A CMP dresser filled with hard particles and a preparation method thereof
By using hard particle filling and chemical vapor deposition diamond coating in CMP trimmer, the problems of high protrusion in the grinding particles, easy detachment of bonding agents and difficult to ensure micropore consistency in the prior art, efficient dressing is achieved Performance and long life trimmer.
Patent Information
- Application Number
- CN202411260519.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-10
AI Technical Summary
During the use of existing CMP trimmers, there are problems such as inconsistent protrusion of the abrasive particles, easy detachment of the bonding agent and complex process, and difficult to guarantee the consistency of micropore size.
CMP trimmer filled with hard particles, including a silicon carbide substrate with micropores with micropores, the distribution density is 0.25-25 pieces/mm2, the Mohs hardness of hard particles is greater than or equal to 6, and the thickness of the covered diamond coating is 3-30μm , the graphite content in the coating is 0.5-5%, and the nitrogen element content is 0.5-8ppm. Diamond coating is formed by chemical vapor deposition technology, and hard particles are evenly arranged on the substrate to improve adhesion and wear resistance.
It improves the dressing performance and service life, ensures the removal ability of the polishing pad and the wear resistance of the substrate, and extends the service life of the dressing device.
Smart Images

Figure CN118769133B_ABST
Abstract
Description
Technical Field
[0001] The present application discloses a CMP dresser filled with hard particles and a preparation method thereof, belonging to the field of semiconductor processing. Background Art
[0002] Chemical mechanical polishing (CMP) is an ultra-precision machining technology that is widely used in integrated circuits, micro-electromechanical systems, optical devices and other fields. In chemical mechanical polishing, a polishing pad is used to remove material from the wafer substrate to flatten the wafer surface, but at the same time, the polishing pad will be worn out. If the polishing pad is replaced frequently, it will inevitably increase the cost, so a CMP dresser is used to dress the polishing pad to reduce the frequency of replacement, thereby reducing costs.
[0003] The common CMP dresser in the prior art is to fix diamond abrasive grains on the substrate, and use the diamond abrasive grains fixed on the dresser to grind the polishing pad to achieve dressing. This type of CMP dresser mainly consists of three parts: substrate, binder, and diamond abrasive grains. The diamond abrasive grains are fixed on the substrate by various fixing methods.
[0004] Patent document 1 (publication number: CN109702651A) discloses a chemical mechanical polishing dresser, specifically disclosed: comprising a base, a plurality of adhesive joints and a plurality of polishing units, the base having a plurality of grooves, the adhesive joints each comprising a sponge disposed in the grooves and a thermosetting adhesive infiltrated into the sponge, the polishing units respectively disposed in the grooves, and each having a plurality of polishing particles, the polishing particles protruding from the grooves and forming a polishing end. The polishing particles may be single crystal diamonds.
[0005] Patent document 1 uses a thermosetting adhesive as a binder. On the one hand, it is difficult to ensure the consistency of the protruding height of the abrasive particles during the manufacturing process of the dresser, which affects the dressing performance; on the other hand, the binder is easy to fall off during the dressing process, reducing its service life.
[0006] The prior art also found CMP dressers that do not use a binder, such as Patent Document 2 (Publication No.: CN113664743A), which discloses a method for manufacturing a CMP diamond dresser, comprising the following steps: step one, cleaning; step two, coating; step three, plating; step four, screening; step five, paving; step six, coating; and step seven, film removal. In step two, the photoresist coated on the stainless steel substrate is patterned using photolithography technology, and the photoresist is retained on the desired pattern. In step three, a Ni film / Cr film / NiCr alloy film is plated on the photolithographic stainless steel substrate using PVD (physical vapor deposition), and the substrate plated with the film is immersed in acetone to form patterned micropores. In step five, the screened diamonds are spread on the patterned stainless steel substrate, and the diamonds are alternately vibrated in the horizontal and vertical directions on a vibration table to uniformly arrange the diamonds in the micropores. In step six, a film is plated on the substrate on which the diamonds are arranged, and the film is plated using physical vapor deposition technology.
[0007] Patent document 2 has a complicated process and it is difficult to ensure the size consistency of its micropores, which seriously affects the finishing performance. In addition, the insufficient bonding force between the substrate and the membrane reduces its service life.
[0008] Therefore, it is hoped that a technical solution can be provided to solve or at least alleviate the above-mentioned deficiencies of the prior art. Summary of the invention
[0009] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a CMP dresser filled with hard particles, which has high dressing performance and service life.
[0010] To achieve the above object, the present invention adopts the following technical solutions:
[0011] A CMP dresser filled with hard particles includes a substrate with micropores, the dresser also includes hard particles protruding from the surface of the substrate and a chemical vapor deposition diamond coating covering the substrate and the hard particles, the hard particles are in contact with the pore walls of the micropores, and the distribution density of the micropores is 0.25-25 / mm 2 The Mohs hardness of the hard particles is greater than or equal to 6, the thickness of the diamond coating is 3-30μm, the graphite content in the diamond coating is 0.5-5%, and the nitrogen content is 0.5-8ppm.
[0012] If the distribution density of micropores is too low, it is easy to cause fewer grooves on the polishing pad, and the grooves are larger, which reduces the removal ability of the polishing pad and increases the loss of the polishing pad; if the distribution density of micropores is too high, it is easy to cause more grooves on the polishing pad, but the grooves are smaller, which reduces the removal ability of the polishing pad. Therefore, the distribution density of micropores is 0.25-25 / mm 2 .
[0013] Hard particles have to withstand great pressure during operation and must have good deformation resistance. When the Mohs hardness of hard particles is too low, their finishing performance and service life are difficult to guarantee. Therefore, the Mohs hardness of hard particles is greater than or equal to 6.
[0014] Chemical vapor deposition diamond coating has the function of protecting the substrate, but when the diamond coating is too thin, it is easy to be worn through during the trimming work, thus reducing the service life; but when the diamond coating is too thick, the adhesion between the diamond coating and the substrate will decrease due to excessive stress, and there is a risk of falling off. Therefore, the thickness of the diamond coating is 3-30μm.
[0015] The right amount of graphite and nitrogen can not only improve the fracture strength and wear ratio of chemical vapor deposition diamond coatings, but also enhance the fracture toughness and avoid diamond brittle cracking; however, graphite and nitrogen tend to gather at the grain boundaries. Too high a graphite content or too much nitrogen will weaken the grain boundary connection in the diamond coating, increase stress and reduce strength. Therefore, the graphite content in the diamond coating is 0.5-5%, and the nitrogen content is 0.5-8ppm.
[0016] Furthermore, the substrate material is silicon carbide. The difference in thermal expansion coefficient between silicon carbide and diamond is small, and carbides are easily formed at the interface to form chemical bonds, so that chemical vapor deposition diamond has excellent adhesion thereon, and it has better rigidity and less deformation during chemical vapor deposition diamond deposition.
[0017] Furthermore, the hard particles are diamond single crystal particles. Diamond single crystal particles not only have a Mohs hardness higher than 6, but also can achieve homoepitaxial and heteroepitaxial growth simultaneously on their surfaces, so the adhesion between the diamond coating and the hard particles is better.
[0018] Furthermore, the chemical vapor deposition diamond coating is a chemical vapor deposition polycrystalline diamond coating, the diamond grain size of the diamond coating is 0.5-15 μm, and the dresser can have higher wear resistance and extend service life.
[0019] Furthermore, the micropores include ceramics.
[0020] Furthermore, the micropores have the same pore size, the same depth and the same spacing, so that the hard particles in the micropores are evenly distributed, so that the micro texture of the surface of the polishing pad being trimmed is uniform, and the trimming performance of the trimmer is guaranteed.
[0021] Furthermore, the micropores are circular in shape, with a pore diameter of 50-250 μm, and a pore depth to pore diameter ratio of 50-80%, which helps to improve cutting performance.
[0022] Furthermore, the protruding height of the hard particles is greater than or equal to 10 μm and less than or equal to the difference between the diameter and the depth of the micropores, so that the hard particles are unlikely to fall off and have higher cutting performance.
[0023] A method for preparing a CMP dresser filled with hard particles comprises the following steps:
[0024] (1) Substrate production: Produce a substrate with micropores, with a distribution density of 0.25-25 / mm 2 ;
[0025] (2) Hard particle placement: clean the substrate and hard particles, ultrasonically vibrate the substrate and hard particles in a diamond powder suspension to roughen the surfaces of the substrate and hard particles, form prefabricated diamond seeds on the surfaces of the substrate and hard particles, and place the hard particles into the micropores on the substrate;
[0026] (3) Diamond coating deposition: Place the substrate in a chemical vapor deposition chamber for chemical vapor deposition to form a diamond coating on the surface of the substrate. The C / H atomic percentage in the diamond coating deposition atmosphere is 0.8%-6%, the N / C atomic percentage is 1.5%-8%, the growth pressure is 3-5kPa, the deposition temperature is 780℃-1050℃, and the diamond coating thickness is 3-30μm. The graphite content in the diamond coating is 0.5-5%, and the nitrogen content is 0.5-8ppm.
[0027] Furthermore, in step (2), after ultrasonic vibration, ceramic powder is added to the micropores. In the subsequent chemical vapor deposition, the hard particles can be consolidated to make them more solid, which is beneficial to prolonging the service life of the trimmer. Preferably, the ceramic powder composition is calculated by weight percentage: Al2O3: 12%, CaO: 14%, BaO: 8.5%, B2O3: 7.6%, Na2O: 9.2%, Bi2O3: 5.4%, MgO: 4.5%, and the rest is SiO2 and unavoidable impurities.
[0028] Furthermore, the micropores in step (1) can be obtained by laser ablation.
[0029] Furthermore, the chemical vapor deposition in step (3) is direct current arc plasma spray chemical vapor deposition, which helps to improve wear resistance.
[0030] Furthermore, step (3) further includes step (4): placing the trimmer into a heating furnace for trimming treatment, wherein the trimming treatment is vacuum heat treatment at a temperature of 400° C. to 800° C. for a holding time of 10 to 30 minutes, followed by cooling in the furnace; this is beneficial to improving trimming properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1It is a structural schematic diagram of the trimmer of the present invention;
[0032] Figure 2 Schematic diagram of the method for preparing a trimmer of the present invention.
[0033] Reference numerals: 1 - chemical vapor deposition diamond coating, 2 - hard particles, 3 - substrate. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The invention will be further described below with reference to examples to further illustrate the method of the present invention and its advantages.
[0036] Example 1
[0037] The hard particle filled CMP dresser includes a silicon carbide substrate with micropores, the dresser also includes silicon dioxide particles protruding from the surface of the substrate and a chemical vapor deposition diamond coating covering the surface of the substrate and the silicon dioxide particles, the silicon dioxide particles are in contact with the pore walls of the micropores, and the distribution density of the micropores is 0.25 / mm 2 The Mohs hardness of the silica particles is 7, the thickness of the diamond coating is 3 μm, the graphite content in the diamond coating is 5%, and the nitrogen content is 8 ppm.
[0038] After testing, the effective cutting point of the trimmer was 100% when the penetration depth of the cutting point was 13 microns. The life test was conducted using the grinding and polishing platform of Applied Materials, with colloidal silica-based slurry and a test pressure of 5 pounds. Wear damage occurred after running 2,600 wafers.
[0039] Example 2
[0040] The hard particle filled CMP dresser includes a silicon carbide substrate with circular micropores, a diamond single crystal particle protruding from the substrate surface, and a chemical vapor deposition diamond coating covering the substrate and the surface of the diamond single crystal particle. The diamond single crystal particle is in contact with the pore wall of the micropore, and the distribution density of the micropore is 12 / mm 2The Mohs hardness of the diamond single crystal particles is 10, the thickness of the diamond coating is 23μm, the graphite content in the diamond coating is 2.6%, the nitrogen content is 3.9ppm, the diamond grain size in the diamond coating is 8.3μm, the micropores have the same pore size, depth and spacing, the pore size is 125μm, the pore depth and pore size ratio is 78%, and the protruding height of the diamond single crystal particles in the micropores is 25μm.
[0041] After testing, the effective cutting point of the trimmer was 100% when the penetration depth of the cutting point was 11 microns. The life test was conducted using the grinding and polishing platform of Applied Materials, with colloidal silica-based slurry and a test pressure of 5 pounds. Wear damage occurred after running 3,680 wafers.
[0042] Example 3
[0043] The hard particle filled CMP dresser includes a silicon carbide substrate with circular micropores, a diamond single crystal particle protruding from the substrate surface, and a chemical vapor deposition polycrystalline diamond coating covering the substrate and the surface of the diamond single crystal particle. The diamond single crystal particle is in contact with the pore wall of the micropore, and the distribution density of the micropore is 4 / mm 2 The Mohs hardness of the diamond single crystal particles is 10, the thickness of the diamond coating is 17μm, the graphite content in the diamond coating is 1.5%, the nitrogen content is 4.9ppm, the diamond grain size in the diamond coating is 5.6μm, the micropores have the same pore size, depth and spacing, the pore size is 180μm, the pore depth and pore size ratio is 65%, and the protruding height of the diamond single crystal particles in the micropores is 51μm.
[0044] After testing, the effective cutting point of the trimmer was 100% when the penetration depth of the cutting point was 7 microns. The life test was conducted using the grinding and polishing platform of Applied Materials, colloidal silica-based slurry, and a test pressure of 5 pounds. Wear damage occurred after running 4,000 wafers.
[0045] Example 4
[0046] The trimmer is prepared as follows:
[0047] (1) Laser ablation is performed on the substrate surface to obtain circular micropores. The laser ablation process parameters are controlled so that the distribution density of the micropores is 25 / mm 2 , the micropores have the same pore size, depth and spacing, the pore size is 98μm, and the ratio of pore depth to pore size is 52%;
[0048] (2) cleaning the substrate and diamond single crystal particles with a Mohs hardness of 10, ultrasonically vibrating the substrate and the diamond single crystal particles in a diamond powder suspension to roughen the surfaces of the substrate and the diamond single crystal particles, forming prefabricated diamond seeds on the surfaces of the substrate and the diamond single crystal particles, and placing the diamond single crystal particles and ceramic powder into micropores on the substrate. The ceramic powder composition is as follows by weight percentage: Al2O3: 12%, CaO: 14%, BaO: 8.5%, B2O3: 7.6%, Na2O: 9.2%, Bi2O3: 5.4%, MgO: 4.5%, and the rest is SiO2 and unavoidable impurities. The protruding height of the diamond single crystal particles is 39 μm.
[0049] (3) placing the substrate in a chemical vapor deposition chamber for direct current arc plasma jet chemical vapor deposition to form a chemical vapor deposition polycrystalline diamond coating on the surface of the substrate, wherein the C / H atomic percentage in the diamond coating deposition atmosphere is 4%, the N / C atomic percentage is 1.5%, the growth gas pressure is 5 kPa, the deposition temperature is 900° C., the diamond coating thickness is 23 μm, the graphite content in the diamond coating is 3.1%, the nitrogen content is 0.9 ppm, and the diamond grain size is 14 μm;
[0050] (4) The dresser is placed in a heating furnace for vacuum heat treatment at a temperature of 540°C for 20 minutes, and then cooled in the furnace.
[0051] After testing, the effective cutting point of the trimmer was 100% when the penetration depth of the cutting point was 6 microns. The life test was conducted using the grinding and polishing platform of Applied Materials, colloidal silica-based slurry, and a test pressure of 5 pounds. Wear damage occurred after running 4,200 wafers.
[0052] Comparative Example 1
[0053] The CMP dresser has a base, an adhesive bonding member and a grinding unit, wherein the base has a plurality of grooves. The adhesive bonding member is a sponge disposed in the groove and a thermosetting adhesive infiltrated into the sponge. The grinding unit is disposed in correspondence with the groove and has a base and a plurality of single crystal diamonds disposed on the base, wherein the single crystal diamonds protrude from the groove, and the height of the grinding end from the base is between 30 microns and 55 microns.
[0054] After testing, the effective cutting point of the trimmer was 100% when the penetration depth of the cutting point was 24 microns. The life test was conducted using the grinding and polishing platform of Applied Materials, with colloidal silica-based slurry and a test pressure of 5 pounds. Wear damage occurred after running 1,089 wafers.
[0055] Comparative Example 2
[0056] The CMP dresser includes a silicon carbide substrate with circular micropores, silicon dioxide particles protruding from the substrate surface, and a chemical vapor deposition diamond coating covering the substrate and the surface of the silicon dioxide particles. The silicon dioxide particles are in contact with the pore walls of the micropores. The distribution density of the micropores is 26 / mm. 2 The thickness of the diamond coating is 2μm, the graphite content in the diamond coating is 0.2%, and the nitrogen content is 0.4ppm.
[0057] The trimmer was tested to have an effective cutting point of 100% when the cutting point penetration depth was 15 microns. The life test was conducted using the grinding and polishing platform of Applied Materials, with colloidal silica-based slurry and a test pressure of 5 pounds. Wear damage occurred after running 2,194 wafers.
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A CMP conditioner filled with hard particles, the conditioner comprising a substrate, characterized in that: The substrate has micropores, and the trimmer also includes hard particles protruding from the surface of the substrate and a chemical vapor deposition diamond coating covering the substrate and the hard particles. The hard particles are in contact with the pore walls of the micropores, and the distribution density of the micropores is 0.25-25 / mm 2 , the Mohs hardness of the hard particles is greater than or equal to 6, the thickness of the diamond coating is 3-30μm, the graphite content in the diamond coating is 0.5-5%, and the nitrogen content is 0.5-8ppm; The substrate is silicon carbide, the hard particles are diamond single crystal particles, the chemical vapor deposition diamond coating is a chemical vapor deposition polycrystalline diamond coating, and the diamond grain size of the diamond coating is 0.5-15 μm; The protrusion height of the hard particles is greater than or equal to 10 μm, and the protrusion height of the hard particles is less than or equal to the difference between the pore diameter and the pore depth of the micropore.
2. The trimmer according to claim 1, characterized in that The micropores also include ceramics.
3. The trimmer according to claim 1, characterized in that The microwells have the same pore diameter, the same depth, and the same spacing.
4. The trimmer according to claim 1, characterized in that The micropores are circular in shape, with a pore diameter of 50-250 μm and a pore depth to pore diameter ratio of 50-80%.
5. The method for preparing a dresser according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Substrate preparation: preparing a substrate with micropores; (2) Hard particle placement: clean the substrate and hard particles, ultrasonically vibrate the substrate and hard particles in a diamond powder suspension to roughen the surfaces of the substrate and hard particles, form prefabricated diamond seeds on the surfaces of the substrate and hard particles, and place the hard particles into the micropores on the substrate; (3) Diamond coating deposition: Place the substrate in a chemical vapor deposition chamber for chemical vapor deposition to form a diamond coating on the surface of the substrate. The C / H atomic percentage in the diamond coating deposition atmosphere is 0.8%-6%, the N / C atomic percentage is 1.5%-8%, the growth gas pressure is 3-5kPa, and the deposition temperature is 780℃-1050℃.
6. The preparation method according to claim 5, characterized in that: In step (2), after ultrasonic vibration, ceramic powder is added into the micropores, and the composition of the ceramic powder is as follows by weight percentage: Al2O3: 12%, CaO: 14%, BaO: 8.5%, B2O3: 7.6%, Na2O: 9.2%, Bi2O3: 5.4%, MgO: 4.5%, and the rest is SiO2 and unavoidable impurities.
7. The preparation method according to claim 5, characterized in that: The micropores in step (1) are obtained by laser ablation, and the chemical vapor deposition in step (3) is direct current arc plasma spray chemical vapor deposition.
8. The preparation method according to claim 5, characterized in that: The step (3) also includes the step (4): placing the trimmer into a heating furnace for shaping treatment, wherein the shaping treatment is vacuum heat treatment at a temperature of 400° C. to 800° C. for a holding time of 10 to 30 minutes, and cooling with the furnace.