Cellulose derivative and preparation method thereof

Through the modification and aminolysis reaction of anhydride groups of trimellitic anhydride acyl chloride and cellulose, combined with imidization treatment, the problems of high solvent cost, difficult separation and poor performance controllability in the preparation process of cellulose derivatives are solved, and the problem is achieved Efficient preparation of water-soluble and water-insoluble cellulose derivatives with excellent processing properties and controllability.

CN118772297APending Publication Date: 2024-10-15TSINGHUA UNIVERSITY
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410983150.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the preparation process of cellulose derivatives in the prior art, there are problems such as high solvent cost, difficult separation, cumbersome separation steps, difficulty in product recovery, and poor performance controllability, especially the processing properties of water-soluble and water-insoluble cellulose derivatives. and insufficient water resistance.

Method used

Trimellitic anhydride acyl chloride and cellulose are used to modify the acid anhydride group, and an amide group is generated through an aminolysis reaction to form a water-soluble cellulose derivative, which can then be converted into a water-insoluble cellulose derivative through an imidization reaction. Ionic liquids and catalysts optimize reaction conditions, simplify preparation processes and improve separation efficiency.

Benefits of technology

It achieves excellent solubility and good processing performance of cellulose derivatives in water, while reducing production costs, simplifying the preparation process, and making the degree of substitution of cellulose hydroxyl groups controllable, making it suitable for different application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772297A_ABST
    Figure CN118772297A_ABST
Patent Text Reader

Abstract

The invention relates to a cellulose derivative and a preparation method thereof. The cellulose derivative of the present invention contains an amide group and a carboxyl group and / or an ammonium salt thereof, has excellent solubility in water, and can obtain a non-water-soluble cellulose derivative after imidization. According to the preparation method, renewable raw materials and recyclable solvents are adopted, and the process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a cellulose derivative and a preparation method thereof, and belongs to the technical field of chemical engineering. Background Art

[0002] The world population has increased from 3.7 billion in 1970 to 7.9 billion in 2021. According to forecasts, the world population will reach 9 billion in 2050 and 11.2 billion in 2100. The continuous increase in population will bring many new tests and challenges to the world's food supply, energy supply, and basic necessities supply.

[0003] From 1978 to 2017, China's energy consumption increased from 397.1 million tons of oil equivalent to 3.1 billion tons of oil equivalent, with an average annual growth of 5.4%. With the rapid development of China's economy, energy consumption will continue to grow at a high speed. When analyzing the composition of my country's energy structure, traditional coal energy still occupies the majority in my country's energy structure.

[0004] Compared with traditional petrochemical energy, the widely existing biomass renewable resources in nature can be considered as an inexhaustible and valuable wealth, and the effective development and utilization of these resources is of great value and significance. Among them, cellulose is the most abundant renewable resource, with an annual global cellulose production of 1.5 trillion tons. However, the actual development and utilization of cellulose resources is very limited.

[0005]

[0006] The above formula (a) shows the structure of cellulose, in which each anhydroglucose unit (C6H 10 O5) has three hydroxyl groups and is thermodynamically in the preferred 4C1 conformation. In this way, the two glucose units rotate alternately to form a thermodynamically stable cellobiose structure in the plane. The molecular formula of cellulose is (C6H 10 O5)n, the value of n is not fixed, and the chain length varies with the source of the raw materials and the processing method. For wood pulp, the usual degree of polymerization is 300-1700, and in cotton it is usually 800-10000. The degree of polymerization of regenerated cellulose is usually 250-500. Microcrystalline cellulose is formed by acid treatment or catalytic hydrolysis, and its degree of polymerization is generally 150-300. When the degree of polymerization reaches 20-30, the glucose chain has all the characteristics of cellulose.

[0007] Cellulose is a white powdery solid at room temperature. Due to its supramolecular structure, it is insoluble in water and common organic and inorganic solvents. Its thermal decomposition temperature is between 315 and 400°C, and it will decompose before melting when heated, which brings certain difficulties to its application.

[0008] There are two main methods for utilizing cellulose: directly dissolving regenerated cellulose in a special solvent and generating cellulose derivatives through a reaction.

[0009] At present, the viscose production of cellulose in industry still dominates. However, a large amount of carbon disulfide and sulfuric acid are inevitably used in the preparation of viscose fibers, which will also produce a large amount of sulfide gas waste, wastewater and toxic waste residue, causing serious damage to the environment. Non-patent document 1 records that at 130°C, N-methylmorpholine-N-oxide (NMMO) can directly dissolve cellulose. This process does not require complex chemical reaction changes and can be directly spun. Non-patent document 2 records that in 1979, Dawsey TR Laboratory first reported that a mixture of lithium chloride (hereinafter sometimes referred to as LiCl) and N,N-dimethylacetamide (hereinafter sometimes referred to as DMAc) produced a small amount of or no degradation of cellulose solution under normal conditions. This solvent has been used to dissolve proteins, synthetic polyamides and chitin

[19] . In addition, special solvents such as ionic liquids for dissolving cellulose have also been widely used and received attention recently. However, the direct use of solvents to dissolve regenerated cellulose has the problems of high solvent costs and difficulty in solvent recovery and separation. In addition, the existing technologies for preparing cellulose derivatives using ionic liquids have the following disadvantages: the prepared cellulose derivative products require special and cumbersome separation steps to be separated from the reaction system, such as adding a precipitant separately, and the separated solution also needs to be distilled to separate the components, and the solution after separating the reaction product cannot be directly used again for the preparation of the cellulose derivative.

[0010] There are mainly two types of cellulose derivatives: esterified cellulose and etherified cellulose. Typical industrial esterified celluloses include cellulose nitrate, cellulose xanthate, cellulose sulfate, cellulose acetate, cellulose acetate propionate, cellulose acetate butyrate, etc., which are water-insoluble celluloses. Common etherified celluloses include methyl cellulose, sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, etc., which are water-soluble cellulose materials. However, the preparation of these celluloses often has problems such as difficulty in separation during the preparation process and limited processability of the prepared materials, and has certain limitations. Therefore, it is expected to develop cellulose derivatives that are easy to separate during the preparation process and have excellent processability of the prepared materials.

[0011] In addition, for cellulose derivatives, the position of the introduction of the modified group in the cellulose derivatives and the influence of the positional relationship between the various modified groups on their performance have not attracted much attention. For example, the positions of the carboxyl group and the amide group in the anhydroglucose unit and the positional relationship between the carboxyl group and the amide group in the amide-modified carboxyl cellulose A prepared in Patent Document 1, such as the number of carbon atoms spaced between the carboxyl group and the amide group, are random, which makes the performance of the amide-modified carboxyl cellulose A and the cellulose derivative containing the imide group formed by further imidization reaction, such as water solubility, poorly controllable.

[0012] Citations

[0013] Non-patent literature:

[0014] Non-patent literature 1: Fink HP, Weigel P, Purz HJ, et al. Structure formation of regenerated cellulose materials from NMMO-solutions [J]. Prog Polym Sci, 2001, 26(9): 1473-1524.

[0015] Non-patent document 2: Dawsey TR, McCormick C L. The Lithium Chloride / Dimethylacetamide Solvent for Cellulose: A Literature Review [J]. Journal of Macromolecular Science, Part C, 2006, 30(3-4): 405-440.

[0016] Patent Literature

[0017] Patent document 1: JP5148456B2 Summary of the invention

[0018] Problem that the invention aims to solve

[0019] In view of the above problems existing in the prior art, the technical problem to be solved by the present invention is to provide a water-soluble cellulose derivative having excellent solubility in water and good processing performance after dissolution, and a water-insoluble cellulose derivative having excellent water resistance. In addition, the technical problem to be solved by the present invention is to provide a method for preparing the above cellulose derivatives, which has a simple and feasible preparation process, convenient separation operation, convenient recovery of the solution after product separation and convenient recycling, and low production cost.

[0020] Solutions for solving problems

[0021] In order to solve the above technical problems, the present inventors conducted in-depth research and found that the above technical problems can be solved by modifying cellulose with both trimellitic anhydride chloride and ammonia.

[0022] Specifically, the present invention solves the problem of the present invention through the following solutions.

[0023] [1] A cellulose derivative, characterized in that it comprises a structure represented by the following formula (1):

[0024]

[0025] In the formula (1), any one of X1 and X2 is -NH2, and the other of X1 and X2 is -OH or -O - NH4 + ;

[0026] * is the position of the ring bond to the anhydroglucose unit of cellulose, and the oxygen atom connected to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose.

[0027] [2] The cellulose derivative according to [1], wherein the degree of substitution of cellulose hydroxyl groups in the cellulose derivative is 0.1 or more, preferably 0.3 or more, more preferably 0.5 or more, and even more preferably 0.8 or more.

[0028] [3] A method for preparing a cellulose derivative according to [1] or [2], characterized by comprising the following steps:

[0029] a) dissolving cellulose in a solvent to obtain a cellulose solution;

[0030] b) mixing the cellulose solution with trimellitic anhydride chloride, and optionally with a catalyst, so that the trimellitic anhydride chloride reacts with the cellulose to obtain anhydride group-modified cellulose;

[0031] c) contacting the anhydride group-modified cellulose with ammonia and performing an aminolysis reaction to obtain the cellulose derivative, and the cellulose derivative is precipitated to the bottom of the reaction system in a solid state;

[0032] d) optionally, separating the cellulose derivative from the reaction system of step c);

[0033] e) optionally, washing the cellulose derivative separated in step d) with a solvent.

[0034] [4] The preparation method according to [3] is characterized in that the solvent in step a) contains an ionic liquid, and the ionic liquid is 1-butyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium acetate, 1-butyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium chloride, or N,N-dimethylacetamide / lithium chloride (DMAc / LiCl), preferably N,N-dimethylacetamide / lithium chloride (DMAc / LiCl); When the ionic liquid is 1-butyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium acetate, 1-butyl-3-methylimidazolium chloride, or 1-allyl-3-methylimidazolium chloride, the solvent optionally comprises a cosolvent, which is at least one selected from dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), 1,3-dimethyl-2-imidazolidinone (DMI) and N,N-dimethylacetamide (DMAc).

[0035] [5] The preparation method according to [3] or [4] is characterized in that in the step b), the molar feed ratio of the trimellitic anhydride chloride to the anhydrous glucose unit of the cellulose is (0.5-6):1, preferably (0.5-5):1, more preferably (0.6-4):1, and even more preferably (1-3.9):1; the reaction temperature in the step b) is 18-100°C, preferably 20-80°C, more preferably 25-70°C; the reaction time in the step b) is 0.5-12 hours, preferably 1-10 hours.

[0036] [6] The preparation method according to any one of [3] to [5] is characterized in that the catalyst is at least one selected from pyridine and its derivatives and amines; preferably at least one selected from pyridine, 4-dimethylaminopyridine, ethylenediamine, and triethylamine; the amount of the catalyst used is 1% to 40% relative to the mass of trimellitic anhydride chloride, preferably 2% to 35%, and more preferably 2.5 to 31%.

[0037] [7] The preparation method according to any one of [3] to [6], characterized in that in the step c), the time of the aminolysis reaction is 1 to 40 minutes, preferably 1 to 30 minutes, and more preferably 5 to 30 minutes; and the amination rate after the aminolysis reaction is 90% or more, preferably 95% or more.

[0038] [8] The preparation method according to any one of [3] to [7], characterized in that in step a), the cellulose is at least one selected from microcrystalline cellulose, nanocellulose, α-cellulose, cotton cellulose, wood cellulose, and bacterial cellulose.

[0039] [9] The preparation method according to any one of [3] to [8], characterized in that in step e), the solvent used for the washing is at least one selected from ketone solvents, alcohol solvents, and water, preferably at least one selected from acetone, butanone, methyl isobutyl ketone, methanol, ethanol, isopropanol, and water.

[0040]

[10] An imidized cellulose derivative, characterized in that it comprises a structure represented by the following formula (2):

[0041]

[0042] In the formula (2), * is the position of bonding to the ring of the anhydroglucose unit of cellulose, and the oxygen atom bonded to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose.

[0043]

[11] The imidized cellulose derivative according to

[10] , wherein the degree of substitution of cellulose hydroxyl groups in the cellulose derivative is 0.1 or more, preferably 0.3 or more, more preferably 0.5 or more, and even more preferably 0.8 or more.

[0044]

[12] A method for preparing an imidized cellulose derivative according to

[10] or

[11] , characterized by comprising the following steps:

[0045] The cellulose derivative is produced by the production method according to any one of [3] to [9], and

[0046] subjecting the cellulose derivative to an imidization reaction;

[0047] Preferably, the temperature of the imidization reaction is 150 to 180° C., preferably 160 to 180° C.; the time of the imidization reaction is 1 to 10 hours, preferably 2 to 8 hours, more preferably 3 to 6 hours.

[0048] Effects of the Invention

[0049] The cellulose derivatives of the present invention comprising an amide group and a carboxyl group and / or an ammonium salt thereof (hereinafter, also referred to as the water-soluble cellulose derivatives of the present invention or the cellulose derivatives of the present invention) have excellent solubility in water and good processing properties after dissolution. In addition, the cellulose derivatives of the present invention can be further converted into water-insoluble cellulose derivatives comprising an imide group (hereinafter, also referred to as water-insoluble cellulose derivatives of the present invention or imidized cellulose derivatives) by imidization (e.g., by heating), which has a wider processing prospect.

[0050] In addition, the cellulose hydroxyl substitution degree of both the cellulose derivative and the imidized cellulose derivative of the present invention is controllable, and cellulose products with different hydroxyl substitution degrees can be prepared according to demand. Moreover, the raw materials are easy to obtain, low in cost and renewable.

[0051] The preparation method of the invention does not require the addition of a precipitant, has a simple and feasible preparation process, is convenient for separation operation, is convenient for recovering the solution after product separation, and the recovered solution can be easily reused in the preparation method, thereby significantly reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 This is a photograph of a 10 wt % aqueous solution of a water-soluble cellulose derivative obtained in Example 1.

[0053] Figure 2 This is the infrared spectrum of the water-soluble cellulose derivative obtained in Example 1.

[0054] Figure 3 This is the hydrogen nuclear magnetic resonance spectrum of the product of the reaction between the anhydride group-modified cellulose obtained in Example 1 and excess ethanol.

[0055] Figure 4 This is a photograph of a colorless transparent film obtained by using the water-soluble cellulose derivative obtained in Example 1 in the evaluation of water solubility.

[0056] Figure 5 This is a photograph of the water-soluble cellulose derivative obtained in Example 2.

[0057] Figure 6 This is a photograph of the imidized cellulose derivative obtained in Example 2. DETAILED DESCRIPTION

[0058] The following is a detailed description of the present invention. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. Any embodiment described as "representative" here does not need to be interpreted as being superior or better than other embodiments.

[0059] <Terms and Definitions>

[0060] In the present specification, the term "alkyl group" includes a linear, branched or cyclic alkyl group, unless otherwise specifically stated.

[0061] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0062] In this specification, the numerical range expressed using "above" or "below" means a numerical range including the number.

[0063] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0064] In this specification, the use of "optionally" or "optionally" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.

[0065] In this specification, when "room temperature" is used, the temperature may be 15 to 25°C.

[0066] In this specification, the unit names used are all international standard unit names, and unless otherwise stated, the "%" used indicates weight or mass percentage.

[0067] In this specification, the references to "preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0068] <First embodiment>

[0069] <Cellulose derivative containing an amide group and a carboxyl group and / or an ammonium salt thereof>

[0070] An object of the present invention is to provide a cellulose derivative comprising a structure represented by the following formula (1):

[0071]

[0072] In formula (1), any one of X1 and X2 is -NH2, and the other of X1 and X2 is -OH or -O - NH4 + ;

[0073] * is the position of the ring bond to the anhydroglucose unit of cellulose, and the oxygen atom connected to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose.

[0074] In one embodiment, the cellulose derivative of the present invention has a main chain structure represented by the above formula (a), and at least part of the hydroxyl groups are replaced by the structure of the above formula (1).

[0075] In one embodiment, the degree of substitution of cellulose hydroxyl groups in the cellulose derivative is 0.1 or more, preferably 0.3 or more, more preferably 0.5 or more, and even more preferably 0.8 or more. The upper limit of the degree of substitution of cellulose hydroxyl groups is 3.0 or less. In addition, different uses of cellulose derivatives have different requirements for the degree of substitution of cellulose hydroxyl groups. Therefore, the range of the degree of substitution of cellulose hydroxyl groups can be selected according to the use of the cellulose derivative, for example, 0.1-3.0, 0.3-3.0, 0.5-3.0, 0.3-2.8, 0.5-2.8, 0.3-2.6, 0.5-2.6, 0.5-2.4, 0.5-2.1, 0.8-1.8.

[0076] The "degree of hydroxyl substitution of cellulose" in the first embodiment of the present invention refers to the average number of hydroxyl groups in each anhydrous glucose unit of cellulose replaced by the structure shown in formula (1). For example, when an average of 1 of the three hydroxyl groups in each anhydrous glucose unit is replaced by the structure shown in formula (1), the degree of hydroxyl substitution of cellulose is 1; when an average of 1.5 of the three hydroxyl groups in each anhydrous glucose unit are replaced by the structure shown in formula (1), the degree of hydroxyl substitution of cellulose is 1.5; and so on, until all the three hydroxyl groups in the anhydrous glucose unit are replaced by the structure shown in formula (1), that is, the maximum degree of hydroxyl substitution of cellulose is 3.

[0077] The cellulose derivative of the present invention may contain only one structure satisfying the above formula (1), or may contain two or more structures satisfying the above formula (1) at the same time.

[0078] In the cellulose derivative of the present invention, the position of -NH2 is not particularly limited as long as it is any one of X1 and X2, and the other of X1 and X2 is -OH or -O. - NH4 + .

[0079] In the present invention, the cellulose derivatives contain the structure represented by formula (1) to introduce amide groups, carboxyl groups and / or ammonium salts thereof, so that the cellulose derivatives have excellent solubility in water and good processing properties after being dissolved.

[0080] <Second Implementation Method>

[0081] <Method for producing cellulose derivative>

[0082] Another object of the present invention is to provide a method for preparing the cellulose derivative of the first embodiment, comprising the following steps:

[0083] a) dissolving cellulose in a solvent to obtain a cellulose solution;

[0084] b) mixing the cellulose solution with trimellitic anhydride chloride, and optionally with a catalyst, and reacting the trimellitic anhydride chloride with the cellulose to obtain anhydride group-modified cellulose, wherein the reaction of the trimellitic anhydride chloride with the cellulose is schematically shown by the following reaction formula (b):

[0085]

[0086] In reaction formula (b), -OH in *-OH represents -OH in anhydroglucose unit of cellulose, * in *-OH and * in the structural formula of the reaction product (cellulose modified by anhydride group) are both positions of ring bonding with anhydroglucose unit of cellulose, and the oxygen atom connected to * in the structural formula of the reaction product (cellulose modified by anhydride group) originates from the hydroxyl group in anhydroglucose unit of cellulose;

[0087] c) contacting the anhydride group-modified cellulose with ammonia and performing an aminolysis reaction to obtain the cellulose derivative, and the cellulose derivative is precipitated to the bottom of the reaction system in a solid state, wherein the aminolysis reaction is schematically shown by the following reaction formula (c):

[0088]

[0089] In reaction formula (c), any one of X1 and X2 is -NH2, and the other of X1 and X2 is -OH or -O - NH4 + , * is the position of the ring bond with the anhydroglucose unit of cellulose, and the oxygen atom connected to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose;

[0090] d) optionally, separating the cellulose derivative from the reaction system of step c);

[0091] e) optionally, washing the cellulose derivative separated in step d) with a solvent.

[0092] The preparation method is described in detail below.

[0093] Step a)

[0094] (Cellulose)

[0095] In one embodiment, the cellulose is at least one selected from microcrystalline cellulose, nanocellulose, α-cellulose, cotton cellulose, wood cellulose, and bacterial cellulose.

[0096] As the raw material of cellulose in step a), natural cellulose extracted from plants or synthetic cellulose can be used, and biomass and fiber fabrics containing cellulose can also be used.

[0097] In one embodiment, as the raw material of cellulose, biomass containing cellulose, fiber fabrics, etc. can be used. Specifically, refined cotton pulp, silver star pulp, cotton linters, bagasse, (waste) cotton cloth, wheat straw, etc. can be used, especially from the perspective of saving resources, waste cotton cloth, wheat straw, etc. can be used.

[0098] In addition, the cellulose raw material can be optionally subjected to one or more of the following operations: acid treatment, alkali treatment, washing, drying, etc., before being dissolved in the solvent, as required. For example, the cotton linters and cotton cloth (e.g., waste cotton cloth) can be optionally washed before being dissolved in the solvent, for example, using water or an alkali solution, preferably a 5% to 10% sodium hydroxide solution for washing pretreatment (the number of washing times can be determined as required, for example, 1 to 5 times, and for example, 2 to 4 times), to remove impurities, and then dried.

[0099] In the embodiment where biomass and / or fiber fabric containing cellulose is used as the raw material of cellulose, the biomass and / or fiber fabric containing cellulose may also be directly dissolved in a solvent in step a) to obtain a cellulose solution.

[0100] In one embodiment, the preparation method of the present invention further comprises the step of extracting cellulose from biomass and / or fiber fabric by extraction operation before step a). After the cellulose is extracted, the cellulose is dissolved in a solvent. For example, for biomass such as bagasse and wheat straw, in order to improve the purity of the product obtained by the above preparation method and reduce impurities in the solvent recovered in step d), it is preferred to extract cellulose therefrom and then dissolve the cellulose in step a).

[0101] In one embodiment, the degree of polymerization of cellulose (the number of anhydroglucose units in cellulose) ranges from 100 to 3000, preferably from 500 to 2900, and more preferably from 600 to 2700.

[0102] (Solvent)

[0103] In the method for preparing a cellulose derivative of the present invention, there are no particular limitations on the method for dissolving cellulose in step a) and the solvent used, as long as cellulose can be dissolved in the solvent.

[0104] In one embodiment, the solvent in step a) comprises an ionic liquid, which is 1-butyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium acetate, 1-butyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium chloride, or N,N-dimethylacetamide / lithium chloride (DMAc / LiCl), preferably N,N-dimethylacetamide / lithium chloride (DMAc / LiCl); wherein when the ionic liquid is 1-butyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium acetate, 1-butyl-3-methylimidazolium chloride, or 1-allyl-3-methylimidazolium chloride, the solvent optionally comprises a co-solvent, which is at least one selected from dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), 1,3-dimethyl-2-imidazolidinone (DMI) and N,N-dimethylacetamide (DMAc).

[0105] Specifically, when the ionic liquid is an imidazolium salt ionic liquid and the solvent includes a cosolvent, the mass ratio of the ionic liquid to the cosolvent may be 1:1 to 1:3, preferably 1:1.5 to 1:2.5, and more preferably 1:1.6 to 1:2.

[0106] In a preferred embodiment, the solvent is N,N-dimethylacetamide / lithium chloride (DMAc / LiCl), which is inexpensive, thereby significantly reducing production costs.

[0107] In the embodiment where the solvent is N,N-dimethylacetamide / lithium chloride (DMAc / LiCl), the content of lithium chloride is 4% to 12%, preferably 5% to 9%, and more preferably 5 to 8%, relative to the total mass of the solvent.

[0108] In an embodiment where the solvent is N,N-dimethylacetamide / lithium chloride (DMAc / LiCl), the solvent can be prepared in advance and the cellulose can be dissolved in the solvent; or, instead of premixing N,N-dimethylacetamide with lithium chloride, both N,N-dimethylacetamide and lithium chloride can be mixed directly with cellulose simultaneously to dissolve the cellulose (e.g., Example 1 below).

[0109] (Dissolution conditions)

[0110] The dissolution in step a) can be carried out at room temperature, or heated as needed, for example, heated to 50-110°C, for example, heated to 55°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C; preferably, heated to 60-100°C.

[0111] (Cellulose solution)

[0112] In the cellulose solution obtained in step a), the mass percentage concentration of cellulose is 0.5% to 5%, preferably 0.5% to 4.5%, and more preferably 2 to 3%, based on the total mass of the cellulose solution.

[0113] Step b)

[0114] (Ratio of trimellitic anhydride chloride to cellulose)

[0115] The molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose can be adjusted according to the requirements of the water solubility of the cellulose derivative, the processing performance after dissolution, etc.

[0116] In one embodiment, the molar feed ratio of trimellitic anhydride chloride to anhydrous glucose units of cellulose is (0.5-6):1, preferably (0.5-5):1, more preferably (0.6-4):1, and even more preferably (1-3.9):1.

[0117] (catalyst)

[0118] In the method for preparing the cellulose derivative of the present invention, a catalyst is optionally used in step b).

[0119] In one embodiment, a catalyst is used in step b), and the catalyst is at least one selected from pyridine (C5H5N) and its derivatives and amines, preferably at least one selected from pyridine (C5H5N), 4-dimethylaminopyridine, ethylenediamine, and triethylamine.

[0120] In one embodiment, a catalyst is used in step b), and the amount of the catalyst used is 1% to 40% relative to the mass of trimellitic anhydride chloride, preferably 2% to 35%, more preferably 2.5 to 31%.

[0121] (Reaction Conditions)

[0122] There is no particular limitation on the reaction conditions in step b), and they can be adjusted according to actual needs. For example, the reaction is carried out under stirring at a stirring speed of 100 to 200 rpm. The reaction temperature in step b) can be 18 to 100° C., preferably 20 to 80° C., and more preferably 25 to 70° C. The reaction time in step b) can be 0.5 to 12 hours, and preferably 1 to 10 hours.

[0123] In addition, in order to reduce the residue of trimellitic anhydride chloride in the solution after the reaction in step b), preferably, after the trimellitic anhydride chloride reacts with cellulose in step b), the conversion rate of trimellitic anhydride chloride is 65% or more, preferably 75% or more, more preferably 85% or more, still more preferably 95% or more, and even more preferably 98% or more.

[0124] The conversion rate of trimellitic anhydride chloride can be controlled by the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose, the reaction temperature, the reaction time, and whether a catalyst is added. If necessary, more than one of the above factors can be adjusted simultaneously to control the conversion rate of trimellitic anhydride chloride.

[0125] Specifically, under the same reaction temperature, reaction time, and catalytic conditions, as the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose increases, the conversion rate of trimellitic anhydride chloride decreases. In particular, when the molar feed ratio exceeds 3:1, the conversion rate of trimellitic anhydride chloride decreases significantly as the molar feed ratio increases.

[0126] In addition, the addition of a catalyst and the increase in the reaction temperature within the reaction temperature range of step b) will increase the reaction rate, thereby shortening the time required to achieve the same conversion rate of trimellitic anhydride chloride.

[0127] When the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose, the reaction temperature, and the catalytic conditions are all the same, as the reaction time goes by, the conversion rate of trimellitic anhydride chloride gradually increases until it becomes constant.

[0128] Step c)

[0129] (ammonia)

[0130] The ammonia used in step c) refers to a substance with a chemical formula of NH3. In the method for preparing a cellulose derivative of the present invention, ammonia gas or ammonia water can be used, as long as the ammonia decomposition reaction can be carried out and preferably the desired amination rate can be achieved. There is no particular limitation on the ammonia concentration in the ammonia water, and any commercially available product can be used. Preferably, the concentration of the ammonia water (25°C) is 25% to 40% by mass, more preferably, 28% to 37% by mass.

[0131] (Reaction Conditions)

[0132] There is no particular limitation on the conditions of the ammonolysis reaction in step c), and they can be adjusted according to actual needs. For example, the temperature of the ammonolysis reaction is usually below 100° C., preferably 0 to 80° C., and more preferably 15 to 60° C. The time of the ammonolysis reaction is usually 1 to 40 minutes, preferably 1 to 30 minutes, and more preferably 5 to 30 minutes.

[0133] In the method for preparing the cellulose derivative of the present invention, after step b), the temperature of the solution of cellulose modified with anhydride groups is optionally adjusted to the temperature of the aminolysis reaction to carry out the aminolysis reaction of step c). When the temperature of the solution of cellulose modified with anhydride groups prepared in step b) is lower than 100° C., the temperature adjustment operation may be omitted and the aminolysis reaction of step c) may be directly carried out.

[0134] Preferably, the amination rate after the aminolysis reaction is 60% or more, more preferably 80% or more.

[0135] In this specification, the "amination rate" is the molar percentage of anhydride groups that react with two NH3 molecules to form amic acid ammonium salt in step c) relative to the total amount of anhydride groups in the cellulose modified with anhydride groups before the aminolysis reaction.

[0136] In step c), after the aminolysis reaction, the cellulose derivative containing amide groups and carboxyl groups and / or ammonium salts thereof obtained by the aminolysis reaction is precipitated to the bottom of the reaction system in a solid state.

[0137] Step d)

[0138] The method for preparing the cellulose derivative of the present invention optionally comprises step d) separating the cellulose derivative from the reaction system of step c). Usually, the separation is performed by filtering, centrifuging, etc. Preferably, the cellulose derivative containing the amide group and the carboxyl group and / or the ammonium salt thereof is separated by filtering.

[0139] In the method for preparing the cellulose derivative of the present invention, in step d), after the cellulose derivative containing the amide group and the carboxyl group and / or its ammonium salt is separated by filtration, centrifugal separation or the like, the solution after the separation of the product is recovered, and the recovered solution can be used again for the preparation of the cellulose derivative of the present invention. Wherein, when the aminolysis reaction in step c) uses ammonia gas, the recovered solution in step d) can be directly used again for the preparation of the cellulose derivative of the present invention, that is, directly recycled and reused. When the aminolysis reaction in step c) uses ammonia water, the recovered solution in step d) needs to be removed from the water introduced by the ammonia water before being used for the preparation of the cellulose derivative of the present invention.

[0140] Step e)

[0141] The method for preparing the cellulose derivative of the present invention optionally comprises step e) washing the cellulose derivative filtered out in step d) with a solvent. The solvent used for washing the cellulose derivative is at least one selected from ketone solvents, alcohol solvents, and water, preferably at least one selected from acetone, butanone, methyl isobutyl ketone, methanol, ethanol, isopropanol, and water.

[0142] The raw materials used in the preparation method of the cellulose derivative of the present invention are renewable, the preparation process is simple and feasible, the separation operation is convenient, the solvent recovery is convenient and the recovered solvent can be recycled as the solvent of the preparation method, and the production cost is significantly reduced.

[0143] <Third Implementation Method>

[0144] <Imidized cellulose derivatives>

[0145] Another object of the present invention is to provide an imidized cellulose derivative comprising a structure represented by the following formula (2):

[0146]

[0147] In formula (2), * is the position of the ring bond to the anhydroglucose unit of cellulose, and the oxygen atom connected to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose.

[0148] In one embodiment, the degree of substitution of cellulose hydroxyl groups in the imidized cellulose derivative is 0.1 or more, preferably 0.3 or more, more preferably 0.5 or more, and even more preferably 0.8 or more. The upper limit of the degree of substitution of cellulose hydroxyl groups is 3.0 or less. In addition, different uses of the imidized cellulose derivatives have different requirements for the degree of substitution of cellulose hydroxyl groups. Therefore, the range of the degree of substitution of cellulose hydroxyl groups can be selected according to the use of the imidized cellulose derivative, for example, 0.1-3.0, 0.3-3.0, 0.5-3.0, 0.3-2.8, 0.5-2.8, 0.3-2.6, 0.5-2.6, 0.5-2.4, 0.5-2.1, 0.8-1.8.

[0149] The "degree of hydroxyl substitution of cellulose" in the third embodiment of the present invention refers to the average number of hydroxyl groups in each anhydrous glucose unit of cellulose replaced by the structure shown in formula (2). For example, when an average of 1 of the three hydroxyl groups in each anhydrous glucose unit is replaced by the structure shown in formula (2), the degree of hydroxyl substitution of cellulose is 1; when an average of 1.5 of the three hydroxyl groups in each anhydrous glucose unit are replaced by the structure shown in formula (2), the degree of hydroxyl substitution of cellulose is 1.5; and so on, until all the three hydroxyl groups in the anhydrous glucose unit are replaced by the structure shown in formula (2), that is, the maximum degree of hydroxyl substitution of cellulose is 3.

[0150] In the present invention, by introducing the structure having an imide group represented by the above formula (2) into cellulose, the imidized cellulose derivative has excellent water resistance, and thus the imidized cellulose derivative can be applied to the field of water-resistant materials.

[0151] <Fourth Implementation Plan>

[0152] <Method for preparing imidized cellulose derivative>

[0153] Another object of the present invention is to provide a method for preparing the above-mentioned imidized cellulose derivative, which comprises: preparing a cellulose derivative by the preparation method of the above-mentioned second embodiment; and subjecting the obtained cellulose derivative to an imidization reaction.

[0154] Preferably, the temperature of the imidization reaction is 150 to 180°C, preferably 160 to 180°C.

[0155] Preferably, the imidization reaction time is 1 to 10 hours, preferably 2 to 8 hours, and more preferably 3 to 6 hours.

[0156] The imidization reaction is schematically shown by the following reaction formula (f):

[0157]

[0158] In reaction formula (f), * is the position of the ring bond to the anhydroglucose unit of cellulose, the oxygen atom connected to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose, and ▲ represents heating.

[0159] In the fourth embodiment, through the above imidization reaction, the structure having an imide group shown in the above formula (2) is formed, thereby imparting excellent water resistance to the cellulose derivative.

[0160] application

[0161] The cellulose derivative containing an amide group and a carboxyl group and / or its ammonium salt according to the first embodiment of the present application can be dissolved in a solvent (e.g., water), and a colorless and transparent water-soluble film can be prepared by evaporating the solvent (water). The water-soluble film can be further heated to obtain a water-insoluble colorless and transparent film material formed by the imidized cellulose derivative according to the third embodiment of the present invention.

[0162] Example

[0163] The present invention is further described by enumerating specific implementation cases below. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content recorded in the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the present invention equally.

[0164] Hereinafter, the testing methods involved in the following embodiments are first described.

[0165] Infrared spectrum test

[0166] The instrument model, sample preparation method and test conditions used for the test are as follows:

[0167] Instrument model: Bruker INVENIO S

[0168] Test mode: Transmission mode (TR)

[0169] Sample preparation method: KBr tablet preparation

[0170] Cellulose hydroxyl substitution degree

[0171] The sample used is the product of the reaction between the anhydride group-modified cellulose obtained in each example and excess ethanol. The H NMR spectrum of the product is measured, and the hydroxyl substitution degree of the cellulose of the sample is calculated based on the integrated area of ​​the H NMR spectrum.

[0172] Specifically, the integral area of ​​the characteristic peak of introduced benzene ring hydrogen (three hydrogens on the benzene ring) appearing at 7.5-8.5ppm in the nuclear magnetic resonance hydrogen spectrum (hereinafter referred to as the integral area of ​​the benzene ring region), the integral area between 3.6-5.5ppm (including 5 hydrogens on the cellulose backbone and 2 hydrogens on the ethanol-esterified methylene) (hereinafter referred to as the integral area of ​​the cellulose backbone region), and the integral area of ​​the broad peak at 1.3ppm (three hydrogens on the ethanol-esterified methyl) (hereinafter referred to as the integral area of ​​the ethanol region) were calculated, and the degree of substitution of cellulose hydroxyl groups was calculated according to the following formula:

[0173] Cellulose hydroxyl substitution degree = {integral area of ​​benzene ring region / [integral area of ​​cellulose skeleton region - (integral area of ​​ethanol region × 2 / 3)]} × 5 / 3

[0174] The degree of substitution of cellulose hydroxy groups obtained by the above formula corresponds to the degree of substitution of hydroxy groups of the water-soluble cellulose derivative after the aminolysis reaction, and also corresponds to the degree of substitution of hydroxy groups of the cellulose derivative after imidization.

[0175] Since the hydrogen peaks on the cellulose backbone overlap with the water peaks, the H NMR spectrum was measured in deuterated DMSO.

[0176] Conversion rate of trimellitic anhydride chloride

[0177] The conversion rate of trimellitic anhydride chloride was calculated according to the following formula:

[0178] Conversion rate of trimellitic anhydride chloride = cellulose hydroxyl substitution degree / (molar feed ratio of trimellitic anhydride chloride to anhydrous glucose unit of cellulose)

[0179] For example, when the degree of substitution of cellulose hydroxyl groups is 0.7, and the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose is 0.8:1, the conversion rate of trimellitic anhydride chloride is 0.7 / 0.8.

[0180] The molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose can be obtained by converting the mass feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose as follows:

[0181] Molar feed ratio = mass feed ratio × 162 / 210

[0182] Here, 210 is the molecular weight of trimellitic anhydride chloride, and 162 is the molecular weight of the cellulose repeating unit.

[0183] Amination rate

[0184] The amination rate was calculated according to the following formula:

[0185] Amination rate = (A / B) × 100%

[0186] Wherein, A is the molar amount of the anhydride group that reacts with two NH3 molecules to form ammonium amide salt when the anhydride group-modified cellulose is subjected to an aminolysis reaction with ammonia in each of the examples, wherein each anhydride group consumes 1 to 2 NH3 molecules, assuming that all NH3 molecules in the ammonia gas introduced during the aminolysis reaction or all NH3 molecules in the ammonia water added react with the anhydride group; and B is the molar amount of the anhydride group in the anhydride group-modified cellulose obtained in each of the examples, obtained based on the degree of substitution of cellulose hydroxyl groups.

[0187] The trimellitic anhydride chloride used in the following examples is produced by Anaiji Chemical and is numbered C010050.

[0188] Example 1

[0189] Take 1g of fully dried cellulose (Mn = 50000g·mol -1 , produced by Adamas-beta, number: P1956782), 45g N,N-dimethylacetamide, 4g lithium chloride are placed in a 100mL single-mouth flask and fully dissolved into a cellulose solution. At 40°C, 1.3g trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose is 1:1) is added and stirred for 4h. After the reaction is completed, the reaction solution is cooled to room temperature, and part of the product is taken out as sample a for measuring the degree of substitution of cellulose hydroxyl groups. Then, high-purity ammonia is introduced for 10 minutes, and the total amount of high-purity ammonia introduced is 0.2058g, and a white precipitate is precipitated. The precipitate is washed 3 times with a 60% acetone aqueous solution and then dried to obtain a water-soluble cellulose derivative. The solubility of the water-soluble cellulose derivative in water (25° C.) was measured to be 11.4 g / 100 g water, the degree of substitution of cellulose hydroxyl groups was 1.0, the conversion rate of trimellitic anhydride chloride was 99%, and the amination rate was 96%.

[0190] The water-soluble cellulose derivative prepared in this example was heated at 180° C. for 4 hours to obtain a water-insoluble imidized cellulose derivative.

[0191] Figure 2 The infrared spectrum of the water-soluble cellulose derivative prepared in this example is shown. Figure 2 As shown, at 1570cm -1 The characteristic peak of carboxylate carbonyl appeared at 1720 cm -1 The absorption peak of the ester carbonyl group appeared, thereby confirming that the water-soluble cellulose derivative of the present invention was obtained in Example 1.

[0192] Figure 3 The H NMR spectrum of the product of the reaction of the sample a taken out above with excess ethanol is shown. The integral area of ​​the characteristic peak of introduced benzene ring hydrogen appearing at 7.5-8.5 ppm in the H NMR spectrum is calculated and regarded as 1, and the integral area of ​​the cellulose skeleton region between 3.6-5.5 ppm is calculated to be 2.33, and the integral area of ​​the ethanol region at 1.3 ppm is calculated to be 1, thereby obtaining the degree of substitution of cellulose hydroxyl groups = {integral area of ​​benzene ring region / [integral area of ​​cellulose skeleton region-(integral area of ​​ethanol region×2 / 3)]}×5 / 3={1 / [2.33-(1×2 / 3)]}×5 / 3=1.0.

[0193] Example 2

[0194] 5 g of fully dried microcrystalline cellulose (Mn = 35000 g·mol -1 , produced by Anaiji Chemical, No.: E081567) was dissolved in a mixed solution of 100g N,N-dimethylacetamide / 7g lithium chloride, and 20g of trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose is 3.09:1) was added at 60°C, and 0.5g of triethylamine was added, and the reaction was stirred for 1h. After the reaction was completed, high-purity ammonia was introduced for 15 minutes, and the total amount of high-purity ammonia introduced was 2.4267g, and a white precipitate was precipitated. The precipitate was washed 3 times with 70% ethanol solution and then dried to obtain a water-soluble cellulose derivative. A photo of the water-soluble cellulose derivative is shown in Figure 5 shown.

[0195] The infrared spectrum confirmed that the water-soluble cellulose derivative of the present invention was obtained in Example 2. The solubility of the water-soluble cellulose derivative in water (25°C) was measured to be 30.4 g / 100 g water, the degree of substitution of cellulose hydroxyl was 2.5, the conversion rate of trimellitic anhydride chloride was 81.2%, and the amination rate was 85%.

[0196] The water-soluble cellulose derivative prepared in this example was heated at 180°C for 4 hours to obtain a water-insoluble imidized cellulose derivative. Figure 6 shown.

[0197] Example 3

[0198] 1g of refined cotton pulp (Mn = 450000g·mol -1 ) was fully dissolved in 100g of 1-butyl-3-methylimidazolium chloride. At 30°C, 2.6g of trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose was 2:1) was added, and 0.8g of pyridine was added, and the reaction was stirred for 6h. After the reaction was completed, high-purity ammonia was introduced for 10 minutes, and the total amount of high-purity ammonia introduced was 0.3156g, and a white precipitate was precipitated. The precipitate was washed 3 times with 70% methanol solution and then dried to obtain a water-soluble cellulose derivative.

[0199] The infrared spectrum confirmed that the water-soluble cellulose derivative of the present invention was obtained in Example 3. The solubility of the water-soluble cellulose derivative in water (25°C) was 18.6 g / 100 g water, the degree of substitution of cellulose hydroxyl was 1.6, the conversion rate of trimellitic anhydride chloride was 80%, and the amination rate was 88%.

[0200] The water-soluble cellulose derivative prepared in this example was heated at 160° C. for 6 hours to obtain a water-insoluble imidized cellulose derivative.

[0201] Example 4

[0202] 1g of silver star paste (Mn = 160000g·mol -1 ) was fully dissolved in 50g of 1-allyl-3-methylimidazolium chloride. At 40°C, 2.6g of trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose was 2:1) and 0.5g of 4-dimethylaminopyridine were added and stirred for 2 hours. After the reaction was completed, high-purity ammonia was introduced for 10 minutes, and the total amount of high-purity ammonia introduced was 0.3247g, and a white precipitate was precipitated. The precipitate was washed 3 times with 60% isopropanol solution and then dried to obtain a water-soluble cellulose derivative.

[0203] The infrared spectrum confirmed that the water-soluble cellulose derivative of the present invention was obtained in Example 4. The solubility of the water-soluble cellulose derivative in water (25°C) was measured to be 19.3 g / 100 g water, the degree of substitution of cellulose hydroxyl was 1.7, the conversion rate of trimellitic anhydride chloride was 85%, and the amination rate was 82%.

[0204] The water-soluble cellulose derivative prepared in this example was heated at 170° C. for 5 hours to obtain a water-insoluble imidized cellulose derivative.

[0205] Example 5

[0206] The cotton linters were pre-treated by washing with 100 ml of 5% sodium hydroxide solution, and then fully dried after removing impurities. 5 g of the dried product was fully dissolved in 200 g of 1-ethyl-3-methylimidazole acetate. At 60 ° C, 10 g of trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose was 1.54:1) was added and stirred for 4 hours. After the reaction was completed, 4.46 g of 25 wt% ammonia water was added to precipitate a white precipitate. The precipitate was washed 3 times with 50% ethanol solution and vacuum dried to obtain a powdered water-soluble cellulose derivative.

[0207] The infrared spectrum confirmed that the water-soluble cellulose derivative of the present invention was obtained in Example 5. The solubility of the water-soluble cellulose derivative in water (25°C) was measured to be 13.4 g / 100 g water, the degree of substitution of cellulose hydroxyl was 1.16, the conversion rate of trimellitic anhydride chloride was 75.4%, and the amination rate was 83.3%.

[0208] The water-soluble cellulose derivative prepared in this example was heated at 160° C. for 10 h to obtain a water-insoluble imidized cellulose derivative.

[0209] Example 6

[0210] 5g of bagasse was treated with 100ml of 5% sulfuric acid at room temperature for 2 days to obtain insoluble bagasse cellulose. After being fully washed and dried, 2g of bagasse cellulose was fully dissolved in 50g of a mixed solution consisting of 1-butyl-3-methylimidazolium acetate and 1,3-dimethyl-2-imidazolidinone in a mass ratio of 1:2. At 40°C, 10g of trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose is 3.85:1) and 1g of triethylamine were added and stirred for 6h. After the reaction was completed, high-purity ammonia was introduced for 30 minutes, and the total amount of high-purity ammonia introduced was 0.96g, and a white precipitate was precipitated. The precipitate was washed 3 times with 60% methyl isobutyl ketone solution and then dried to obtain a powdered water-soluble cellulose derivative.

[0211] According to the infrared spectrum, it was confirmed that the water-soluble cellulose derivative of the present invention was obtained in Example 6. The solubility of the water-soluble cellulose derivative in water (25°C) was measured to be 32.8 g / 100 g water, the degree of substitution of cellulose hydroxyl was 2.6, the conversion rate of trimellitic anhydride chloride was 67.6%, and the amination rate was 76%. The prepared cellulose derivative has good solubility in water.

[0212] The water-soluble cellulose derivative prepared in this example was heated at 180° C. for 3 hours to obtain a water-insoluble imidized cellulose derivative.

[0213] Example 7

[0214] 5g of waste cotton cloth was fully washed with water, washed with 10% sodium hydroxide solution, and dried for use. 1g of the treated cotton cloth was fully dissolved in 50ml of N,N-dimethylacetamide solution containing 8% lithium chloride. At 20°C, 2.6g of trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose is 2:1) and 0.5g of pyridine were added and stirred for 10h. After the reaction was completed, high-purity ammonia was introduced for 5 minutes, and the total amount of high-purity ammonia introduced was 0.2527g, and a white precipitate was precipitated. The precipitate was washed 3 times with 60% isopropanol solution and then dried to obtain a powdery water-soluble cellulose derivative.

[0215] The infrared spectrum confirmed that the water-soluble cellulose derivative of the present invention was obtained in Example 7. The solubility of the water-soluble cellulose derivative in water (25°C) was 16.6 g / 100 g water, the degree of substitution of cellulose hydroxyl was 1.4, the conversion rate of trimellitic anhydride chloride was 70%, and the amination rate was 72%.

[0216] The water-soluble cellulose derivative prepared in this example was reacted at 180° C. for 6 hours to obtain a water-insoluble imidized cellulose derivative as a light yellow powdery solid product.

[0217] Example 8

[0218] 5g of wheat straw was treated with 100ml of 5% dilute hydrochloric acid at room temperature for 2 days to obtain insoluble wheat straw cellulose. After being fully washed and dried, 2g of wheat straw cellulose was fully dissolved in a 50g mixed solution consisting of 1-butyl-3-methylimidazolium chloride and dimethyl sulfoxide (DMSO) in a mass ratio of 1:2. At 50°C, 6g of trimellitic anhydride chloride (the molar feed ratio of trimellitic anhydride chloride to the anhydrous glucose unit of cellulose is 2.3:1) and 0.8g of 4-dimethylaminopyridine were added and stirred for 5h. After the reaction was completed, 2.63g of 25wt% ammonia water was added and reacted for 10 minutes to precipitate a white precipitate. The precipitate was washed 3 times with 60% acetone solution and then dried to obtain a powdered water-soluble cellulose derivative.

[0219] According to the infrared spectrum, it was confirmed that the water-soluble cellulose derivative of the present invention was obtained in Example 8. The solubility of the water-soluble cellulose derivative in water (25°C) was measured to be 22.1 g / 100 g water, the degree of substitution of cellulose hydroxyl was 1.86, the conversion rate of trimellitic anhydride chloride was 80.6%, and the amination rate was 68%. The prepared cellulose derivative has good solubility in water.

[0220] The water-soluble cellulose derivative prepared in this example was heated at 160° C. for 8 hours to obtain a water-insoluble imidized cellulose derivative.

[0221] Water solubility evaluation :

[0222] 1 g of the water-soluble cellulose derivative prepared in Example 1 was dissolved in 30 g of water, and the solvent (water) was evaporated to obtain a water-soluble colorless transparent film, which was further heated at 180°C for 4 h to obtain a water-insoluble colorless transparent film. A photo of the colorless transparent film is shown in FIG. Figure 4 shown.

[0223] In contrast, 1g of cellulose (Mn = 50000g·mol -1 , produced by Adamas-beta, number: P1956782) was insoluble in 30g of water, and only cellulose powder was obtained after evaporation of the water. 1g of sodium carboxymethylcellulose was dissolved in 30g of water, and a transparent film was prepared after evaporation of the water, and the film was quickly dissolved in water. 1g of hydroxypropyl methylcellulose was dissolved in 30g of water, and a transparent film was prepared after evaporation of the water, and the film was quickly dissolved in water.

[0224] The above water solubility evaluation test shows that the cellulose derivative of the present invention has excellent water solubility, and its water solubility is at the same level as that of sodium carboxymethylcellulose and hydroxypropyl methylcellulose.

[0225] Industrial Applicability

[0226] The cellulose derivatives containing amide groups and carboxyl groups and / or their ammonium salts of the present invention can be applied to the fields of spinning, film manufacturing, etc., and the preparation method of the cellulose derivatives containing amide groups and carboxyl groups and / or their ammonium salts of the present invention can be widely used in the production of water-soluble cellulose derivatives in industry.

Claims

1. A cellulose derivative, It is characterized in that Contains the structure shown in the following formula (1): In the formula (1), X 1 and X 2 Any one of them is -NH 2 , X 1 and X 2 The other is -OH or -O - NH 4 + ; * is the position of the ring bond to the anhydroglucose unit of cellulose, and the oxygen atom connected to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose.

2. The cellulose derivative according to claim 1, It is characterized in that The degree of substitution of cellulose hydroxyl groups in the cellulose derivative is 0.1 or more, preferably 0.3 or more, more preferably 0.5 or more, and still more preferably 0.8 or more.

3. A method for preparing a cellulose derivative according to claim 1 or 2, It is characterized in that The following steps are involved: a) dissolving cellulose in a solvent to obtain a cellulose solution; b) mixing the cellulose solution with trimellitic anhydride chloride, and optionally with a catalyst, to react the trimellitic anhydride chloride with the cellulose to obtain anhydride group-modified cellulose; c) contacting the anhydride group-modified cellulose with ammonia and performing an aminolysis reaction to obtain the cellulose derivative, and the cellulose derivative is precipitated to the bottom of the reaction system in a solid state; d) optionally, separating the cellulose derivative from the reaction system of step c); e) optionally, washing the cellulose derivative separated in step d) with a solvent.

4. The preparation method according to claim 3, It is characterized in that The solvent in step a) comprises an ionic liquid, and the ionic liquid is 1-butyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium acetate, 1-butyl-3-methylimidazolium chloride, 1-allyl-3-methylimidazolium chloride, or N,N-dimethylacetamide / lithium chloride (DMAc / LiCl), preferably N,N-dimethylacetamide / lithium chloride (DMAc / LiCl); wherein when the ionic liquid is 1-butyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium acetate, 1-butyl-3-methylimidazolium chloride, or 1-allyl-3-methylimidazolium chloride, the solvent optionally comprises a cosolvent, and the cosolvent is at least one selected from dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), 1,3-dimethyl-2-imidazolidinone (DMI) and N,N-dimethylacetamide (DMAc).

5. The preparation method according to claim 3 or 4, It is characterized in that In the step b), the molar feed ratio of the trimellitic anhydride chloride to the anhydrous glucose unit of the cellulose is (0.5-6):1, preferably (0.5-5):1, more preferably (0.6-4):1, and even more preferably (1-3.9):1; the reaction temperature in the step b) is 18-100°C, preferably 20-80°C, more preferably 25-70°C; the reaction time in the step b) is 0.5-12 hours, preferably 1-10 hours.

6. The preparation method according to any one of claims 3 to 5, It is characterized in that The catalyst is at least one selected from pyridine and its derivatives and amines; preferably at least one selected from pyridine, 4-dimethylaminopyridine, ethylenediamine, and triethylamine; the amount of the catalyst used is 1% to 40% relative to the mass of trimellitic anhydride chloride, preferably 2% to 35%, and more preferably 2.5 to 31%.

7. The preparation method according to any one of claims 3 to 6, It is characterized in that In the step c), the duration of the aminolysis reaction is 1 to 40 minutes, preferably 1 to 30 minutes, more preferably 5 to 30 minutes; the amination rate after the aminolysis reaction is above 90%, preferably above 95%.

8. The preparation method according to any one of claims 3 to 7, It is characterized in that In the step a), the cellulose is at least one selected from microcrystalline cellulose, nanocellulose, α-cellulose, cotton cellulose, wood cellulose, and bacterial cellulose.

9. The preparation method according to any one of claims 3 to 8, It is characterized in that In the step e), the solvent used for the washing is at least one selected from ketone solvents, alcohol solvents, and water, preferably at least one selected from acetone, butanone, methyl isobutyl ketone, methanol, ethanol, isopropanol, and water.

10. An imidized cellulose derivative, It is characterized in that Contains the structure shown in the following formula (2): In the formula (2), * is the position of bonding to the ring of the anhydroglucose unit of cellulose, and the oxygen atom bonded to * is derived from the hydroxyl group in the anhydroglucose unit of cellulose.

11. The imidized cellulose derivative according to claim 10, It is characterized in that The degree of substitution of cellulose hydroxyl groups in the cellulose derivative is 0.1 or more, preferably 0.3 or more, more preferably 0.5 or more, and still more preferably 0.8 or more.

12. A method for preparing the imidized cellulose derivative according to claim 10 or 11, It is characterized in that The following steps are involved: The cellulose derivative is prepared by the preparation method according to any one of claims 3 to 9, and subjecting the cellulose derivative to an imidization reaction; Preferably, the temperature of the imidization reaction is 150 to 180° C., preferably 160 to 180° C.; the time of the imidization reaction is 1 to 10 hours, preferably 2 to 8 hours, more preferably 3 to 6 hours.

Citation Information

Cited By

  • Carboxymethyl cellulose-based imidazole zwitterionic polymer as well as preparation method and application thereof

    CN119306852A

  • A carboxymethyl cellulose-based imidazole zwitterionic polymer and its preparation method and application

    CN119306852B

  • High-transparency high-temperature-resistant cellulose-based polyimide film and preparation method thereof

    CN122444995A