is completed.

[0020] Furthermore, the particle size of the nano titanium dioxide in step A is 10-50 nm, and the crystal form of the nano titanium dioxide is anatase.

[0021] Furthermore, the concentration of the dilute hydrochloric acid solution in step C is 0.1 mol / L.

[0022] Furthermore, the dripping rate in step C is controlled at 1-3 drops / s.

[0023] Furthermore, the concentration of the ammonium persulfate solution in step C is 0.3-0.35 mol / L.

[0024] As a preferred technical solution of the present invention, the mass fraction of the concentrated sulfuric acid in step (7) is 70-75%.

[0025] Beneficial effects of the present invention:

[0026] (1) The present invention first uses a mixture of phosphoric acid solution and boric acid as an activator and sawdust as a raw material to prepare a precursor, then adds hydrogen peroxide for surface treatment to enrich the surface hydroxyl groups, then adds vinyl trimethoxy silane to modify the double bonds through the action of methoxy and hydroxyl groups, and methacrylic acid as a monomer undergoes double bond polymerization to graft the polymer, and finally adds modified titanium dioxide that has been modified with vinyl trimethoxy silane, grafted with methacrylic acid, and then in-situ polymerized with aniline, and uses ethylenediamine as a cross-linking agent to achieve the composite of the photocatalyst to prepare an activated carbon, which has excellent adsorption performance when actually used, and can also efficiently degrade pollutants, and the photocatalyst and the activated carbon have a strong binding force and are not easy to separate.

[0027] (2) The present invention creatively uses hydrogen peroxide to firstly perform surface treatment on the activated carbon after activation to enrich the hydroxyl groups on its surface. After surface treatment, its adsorption effect on polar pollutants can be enhanced. Then, vinyl trimethoxy silane is added to modify the double bonds through the action of methoxy and hydroxyl groups. Finally, methacrylic acid is introduced as a polymerization monomer to achieve double bond polymerization, thereby grafting a polymer containing a carboxyl group on the side chain. In addition, the present invention also sequentially performs vinyl trimethoxy silane modification on titanium dioxide, methacrylic acid polymerization grafting, and finally adds aniline to cause it to undergo in-situ polymerization to synthesize polyaniline. During the synthesis of polyaniline, its imine group can The modified titanium dioxide containing polyaniline is obtained by interacting with the carboxyl group, thereby achieving modification. The polyaniline is a conductive polymer with many characteristics such as narrow band gap and high visible light absorption coefficient. The introduction of the polyaniline can effectively absorb photons of visible light and generate electron pp* transition, promote the generation and separation of electrons and holes, so that there is a synergistic effect between titanium dioxide and polyaniline, thereby greatly improving the photocatalytic activity. Finally, ethylenediamine is used as a cross-linking agent, and the activated carbon grafted with a polymer structure and the modified titanium dioxide are compounded through the action of amino and carboxyl groups to prepare the activated carbon provided by the present invention. The binding force between the two is strong and separation is not easy to occur.

[0028] (3) The present invention creatively uses methacrylic acid as a polymerization monomer to polymerize and graft activated carbon and photocatalyst respectively, each of which forms a polymer structure, and then in situ generates polyaniline from the polymer structure of the photocatalyst, and finally realizes the composite of the two through the cross-linking effect of ethylenediamine; compared with the in situ polymerization of aniline on activated carbon, the preparation method of the present invention can not only promote the improvement of photocatalytic activity from the perspective of spatial barrier, but also because polyaniline contains a large number of benzene ring structures and has a very strong steric hindrance effect, it can also effectively "block" various free radicals generated by the photocatalyst from attacking the main chain of the polymer structure, thereby playing a role in delaying degradation. The two can achieve a very good combination with long-term effectiveness. At the same time, the polymer structure contains a large number of carboxyl groups, which further promotes the adsorption of polar pollutants. DETAILED DESCRIPTION

[0029] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0030] The wood chips in all the embodiments and comparative examples of the present invention are eucalyptus wood chips.

[0031] Example 1

[0032] A preparation process of activated carbon with high adsorption and high degradation performance, the preparation process comprising the following steps:

[0033] (1) 50 parts by weight of sawdust were washed with deionized water, then vacuum dried at 50° C. until constant weight was achieved, and crushed to a particle size of 1 mm to obtain material A;

[0034] (2) adding 50 parts by weight of phosphoric acid solution and 4 parts by weight of boric acid to the material A, stirring and mixing at room temperature for 5 minutes, then immersing at 70° C. for 3 hours, filtering, removing the filtrate, and obtaining material B;

[0035] (3) carbonizing the material B under a nitrogen atmosphere, cooling it naturally to room temperature, then activating it under a carbon dioxide atmosphere, cooling it naturally to room temperature, washing it with deionized water, and finally drying it under vacuum at 50° C. until constant weight is obtained to obtain material C;

[0036] (4) Add 150 parts by weight of hydrogen peroxide to the material C, stir and mix at room temperature for 5 minutes, then soak at 50°C for 2 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50°C until constant weight, to obtain material D;

[0037] (5) Adding 200 parts by weight of anhydrous ethanol, 0.5 parts by weight of deionized water and 3 parts by weight of vinyltrimethoxysilane to the material D, stirring the mixture at 60° C. for 20 h, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50° C. until constant weight is obtained to obtain material E;

[0038] (6) Add 200 parts by weight of deionized water, 12 parts by weight of methacrylic acid and 0.5 parts by weight of potassium persulfate to the material E, then stir at 80° C. for 2 h, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50° C. until constant weight, to obtain material F;

[0039] (7) Add 200 parts by weight of anhydrous ethanol, 8 parts by weight of modified titanium dioxide and 2 parts by weight of ethylenediamine to the material F, stir and mix at room temperature for 5 min, adjust the pH to 4 with concentrated sulfuric acid, and then stir at 50° C. for 2 h. Filter and remove the filtrate, wash with deionized water, and finally vacuum dry at 50° C. until constant weight is reached. The preparation is completed.

[0040] The mass fraction of the phosphoric acid solution in step (2) is 45%.

[0041] The carbonization in step (3) refers to heating the temperature to 350°C at a heating rate of 10°C / min and then maintaining the temperature for 1 hour; the activation refers to heating the temperature to 500°C at a heating rate of 10°C / min and then maintaining the temperature for 1 hour.

[0042] The concentration of the hydrogen peroxide in step (4) is 1 mol / L.

[0043] The modified titanium dioxide in step (7) is prepared by the following steps:

[0044] Step A: Add 80 parts by weight of anhydrous ethanol, 0.5 parts by weight of deionized water and 1 part by weight of vinyltrimethoxysilane to 5 parts by weight of nano titanium dioxide, then stir at 60° C. for 20 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 60° C. until constant weight to obtain material a;

[0045] Step B: adding 80 parts by weight of deionized water, 2 parts by weight of methacrylic acid and 0.3 parts by weight of potassium persulfate to the material a, stirring at 70° C. for 4 hours, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 60° C. until constant weight, to obtain material b;

[0046] Step C: add 80 parts by weight of dilute hydrochloric acid solution and 4 parts by weight of aniline to the material b, then add 30 parts by weight of ammonium persulfate solution dropwise while stirring at 2°C, continue stirring at a constant temperature for 5 hours after the addition is completed, let stand for 2 hours, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 60°C until constant weight, and the preparation is completed.

[0047] The particle size of the nano titanium dioxide in step A is 10 nm, and the crystal form of the nano titanium dioxide is anatase.

[0048] The concentration of the dilute hydrochloric acid solution in step C is 0.1 mol / L.

[0049] The dripping rate in step C is controlled at 1 drop / s.

[0050] The concentration of the ammonium persulfate solution in step C is 0.3 mol / L.

[0051] The mass fraction of the concentrated sulfuric acid in step (7) is 70%.

[0052] Example 2

[0053] A preparation process of activated carbon with high adsorption and high degradation performance, the preparation process comprising the following steps:

[0054] (1) 60 parts by weight of sawdust were washed with deionized water, then vacuum dried at 60° C. until constant weight was achieved, and crushed to a particle size of 2 mm to obtain material A;

[0055] (2) adding 80 parts by weight of phosphoric acid solution and 6 parts by weight of boric acid to the material A, stirring and mixing at room temperature for 10 minutes, then immersing at 80° C. for 4 hours, filtering, removing the filtrate, and obtaining material B;

[0056] (3) carbonizing the material B under a nitrogen atmosphere, cooling it naturally to room temperature, then activating it under a carbon dioxide atmosphere, cooling it naturally to room temperature, washing it with deionized water, and finally drying it under vacuum at 60° C. until constant weight is obtained to obtain material C;

[0057] (4) Add 200 parts by weight of hydrogen peroxide to the material C, stir and mix at room temperature for 10 minutes, then immerse at 60° C. for 3 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 60° C. until constant weight, to obtain material D;

[0058] (5) Add 250 parts by weight of anhydrous ethanol, 1 part by weight of deionized water and 4 parts by weight of vinyltrimethoxysilane to the material D, then stir at 70° C. for 24 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 60° C. until constant weight, to obtain material E;

[0059] (6) Add 250 parts by weight of deionized water, 14 parts by weight of methacrylic acid and 1 part by weight of potassium persulfate to the material E, then stir at 85° C. for 3 h, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 60° C. until constant weight, to obtain material F;

[0060] (7) Add 250 parts by weight of anhydrous ethanol, 10 parts by weight of modified titanium dioxide and 3 parts by weight of ethylenediamine to the material F, stir and mix at room temperature for 10 min, adjust the pH to 4 with concentrated sulfuric acid, and then stir at 60° C. for 3 h. Filter and remove the filtrate, wash with deionized water, and finally vacuum dry at 60° C. until constant weight is achieved. The preparation is completed.

[0061] The mass fraction of the phosphoric acid solution in step (2) is 50%.

[0062] The carbonization in step (3) refers to heating the temperature to 400°C at a heating rate of 15°C / min and then maintaining the temperature for 2 hours; the activation refers to heating the temperature to 600°C at a heating rate of 15°C / min and then maintaining the temperature for 1.5 hours.

[0063] The concentration of the hydrogen peroxide in step (4) is 1.5 mol / L.

[0064] The modified titanium dioxide in step (7) is prepared by the following steps:

[0065] Step A: Add 100 parts by weight of anhydrous ethanol, 1 part by weight of deionized water and 1 part by weight of vinyltrimethoxysilane to 7 parts by weight of nano titanium dioxide, then stir at 70° C. for 24 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 70° C. until constant weight to obtain material a;

[0066] Step B: adding 100 parts by weight of deionized water, 2 parts by weight of methacrylic acid and 0.5 parts by weight of potassium persulfate to the material a, stirring at 80° C. for 6 hours, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 70° C. until constant weight, to obtain material b;

[0067] Step C: add 100 parts by weight of dilute hydrochloric acid solution and 5 parts by weight of aniline to the material b, then add 40 parts by weight of ammonium persulfate solution dropwise while stirring at 4°C, continue stirring at a constant temperature for 6 hours after the addition is completed, let stand for 3 hours, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 70°C until constant weight, and the preparation is completed.

[0068] The particle size of the nano titanium dioxide in step A is 50 nm, and the crystal form of the nano titanium dioxide is anatase.

[0069] The concentration of the dilute hydrochloric acid solution in step C is 0.1 mol / L.

[0070] The rate of dripping in step C is controlled at 3 drops / s.

[0071] The concentration of the ammonium persulfate solution in step C is 0.35 mol / L.

[0072] The mass fraction of the concentrated sulfuric acid in step (7) is 75%.

[0073] Example 3

[0074] A preparation process of activated carbon with high adsorption and high degradation performance, the preparation process comprising the following steps:

[0075] (1) 55 parts by weight of sawdust were washed with deionized water, then vacuum dried at 55° C. until constant weight was achieved, and crushed to a particle size of 1.5 mm to obtain material A;

[0076] (2) adding 70 parts by weight of phosphoric acid solution and 5 parts by weight of boric acid to the material A, stirring and mixing at room temperature for 8 minutes, then immersing at 75° C. for 3.5 hours, filtering, removing the filtrate, and obtaining material B;

[0077] (3) carbonizing the material B under a nitrogen atmosphere, cooling naturally to room temperature, then activating it under a carbon dioxide atmosphere, cooling naturally to room temperature, washing it with deionized water, and finally vacuum drying it at 55° C. until constant weight is obtained to obtain material C;

[0078] (4) Add 180 parts by weight of hydrogen peroxide to the material C, stir and mix at room temperature for 8 minutes, then soak at 55° C. for 2.5 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 55° C. until constant weight, to obtain material D;

[0079] (5) Add 220 parts by weight of anhydrous ethanol, 0.8 parts by weight of deionized water and 3.5 parts by weight of vinyltrimethoxysilane to the material D, and then stir at 65° C. for 22 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 55° C. until constant weight, to obtain material E;

[0080] (6) Add 230 parts by weight of deionized water, 13 parts by weight of methacrylic acid and 0.8 parts by weight of potassium persulfate to the material E, then stir at 83° C. for 2.5 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 55° C. until constant weight, to obtain material F;

[0081] (7) Add 220 parts by weight of anhydrous ethanol, 9 parts by weight of modified titanium dioxide and 2.5 parts by weight of ethylenediamine to the material F, stir and mix at room temperature for 8 minutes, adjust the pH to 4 with concentrated sulfuric acid, and then stir at 55°C for 2.5 hours. Filter and remove the filtrate, wash with deionized water, and finally vacuum dry at 55°C until constant weight. The preparation is completed.

[0082] The mass fraction of the phosphoric acid solution in step (2) is 48%.

[0083] The carbonization in step (3) refers to heating the temperature to 380°C at a heating rate of 13°C / min and then maintaining the temperature for 1.5 hours; the activation refers to heating the temperature to 550°C at a heating rate of 13°C / min and then maintaining the temperature for 1.3 hours.

[0084] The concentration of the hydrogen peroxide in step (4) is 1.3 mol / L.

[0085] The modified titanium dioxide in step (7) is prepared by the following steps:

[0086] Step A: Add 90 parts by weight of anhydrous ethanol, 0.8 parts by weight of deionized water and 1 part by weight of vinyltrimethoxysilane to 6 parts by weight of nano titanium dioxide, then stir at 65° C. for 23 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 65° C. until constant weight to obtain material a;

[0087] Step B: adding 90 parts by weight of deionized water, 2 parts by weight of methacrylic acid and 0.4 parts by weight of potassium persulfate to the material a, stirring at 75° C. for 5 hours, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 65° C. until constant weight, to obtain material b;

[0088] Step C: Add 90 parts by weight of dilute hydrochloric acid solution and 4.5 parts by weight of aniline to the material b, then add 35 parts by weight of ammonium persulfate solution dropwise while stirring at 3°C, continue stirring at a constant temperature for 5.5 hours after the addition is completed, let stand for 2.5 hours, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 65°C until constant weight, and the preparation is completed.

[0089] The particle size of the nano titanium dioxide in step A is 30 nm, and the crystal form of the nano titanium dioxide is anatase.

[0090] The concentration of the dilute hydrochloric acid solution in step C is 0.1 mol / L.

[0091] The rate of the dripping in step C is controlled at 2 drops / s.

[0092] The concentration of the ammonium persulfate solution in step C is 0.33 mol / L.

[0093] The mass fraction of the concentrated sulfuric acid in step (7) is 73%.

[0094] Comparative Example 1

[0095] Based on Example 1, step C is not performed, and the rest remain unchanged.

[0096] Comparative Example 2

[0097] On the basis of Example 1, 4 parts by weight of aniline in step C was changed to 8 parts by weight of aniline, and the rest remained unchanged.

[0098] Comparative Example 3

[0099] On the basis of Example 1, step C is omitted, and step (7) is changed to adding 80 parts by weight of dilute hydrochloric acid solution and 4 parts by weight of aniline to the material F, and then adding 30 parts by weight of ammonium persulfate solution dropwise at 2°C while stirring. After the addition is completed, the material is stirred at a constant temperature for 5 h, left to stand for 2 h, filtered, the filtrate is removed, washed with anhydrous ethanol, and finally vacuum dried at 60°C until constant weight is obtained to obtain material E, wherein the concentration of the dilute hydrochloric acid solution is 0.1 mol / L, the rate of the addition is controlled at 1 drop / s, and the concentration of the ammonium persulfate solution is 0.3 mol / L; step (8) is added to add 200 parts by weight of anhydrous ethanol, 8 parts by weight of modified titanium dioxide and 2 parts by weight of ethylenediamine to the material E, stirring and mixing at room temperature for 5 min, adjusting the pH to 4 with concentrated sulfuric acid, and then stirring at 50°C for 2 h, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50°C until constant weight is obtained, and the preparation is completed; the rest remains unchanged.

[0100] Comparative Example 4

[0101] On the basis of Example 1, step C is omitted, and step (7) is changed to adding 200 parts by weight of anhydrous ethanol, 8 parts by weight of modified titanium dioxide and 2 parts by weight of ethylenediamine to the material F, stirring at room temperature for 5 min, adjusting the pH to 4 with concentrated sulfuric acid, stirring at 50°C for 2 h, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50°C until constant weight is obtained to obtain material E; step (8) is added to the material E, and then 30 parts by weight of ammonium persulfate solution is added dropwise at 2°C while stirring, and after the addition is completed, the material is stirred at a constant temperature for 5 h, allowed to stand for 2 h, filtered, the filtrate is removed, washing with anhydrous ethanol, and finally vacuum drying at 60°C until constant weight is obtained, and the preparation is completed. The concentration of the dilute hydrochloric acid solution is 0.1 mol / L, the dropping rate is controlled at 1 drop / s, and the concentration of the ammonium persulfate solution is 0.3 mol / L; the rest remains unchanged.

[0102] Comparative Example 5

[0103] Based on Example 1, step (4) is not performed and the rest remain unchanged.

[0104] Comparative Example 6

[0105] On the basis of Example 1, step (7) is changed to adding 200 parts by weight of anhydrous ethanol and 8 parts by weight of modified titanium dioxide to the material F, stirring for 5 min at room temperature, then stirring for 2 h at 50° C., filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50° C. until constant weight, and the preparation is completed; the rest remains unchanged.

[0106] Test Example 1

[0107] Adsorption performance test:

[0108] 1 g of activated carbon prepared in Examples 1-3 and Comparative Examples 1-6 was weighed respectively, and formaldehyde was used as polar VOCs. Formaldehyde gas with a concentration of 200 ppm and a relative humidity of 50% was then introduced respectively, wherein the residence time was 1 s. The exhaust gas was discharged, and the formaldehyde concentration of the exhaust gas was detected by gas chromatograph.

[0109] Table 1. Adsorption performance test results

[0110]

[0111] Test Example 2

[0112] Photocatalytic degradation performance test:

[0113] The activated carbons prepared in Examples 1-3 and Comparative Examples 1-6 were respectively tested for photocatalytic degradation performance according to the reference standard GB / T 23761-2009.

[0114] Table 2. Photocatalytic degradation performance test results

[0115]

[0116] Test Example 3

[0117] Long-term test:

[0118] The activated carbons prepared in Examples 1-3 and Comparative Examples 1-6 were respectively irradiated with a 400 W metal halide lamp for 24 h, then washed with deionized water, and finally vacuum dried at 50°C to a constant weight. The photocatalytic degradation performance test was repeated according to the test conditions of Test Example 2 (after long-term irradiation, chemical bonds in different forms will be degraded to varying degrees and may break, making it impossible to form an effective bond. After washing with deionized water, the "free" photocatalyst is easily removed).

[0119] Table 3. Long-term effect test results

[0120]

[0121] Comparison between Example 1 and Comparative Examples 1-6 shows that:

[0122] The difference between Comparative Example 1 and Example 1 is that polyaniline is not synthesized in situ.

[0123] The difference between Comparative Example 2 and Example 1 is that the degree of polymerization of polyaniline is increased.

[0124] The difference between Comparative Example 3 and Example 1 is that polyaniline is synthesized in situ on activated carbon.

[0125] The difference between Comparative Example 4 and Example 1 is that the modified titanium dioxide is first compounded with activated carbon and then the polyaniline is synthesized in situ.

[0126] The difference between Comparative Example 5 and Example 1 is that no surface treatment with hydrogen peroxide was performed.

[0127] The difference between Comparative Example 6 and Example 1 is that the modified titanium dioxide and activated carbon are compounded by physical blending.

[0128] From the comparison of Test Examples 1-3, Example 1 and Comparative Examples 1-6, it can be seen that the activated carbon prepared by the present invention has excellent adsorption performance and degradation performance, the photocatalyst and the activated carbon have a strong binding force, even under the action of photocatalysis, the compounded chemical bonds break slowly, effectively ensuring the long-term effect, at the same time, only by in-situ synthesis of polyaniline on titanium dioxide and then forming a cross-linked composite can a better technical effect be achieved. In addition, the degree of polymerization of polyaniline cannot be too large, otherwise it will affect the adsorption of the activated carbon itself due to excessive steric hindrance, which is not conducive to photocatalytic degradation.

[0129] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A process for preparing activated carbon with high adsorption and high degradation performance, characterized in that: The preparation process comprises the following steps: (1) 50-60 parts by weight of sawdust were washed with deionized water, then vacuum dried at 50-60° C. until constant weight was achieved, and crushed to a particle size of 1-2 mm to obtain material A; (2) adding 50-80 parts by weight of phosphoric acid solution and 4-6 parts by weight of boric acid to the material A, stirring for 5-10 minutes at room temperature, then immersing at 70-80° C. for 3-4 hours, filtering, removing the filtrate, and obtaining material B; (3) carbonizing the material B under a nitrogen atmosphere, cooling it naturally to room temperature, then activating it under a carbon dioxide atmosphere, cooling it naturally to room temperature, washing it with deionized water, and finally vacuum drying it at 50-60° C. until constant weight is obtained to obtain material C; (4) Add 150-200 parts by weight of hydrogen peroxide to the material C, stir for 5-10 minutes at room temperature, then soak at 50-60°C for 2-3 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60°C until constant weight, to obtain material D; (5) Add 200-250 parts by weight of anhydrous ethanol, 0.5-1 parts by weight of deionized water and 3-4 parts by weight of vinyltrimethoxysilane to the material D, and then stir at 60-70° C. for 20-24 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60° C. until constant weight, to obtain material E; (6) Add 200-250 parts by weight of deionized water, 12-14 parts by weight of methacrylic acid and 0.5-1 parts by weight of potassium persulfate to the material E, then stir at 80-85° C. for 2-3 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60° C. until constant weight, to obtain material F; (7) Add 200-250 parts by weight of anhydrous ethanol, 8-10 parts by weight of modified titanium dioxide and 2-3 parts by weight of ethylenediamine to the material F, stir and mix at room temperature for 5-10 minutes, adjust the pH to 4 with concentrated sulfuric acid, and then stir at 50-60° C. for 2-3 hours, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60° C. until constant weight, and the preparation is completed; The concentration of the hydrogen peroxide in step (4) is 1-1.5 mol / L; The modified titanium dioxide in step (7) is prepared by the following steps: Step A: adding 80-100 parts by weight of anhydrous ethanol, 0.5-1 parts by weight of deionized water and 1 part by weight of vinyltrimethoxysilane to 5-7 parts by weight of nano titanium dioxide, stirring at 60-70° C. for 20-24 hours, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 60-70° C. until constant weight, to obtain material a; Step B: adding 80-100 parts by weight of deionized water, 2 parts by weight of methacrylic acid and 0.3-0.5 parts by weight of potassium persulfate to the material a, stirring at 70-80° C. for 4-6 hours, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 60-70° C. until constant weight, to obtain material b; Step C: add 80-100 parts by weight of dilute hydrochloric acid solution and 4-5 parts by weight of aniline to the material b, then add 30-40 parts by weight of ammonium persulfate solution dropwise while stirring at 2-4°C, continue stirring at a constant temperature for 5-6 hours after the addition is completed, let stand for 2-3 hours, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 60-70°C until constant weight, and the preparation is completed.

2. The process for preparing activated carbon with high adsorption and high degradation performance according to claim 1, characterized in that: The mass fraction of the phosphoric acid solution in step (2) is 45-50%.

3. The process for preparing activated carbon with high adsorption and high degradation performance according to claim 1, characterized in that: The carbonization in step (3) refers to heating the temperature to 350-400°C at a heating rate of 10-15°C / min and then maintaining the temperature for 1-2 hours; the activation refers to heating the temperature to 500-600°C at a heating rate of 10-15°C / min and then maintaining the temperature for 1-1.5 hours.

4. The process for preparing activated carbon with high adsorption and degradation performance according to claim 1, characterized in that: The particle size of the nano titanium dioxide in step A is 10-50 nm, and the crystal form of the nano titanium dioxide is anatase.

5. The process for preparing activated carbon with high adsorption and high degradation performance according to claim 1, characterized in that: The concentration of the dilute hydrochloric acid solution in step C is 0.1 mol / L.

6. The process for preparing activated carbon with high adsorption and high degradation performance according to claim 1, characterized in that: The dripping rate in step C is controlled at 1-3 drops / s.

7. The process for preparing activated carbon with high adsorption and high degradation performance according to claim 1, characterized in that: The concentration of the ammonium persulfate solution in step C is 0.3-0.35 mol / L.

8. The process for preparing activated carbon with high adsorption and high degradation performance according to claim 1, characterized in that: The mass fraction of the concentrated sulfuric acid in step (7) is 70-75%.

Citation Information

Patent Citations

  • Method for preparing wood activated carbon by phosphoric acid method

    CN102153082A

  • Photocatalytic degradation material of polyaniline-europium doped titanium dioxide and preparation method thereof

    CN112473735A

  • Preparation process and application of shell activated carbon with adsorption and degradation functions

    CN117839633A