Hydrophobic flocculant as well as preparation method and application thereof

By embedding adsorption and hydrophobic structural units in the flocculant, combined with low-pressure UV-initiated copolymer technology, a hydrophobic flocculant suitable for mineral processing wastewater treatment is prepared, which solves the problem of inability to effectively treat fine or micro-nano particles in the existing technology. , achieving the effects of efficient turbidity removal and low chemical residue.

CN118772332AActive Publication Date: 2024-10-15ANHUI UNIV OF SCI & TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410971128.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-15
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing flocculants cannot effectively adsorb fine or micro-nano particles when treating mineral processing wastewater, resulting in high turbidity of circulating water and large amounts of chemical residues, affecting the quality of concentrate products and the ecological environment.

Method used

A hydrophobic flocculant composed of adsorption structural units and hydrophobic structural units embedded in the polyacrylamide molecular chain is prepared through low-pressure UV-initiated copolymer polymerization. The selection of hydrophobic monomers is optimized through molecular dynamics simulation to enhance the adsorption capacity and adsorption capacity of the flocculant. Associative properties.

Benefits of technology

It achieves efficient adsorption and sedimentation of fine or micro-nano particles, reduces pharmaceutical residues, improves turbidity removal efficiency and sedimentation speed, and reduces pollution of water resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772332A_ABST
    Figure CN118772332A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of hydrophobic association functional high-molecular compounds, and particularly relates to a hydrophobic flocculant as well as a preparation method and application thereof. The structure of the hydrophobic flocculant disclosed by the invention comprises an adsorption structure unit and a hydrophobic structure unit, and the two structure units are embedded in a polyacrylamide molecular chain. Based on the adsorption capacity of an adsorption structure unit and fine particles, methacrylamido propyl trimethyl ammonium chloride is selected as a cationic monomer; a molecular dynamics simulation method is adopted to comprehensively analyze the hydrophobic performance and association characteristics of a hydrophobic structure unit, and perfluorohexyl ethyl methacrylate is used as a hydrophobic monomer. The flocculating agent is novel in structure, excellent in turbidity removal effect and small in agent residual quantity, and has high application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrophobic associating functional polymer compounds, and in particular relates to a hydrophobic flocculant and a preparation method and application thereof. Background Art

[0002] As environmental pollution becomes increasingly serious, the control and treatment of water pollution has gradually attracted people's attention and made progress in various aspects. There are many ways to treat water, including ultrasonic treatment, electrodialysis, membrane filtration and centrifugal separation. Among them, the flocculation sedimentation process is simple to operate and low in cost. It is a mature wastewater treatment process with good treatment effect and is widely used by water treatment companies at home and abroad.

[0003] Commercial flocculants on the market mainly include cationic, anionic, nonionic and amphoteric flocculants. Considering the large content of fine particles in wastewater and the negative charge on the surface, the electrostatic repulsion between particles makes wastewater difficult to treat. Cationic flocculants can neutralize negatively charged particles and accelerate the coagulation of particles and flocculant molecules to form flocs through bridging. Therefore, the effect of cationic flocculants with high ionicity is more worth looking forward to, but the synthesis process of flocculants with high cationicity is more complicated.

[0004] In addition, for the treatment of mineral processing wastewater, especially for the wet mineral processing and metallurgical industries, due to the decline in mineral grade and the improvement of sorting technology, the particle size in the mineral processing wastewater continues to decrease, and the hydration effect on the particle surface gradually becomes significant. In addition to the electrostatic repulsion, the hydration repulsion between particles becomes stronger, resulting in the stable suspension of fine or micro-nano-scale particles in the mineral processing wastewater. Faced with mineral processing wastewater with high solid suspended matter content and good stability, the commercial flocculants currently on the market do not take into account the hydration characteristics of the particles, and even enhance the combination of the surface and water molecules, resulting in the inability of the flocculants to stably adsorb fine or micro-nano particles, high turbidity of the circulating water and large amount of residual reagents, which in turn leads to a series of problems such as deterioration of circulating water quality, pollution of concentrate products, low utilization rate of tailings and difficulty in storage, and even causes water pollution, soil damage and dust pollution to the ecological environment.

[0005] Therefore, it has become an urgent need in the market to provide a new flocculant suitable for mineral processing wastewater treatment, with excellent turbidity removal effect and low reagent residue. Summary of the invention

[0006] In view of this, the first object of the present invention is to provide a hydrophobic flocculant suitable for mineral processing wastewater treatment, with excellent turbidity removal effect and low reagent residue, in order to solve the problems existing in the prior art.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A hydrophobic flocculant comprises an adsorption structural unit and a hydrophobic structural unit embedded in a polyacrylamide molecular chain, wherein the cationic monomer constituting the adsorption structural unit is methacrylamidopropyltrimethylammonium chloride, and the hydrophobic monomer constituting the hydrophobic structural unit is perfluorohexylethyl methacrylate.

[0009] It is worth noting that the adsorption structural unit in the hydrophobic flocculant has a positively charged group. In addition to electrically neutralizing the negatively charged particles in the wastewater, it also has excellent adsorption capacity, can capture fine or micro-nano particles and cause the particles to aggregate into large flocs, thereby achieving separation of particles from the suspension. The introduction of the hydrophobic structural unit can weaken or break the hydration film on the surface of the particles, promote the stable adsorption of the adsorption structural unit on the surface of the particles, and in addition, the hydrophobic structural unit helps the molecular chain of the hydrophobic flocculant to associate and stretch, in addition to enhancing the bridging performance of the polymer, it can also reduce the residual agent of the flocculant and improve the flocculation treatment effect and the floc dehydration effect.

[0010] The present invention uses perfluorohexylethyl methacrylate as a hydrophobic monomer to construct a hydrophobic structural unit. On the one hand, the fluorocarbon side chain on the hydrophobic structural unit has the strongest hydrophobic association performance based on the molecular dynamics simulation method, which can promote the adsorption of the adsorption structure unit on the surface of fine or micro-nano particles, enhance the bridging mechanism to form larger flocs, and improve the turbidity removal efficiency and sedimentation rate. On the other hand, the fluorocarbon side chain length is less than 6, which is easier to degrade and reduces the pollution to water resources.

[0011] Furthermore, the cationicity of the copolymer is 10-50%, and the hydrophobicity is 2.5-17.5%.

[0012] The hydrophobic flocculant disclosed in the present invention has a stronger adsorption capacity of the adsorption structural units on the surface of fine or micro-nano particles, which enhances the turbidity removal efficiency of the flocculant and reduces the possibility of floc breakage and recombination; the hydrophobic structural units on the flocculant have excellent hydrophobic and associative properties, can break or weaken the hydration effect on the surface of particles and enhance the bridging mechanism, reduce the residual agent in wastewater treatment, and promote filter press dehydration.

[0013] The second object of the present invention is to provide a method for preparing the hydrophobic flocculant as described above.

[0014] A method for preparing a hydrophobic flocculant comprises the following steps: using acrylamide as a main monomer, methacrylamidopropyltrimethylammonium chloride as a cationic monomer, and perfluorohexylethyl methacrylate as a hydrophobic monomer, and initiating copolymer polymerization by low-pressure ultraviolet light.

[0015] It is worth noting that the short wave in the low-pressure ultraviolet (UV) copolymerization reaction adopted in the present invention can provide efficient radiation energy for initiation, resulting in a large number of reaction areas centered on initiating free radicals, thereby increasing the copolymerization reaction rate and forming a porous structure, which is beneficial to reducing the dissolution time of the hydrophobic flocculant and improving the use efficiency of the flocculant in industrial production.

[0016] Furthermore, the preparation method specifically comprises the following steps:

[0017] S1. Mix a certain amount of hydrophobic monomer, surfactant and deionized water, adjust the pH of the reaction system to 2.5-5.5, and obtain a transparent solution after sufficient dispersion, which is liquid A;

[0018] S2, adding a certain amount of acrylamide monomer, cationic monomer and solubilizer to liquid A, introducing nitrogen protection throughout the process, and fully mixing at room temperature to obtain liquid B;

[0019] S3, adding a certain amount of photoinitiator to liquid B, after fully mixing, transferring the mixed liquid to a light irradiation reaction device;

[0020] S4, irradiating with a low-pressure ultraviolet lamp for a certain period of time, and curing at room temperature for 2 to 4 hours to obtain a gelatinous substance C;

[0021] S5, transferring the colloid C into a mixture of ethanol and acetone, and chopping it into pieces, so as to fully wash it to obtain a solid D;

[0022] S6. Dry the solid D for 24 hours and grind it to obtain a finished flocculant.

[0023] Furthermore, the surfactant in step S1 is hexadecyltrimethylammonium bromide, the solubilizer in step S2 is urea, and the photoinitiator in step S3 is one of azobisisobutylamidine hydrochloride, azobisisopropylimidazoline hydrochloride, azobiscyanovaleric acid, azobisimidazoline propane, and irgacure 2959.

[0024] In some embodiments, the photoinitiator is irgacure 2959.

[0025] Furthermore, in step S2, the total monomer mass of the hydrophobic monomer, acrylamide monomer and cationic monomer accounts for 15-45% of the mass of liquid B, the molar mass of the cationic monomer accounts for 10-50% of the total monomers, and the molar mass ratio of the acrylamide monomer to the hydrophobic monomer is (7.75-6.25):(0.25-1.75).

[0026] Furthermore, the amount of surfactant used in step S1 is 1.3-5.3% of the total monomer mass fraction, the amount of solubilizer used in step S2 is 0.1-0.7% of the total monomer mass fraction, and the amount of photoinitiator used in step S3 is 0.01-0.07% of the total monomer mass fraction.

[0027] Furthermore, the low-pressure ultraviolet lamp in step S4 is 24W or 48W, the radiation wavelength is 253.7nm, and the light radiation reaction time is 2-8h.

[0028] The third object of the present invention is to provide a use of the hydrophobic flocculant as described above in wastewater treatment.

[0029] It is worth noting that the hydrophobic flocculant disclosed in the present invention is mainly used in the treatment of mineral processing wastewater with a large number of fine or micro-nano particles. The surface of particles in mineral processing wastewater usually has a strong negative charge. The smaller the particle size, the stronger the surface hydration. The electrostatic repulsion and hydration repulsion between particles are the essential reasons for the stable suspension of particles. Therefore, the hydrophobic flocculation disclosed in the present invention has adsorption and hydrophobic structural units, which can weaken or break the electrostatic repulsion and hydration repulsion between particles, improve turbidity removal efficiency, sedimentation rate and dehydration effect, etc., and achieve efficient treatment of mineral processing wastewater.

[0030] Compared with the prior art, the hydrophobic flocculant disclosed in the present invention uses a hydrophobic polyacrylamide polymerized from a cationic monomer and a hydrophobic monomer and acrylamide, and has a low system viscosity and a good flocculation effect. The obtained hydrophobic flocculant has an excellent turbidity removal effect in wastewater treatment and a small amount of residual agents, and has a strong application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without creative work.

[0032] Figure 1 is the reaction equation of the polymerization reaction disclosed in the present invention.

[0033] Figure 2 : is the radial water density distribution of the hydrophobic structural unit in Experimental Example 1 of the present invention.

[0034] Figure 3 The hydrophobic structural unit R in Experimental Example 1 of the present invention g The distribution probability of .

[0035] Figure 4The adsorption amount of polyacrylamide flocculant on kaolinite particles and the residual amount in aqueous solution in Comparative Example 1 of the present invention are: (a): N682; (b): A6056; (c): C6360; (d): turbidity of supernatant.

[0036] Figure 5 The adsorption amount (a) of the cationic flocculant (P(AM-MAPTAC)) on the kaolinite surface and the turbidity of the supernatant (b) in Comparative Example 1 of the present invention are shown.

[0037] Figure 6 The adsorption amount (a) of the hydrophobic flocculant (P(AM-MAPTAC-TEMAc6)) on the kaolinite surface and the turbidity of the supernatant (b) in Comparative Example 1 of the present invention are shown.

[0038] Figure 7 This is a scanning electron microscope image of the hydrophobic flocculant (P(AM-MAPTAC-TEMAc6)) obtained in Example 1 of the present invention.

[0039] Figure 8 The hydrophobic flocculant (P(AM-MAPTAC-TEMAc6)) obtained in Example 2 of the present invention 1 HNMR spectrum. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.

[0042] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.

[0043] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.

[0044] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.

[0045] The invention discloses a hydrophobic flocculant and a preparation method and application thereof. The hydrophobic flocculant disclosed in the invention comprises a cationic structural unit and a hydrophobic structural unit, wherein the cationic structural unit and the hydrophobic structural unit are embedded in a polyacrylamide carbon chain. A molecular dynamics simulation method is used to comprehensively analyze hydrophobic properties and associative properties, and methacrylamidopropyltrimethylammonium chloride is selected as a cationic monomer and perfluorohexylethyl methacrylate is selected as a hydrophobic monomer. The flocculant has a novel structure, excellent turbidity removal effect, and a small amount of residual agent, and has a strong application potential.

[0046] The specific steps of the preparation method disclosed in the present invention include:

[0047] S1. Mix a certain amount of hydrophobic monomer, surfactant and deionized water, adjust the pH of the reaction system to 2.5-5.5, and obtain a transparent solution after sufficient dispersion, which is liquid A;

[0048] S2, adding a certain amount of acrylamide monomer, cationic monomer and solubilizer to liquid A, introducing nitrogen protection throughout the process, and fully mixing at room temperature to obtain liquid B;

[0049] S3, adding a certain amount of photoinitiator to liquid B, after fully mixing, transferring the mixed liquid to a light irradiation reaction device;

[0050] S4, irradiating with a low-pressure ultraviolet lamp for a certain period of time, and curing at room temperature for 2 to 4 hours to obtain a gelatinous substance C;

[0051] S5, transferring the colloid C into a mixture of ethanol and acetone, and chopping it into pieces, so as to fully wash it to obtain a solid D;

[0052] S6. Dry the solid D for 24 hours and grind it to obtain a finished flocculant.

[0053] As an embodiment of the present invention, the pH value in step S1 includes 2.5, 3.0, 3.5, 4.0, 4.5, 5.0 and 5.5. Preferably, the pH value in step S1 is 4.0.

[0054] Furthermore, the surfactant in step S1 is hexadecyltrimethylammonium bromide, the solubilizer in step S2 is urea, and the photoinitiator in step S3 is one of azobisisobutylamidine hydrochloride, azobisisopropylimidazoline hydrochloride, azobiscyanovaleric acid, azobisimidazoline propane, and irgacure 2959.

[0055] As an embodiment of the present invention, the photoinitiator is irgacure 2959.

[0056] Furthermore, in step S2, the total monomer mass of the hydrophobic monomer, acrylamide monomer and cationic monomer accounts for 15-45% of the mass of liquid B, the molar mass of the cationic monomer accounts for 10-50% of the total monomers, and the molar mass ratio of the acrylamide monomer to the hydrophobic monomer is (7.75-6.25):(0.25-1.75).

[0057] As an embodiment of the present invention, the molar mass ratio of the acrylamide monomer, the cationic monomer, and the hydrophobic monomer is 7.75:2:0.25, 7.5:2:0.5, 7.25:2:0.75, 7:2:1, 6.75:2:1.25, 6.5:2:1.5, 6.25:2:1.75. Under preferred conditions, the molar mass ratio of the acrylamide monomer, the cationic monomer, and the hydrophobic monomer is 7.5:2:0.5, 7.25:2:0.75, and 7:2:1. Under more preferred conditions, the molar mass ratio of the acrylamide monomer, the cationic monomer, and the hydrophobic monomer is 7.25:2:0.75 and 7:2:1.

[0058] Furthermore, the amount of surfactant used in step S1 is 1.3-5.3% of the total monomer mass fraction, the amount of solubilizer used in step S2 is 0.1-0.7% of the total monomer mass fraction, and the amount of photoinitiator used in step S3 is 0.01-0.07% of the total monomer mass fraction.

[0059] Furthermore, the low-pressure ultraviolet lamp in step S4 is 24W or 48W, the radiation wavelength is 253.7nm, and the light radiation reaction time is 2-8h.

[0060] As an embodiment of the present invention, the light irradiation reaction time in step S4 is 2 hours, 4 hours, 6 hours, or 8 hours. Under preferred conditions, the light irradiation reaction time is 4 hours or 6 hours, and under more preferred conditions, the light irradiation reaction time is 4 hours.

[0061] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0062] Example 1

[0063] First, 0.645 mL of hydrophobic monomer (perfluorohexylethyl methacrylate), 0.1 g of surfactant CTAB (hexadecyltrimethylammonium bromide) and 5.905 mL of deionized water were added to a quartz synthesis bottle, and stirred with a magnetic stirrer at a speed of 500 r / min for 1 h to make the solution transparent, as solution A. At this time, dilute hydrochloric acid solution and sodium hydroxide solution were used to adjust the solution pH to 4.0. Then, 1.089 g of acrylamide monomer, 1.835 mL of cationic monomer (methacrylamidopropyltrimethylammonium chloride) and 0.009 g of solubilizer (urea) were added to liquid A, and nitrogen protection was introduced throughout the process. The reaction temperature was adjusted to 25° C. in a water bath, and the mixture was stirred at 500 r / min with a magnetic stirrer for 1 h to be fully mixed to obtain liquid B; 0.0009 g of photoinitiator was added to liquid B, and the mixture was stirred for 10 min. The quartz synthesis bottle containing the mixed liquid was placed in a UV ultraviolet photocatalyst for light reaction for 4 h. After the light irradiation was completed, the mixture was cured at room temperature for 4 h to obtain a colloid C.

[0064] After solidification, transfer the colloid C to a mixture of ethanol and acetone and cut it into pieces with scissors to wash it thoroughly. After washing, dry it in an electric blast drying oven at 60°C for 24 hours to obtain a solid product. Grind the solid to obtain a powder, which is the hydrophobic flocculant.

[0065] The hydrophobic flocculant P (AM-MAPTAC-TEMAc6) obtained in this example has polyacrylamide as the main chain, and the adsorption structural unit and the hydrophobic structural unit are embedded in the polyacrylamide molecular chain, wherein the total monomer mass accounts for 30% of the total solution mass, the molar mass fraction ratio of acrylamide monomer, cationic monomer and hydrophobic monomer is 7:2:1, and the hydrophobicity of the copolymerized hydrophobic flocculant is 10%, and the intrinsic viscosity is 540mL / g. The scanning electron microscope image of the obtained hydrophobic flocculant P (AM-MAPTAC-TEMAc6) is as follows: Figure 7 shown.

[0066] Example 2

[0067] First, 0.604 mL of hydrophobic monomer (perfluorohexylethyl methacrylate), 0.1 g of surfactant CTAB (hexadecyltrimethylammonium bromide) and 5.164 mL of deionized water were added to a quartz synthesis bottle, and stirred with a magnetic stirrer at a speed of 500 r / min for 1 h to make the solution transparent, as solution A. At this time, dilute hydrochloric acid solution and sodium hydroxide solution were used to adjust the solution pH to 4.0. Then, 1.408 g of acrylamide monomer, 2.291 mL of cationic monomer (methacrylamidopropyltrimethylammonium chloride) and 0.0105 g of solubilizer (urea) were added to liquid A, and nitrogen protection was introduced throughout the process. The reaction temperature was adjusted to 25°C in a water bath, and the mixture was stirred at 500 r / min with a magnetic stirrer for 1 h to be fully mixed to obtain liquid B; 0.0012 g of photoinitiator was added to liquid B, and the mixture was stirred for 10 min. The quartz synthesis bottle containing the mixed liquid was placed in a UV ultraviolet photocatalyst for light reaction for 4 h. After the light irradiation was completed, the mixture was cured at room temperature for 4 h to obtain a colloid C.

[0068] After solidification, transfer the colloid C to a mixture of ethanol and acetone and cut it into pieces with scissors to wash it thoroughly. After washing, dry it in an electric blast drying oven at 60°C for 24 hours to obtain a solid product. Grind the solid to obtain a powder, which is the hydrophobic flocculant.

[0069] The hydrophobic flocculant obtained in this example has polyacrylamide as the main chain, and the adsorption structural unit and the hydrophobic structural unit are embedded in the polyacrylamide molecular chain, wherein the total monomer mass accounts for 35% of the total solution mass, and the molar mass fraction ratio of acrylamide monomer, cationic monomer and hydrophobic monomer is 7.25:2:0.75. The hydrophobicity of the copolymerized hydrophobic flocculant is 7.5%, and the intrinsic viscosity is 727 mL / g. The obtained hydrophobic flocculant P(AM-MAPTAC-TEMAc6) 1 HNMR spectrum Figure 8 As shown, the generation of polymer can be seen.

[0070] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following comparative examples and embodiments are used to further illustrate the technical features and / or technical advantages of the hydrophobic flocculant and the preparation method thereof disclosed in the present invention, but they should not be construed as limiting the present invention. The parameters and process flow adjustments made by those skilled in the art according to the above invention content or the applications made according to the above properties are also deemed to fall within the protection scope of the present invention.

[0071] Experimental Example 1 Selection of hydrophobic structural units

[0072] The hydrophobic structural units are polymerized with butyl acrylate (BA), styrene (STY), lauric acrylate (LA), trifluoroethyl methacrylate (TFEMA) and perfluorohexylethyl methacrylate (TEMAc6) as monomers. Taking P-BA as an example, P- means the structural unit after polymerization. 1 Subscript 1 indicates a hydrophobic structural unit, P-BA 10 The subscript 10 indicates 10 hydrophobic structural units.

[0073] In order to study the hydrophobic properties of the hydrophobic structural unit, the present invention adopts the molecular dynamics simulation (MD) method to calculate the radial water density distribution of the hydrophobic side chain of the hydrophobic structural unit and analyze its influence on the surrounding water structure. The results are as follows: Figure 2 The radial radius is Within the range, the order of water density around the hydrophobic structural unit is P-BA 1 >P-STY 1 >P-LA 1 >P-TFEMA 1 >P-TEMAc6 1 , and the water density is not much different. It is known that P-BA 1 and P-LA 1 The side chains of P-TFEMA are hydrocarbon chains with carbon chain lengths of 4 and 12 respectively. 1 and P-TEMAc6 1 The branched chains are mainly carbon-fluorine chains; the carbon chain lengths are 2 and 8, respectively. 1 and P-TFEMA 1 The water density difference is greater than P-LA 1 and P-BA 1 The water density is poor, and P-TEMAc6 1 and P-TFEMA 1 The water density is less than that of P-LA 1 and P-BA 1 , which shows that the carbon-fluorine structure has a significant effect on the water density. After, P-STY 1 The ring structure makes it The water density before the P-LA is the smallest; 1 Density is lower than P-TFEMA 1 , the effect of carbon chain length on water density begins to be significant. Within the range, the carbon fluorine branch head and -CH 3 The distance is P-TEMAc6 1 and P-TFEMA 1 The main chain is higher than P-LA1 and P-BA 1 One more -CH 3 group, which indicates that -CH 3 Adsorption of water molecules leads to P-TEMAc6 1 and P-TFEMA 1 The water density increases, and the affected area is about Radius greater than After that, the order of water density around the hydrophobic structural unit is P-STY 1 >P-BA 1 ≈P-TFEMA 1 >P-LA 1 >P-TEMAc6 1 , it can be seen that P-LA 1 and P-TEMAc6 1 The surrounding water density is smaller than that of P-BA with a smaller carbon chain length. 1 and P-TFEMA 1 , which indicates that the longer the carbon chain, the greater the effect on water density. 1 and P-TFEMA 1 The water density difference is greater than P-LA 1 and P-BA 1 The water density is poor, and P-TEMAc6 1 The water density is significantly lower than that of P-LA 1 It is not difficult to judge that the more carbon-fluorine structures there are, the more significant the impact on the surrounding water. 1 exist is the distance to the hydrogen on the benzene ring, The radial range is composed of atoms on the benzene ring, so the water density is relatively small. In summary, the order of hydrophobicity is P-TEMAc6 1 >P-LA 1 >P-TFEMA 1 ≈P-BA 1 >P-STY 1 .

[0074] Furthermore, the radius of gyration (R g ) is the distance between the atoms in the molecular chain and the isocenter, which is an indicator of the mass weight radius in MD simulation and is defined as:

[0075]

[0076] Among them, R g The radius of gyration m i is the mass of atom i (g); r i is the distance between atom i and the isocenter According to Rg and distribution probability Calculate the root mean square radius (MSR). MSR can directly reflect the conformation and size parameters of the hydrophobic structural unit and is an important parameter used to analyze the degree of intermolecular association. It is defined as:

[0077]

[0078] Considering that when the hydrophobic structural unit exists in isolation in an aqueous solution, there is no interaction between molecules, and the conformational stretching or contraction eventually reaches a dynamic equilibrium. When the concentration of the hydrophobic structural unit increases, the presence of the hydrophobic side chains causes the molecules to associate and aggregate, and the hydrophobic region is relatively concentrated, causing the molecules to mainly contract. The stronger the association performance, the deeper the curling of the hydrophobic structural unit. Table 1 shows the MSR of the hydrophobic structural unit. It can be seen from Table 1 that the MSR of P-TFEMA with the shortest chain length and P-STY with a benzene ring structure are equal before and after the concentration change. Because P-TFEMA 1 and P-STY 1 The hydrophobicity of P-TFEMA is weak and the chain length is short. 10 and P-STY 10 The aggregation state is formed slowly and the association performance is weak. 1 P-TFEMA 1 The hydrophobic properties of P-BA are comparable. 10 The MSR of the 10 The associative properties are stronger than those of P-TFEMA 10 , which is mainly P-BA 1 The carbon chain of P-LA is longer. 10 and P-TEMAc6 10 Compared with P-LA 1 and P-TEMAc6 1 Curled separately and P-LA 10 and P-TEMAc6 10 This further suggests that the associative properties increase with increasing chain length or increasing hydrophobicity. Figure 3 R is the hydrophobic structural unit g of It can be seen that compared with the hydrophobic structural unit in isolation, the concentration of P-TFEMA increased 10 and P-STY 10 R g The distribution remains basically unchanged; P-BA 10 In R g for Distribution probability increased; P-TEMAc6 10 Mainly focused on Rg for Whereas P-LA 10 R g exist In summary, the strength of the association performance of the hydrophobic structural unit is P-TEMAc6 10 >P-LA 10 >P-BA 10 >P-TFEMA 10 ≈P-STY 10 Since the larger the molecule, the stronger the steric hindrance effect and the more difficult the copolymerization reaction is, combined with the hydrophobic performance analysis, P-TEMAc6 was used as the hydrophobic active hydrophobic structure of the new flocculant.

[0079] Table 1 MSR of hydrophobic structural units

[0080]

[0081] Comparative Example 1 Analysis of the adsorption performance and turbidity removal efficiency of commercially available polyacrylamide flocculants, monocationic flocculants and the flocculant of the present invention

[0082] N682, A6056 and C6360 are representative commercially available polyacrylamide flocculants (Table 2). Among them, C6360 is a cationic polyacrylamide, and the cationic monomer used to synthesize it is acryloyloxyethyltrimethylammonium chloride (DAC).

[0083] Table 2 Commercially available polyacrylamide structural formula

[0084]

[0085] Different active functional groups on flocculants lead to different adsorption properties on mineral particles, which manifests macroscopically as different adsorption amounts. Figure 4 (a) and (b) are the adsorption amounts of commercially available polyacrylamide flocculants on the surface of fine kaolinite particles. Figure 4It can be seen that N682 and A6056 have the same adsorption trend on kaolinite particles. When the dosage of N682 is less than 0.06 mg / g or A6056 is less than 0.03 mg / g, it is a rapid adsorption stage on kaolinite particles; when N682 is greater than 0.06 mg / g or A6056 is greater than 0.03 mg / g, the adsorption amount increases slowly. The dosage of N682 or A6056 is low, the surface of kaolinite particles has sufficient relative adsorption sites, and the adsorption amount increases rapidly. When the dosage increases, the adsorption sites are relatively insufficient, and N682 or A6056 will slow down the increase in adsorption through intermolecular interactions. Under the same dosage, the adsorption amount of N682 is higher than that of A6056, indicating that the adsorption performance of N682 on the kaolinite surface is stronger than that of A6056. In addition, although the adsorption amount increases with the increase in the dosage of N682 or A6056, more N682 or A6056 molecular chains remain, which has a significant effect on the adsorption effect. Before the dosage of C6360 was 0.36 mg / g, the adsorption amount basically increased linearly, and C6360 occupied more molecular chains on the same kaolinite adsorption site, which means that C6360 has the strongest adsorption capacity. When the dosage reached 0.48 mg / g, a large amount of C6360 diffused in the water, and the electrostatic repulsion between the residual molecular chains affected the molecules that had been adsorbed on the kaolinite surface, resulting in a decrease in the adsorption amount.

[0086] like Figure 4 As shown in (d), before the dosage of N682 is 0.06 mg / g, the turbidity of the supernatant drops rapidly; in the range of 0.06-0.12 mg / g, the rate of turbidity decreases slowly. The increase in dosage and the adsorption capacity of kaolinite particles increase, which can capture more fine particles in the suspension, so the turbidity decreases; when it is greater than 0.12 mg / g, the residual N682 hinders the flocculation and sedimentation of particles, and the turbidity begins to increase. Before the dosage of A6056 is 0.03 mg / g, the turbidity decreases relatively quickly; in the range of 0.03-0.12 mg / g, the rate of turbidity decreases slowly; also when it is greater than 0.12 mg / g, the turbidity begins to increase. It can be found that before 0.03 mg / g, the adsorption capacity of A6056 is weaker than that of N682, but the residual amount is greater than N682. The bridging effect between the residual flocculant and the particles is more conducive to capturing fine mineral particles, and the turbidity of A6056 is lower than that of N682. This phenomenon can also be observed when C6360 is used to treat kaolinite suspension. C6360 has the strongest adsorption capacity, and the turbidity is as high as 1256.67 NTU at a dosage of 0.015 mg / g. Its adsorption on kaolinite particles has little effect on the negative charge of the surface and it is difficult to form a bridging mechanism, resulting in high turbidity. In the range of 0.03 to 0.36 mg / g, the particles adsorbed with C6360 aggregate and settle, and the turbidity continues to decrease. When it reaches 0.48 mg / g, the residual molecular chains lead to a decrease in adsorption capacity and an increase in turbidity.

[0087] The monocationic flocculant P(AM-MAPTAC) was prepared by using methacrylamidopropyltrimethylammonium chloride as the cationic monomer, wherein P(AM-MAPTAC)-20 and P(AM-MAPTAC)-30 respectively represent cationic degrees of 20% and 30%.

[0088] Figure 5 (a) is the adsorption amount of P(AM-MAPTAC) on fine kaolinite particles. It can be seen that before the dosage of the agent is 0.36 mg / g, the adsorption amount basically shows a linear increase trend; after it is greater than 0.36 mg / g, the increase in the adsorption amount decreases compared to the addition amount, and the residual amount of P(AM-MAPTAC)-30 in the aqueous solution is greater than that of P(AM-MAPTAC)-20. This means that before 0.36 mg / g, the adsorption sites on the surface of kaolinite particles are sufficient to accommodate more P(AM-MAPTAC) molecules, and P(AM-MAPTAC) can continue to adsorb on the surface of kaolinite as the dosage increases, and its adsorption effect on kaolinite particles continues to increase. When the concentration is greater than 0.36 mg / g, P(AM-MAPTAC)-30 has reached saturated adsorption on the kaolinite surface, and even affects the molecules that have been adsorbed on the surface, resulting in a decrease in the adsorption amount; while the adsorption amount of P(AM-MAPTAC)-20 on kaolinite particles is still increasing, which is mainly caused by the electrostatic repulsion between molecules. The cationicity of P(AM-MAPTAC)-30 is greater than that of P(AM-MAPTAC)-20. The greater the electrostatic repulsion, the easier it is for P(AM-MAPTAC) to remain in the aqueous solution.

[0089] The above has shown that the order of adsorption capacity of three commercially available polyacrylamide flocculants on kaolinite particles is C6360>N682>A6056. It is not difficult to find that the adsorption amount of P(AM-MAPTAC) also decreases after it exceeds 0.36 mg / g, but the decrease is smaller than that of C6360, which indicates that the adsorption capacity of P(AM-MAPTAC)-30 on kaolinite particles is stronger than that of C6360.

[0090] Figure 5 (b) is the turbidity of the supernatant after the kaolinite suspension has settled. Figure 5 As shown, before the dosage of the agent is 0.12 mg / g, the turbidity of the supernatant of P(AM-MAPTAC)-30 is less than that of P(AM-MAPTAC)-20. This is mainly because the charge density of P(AM-MAPTAC)-30 is large, the double layer thickness of the kaolinite particles adsorbed with P(AM-MAPTAC)-30 is smaller than that of P(AM-MAPTAC)-20, and the electrostatic repulsion between the particles is small, which makes it easier for aggregation and sedimentation to occur. After 0.12 mg / g, the turbidity is less than 30NTU, and P(AM-MAPTAC) can remove fine kaolinite particles very well.

[0091] Take the hydrophobic flocculant prepared in Example 1-2 as P(AM-MAPTAC-TEMAc6), Figure 6 (a) and (b) are the adsorption amount of P(AM-MAPTAC-TEMAc6) on kaolinite particles and the turbidity of the supernatant after sedimentation, respectively, where P(AM-MAPTAC-TEMAc6)-7.5 and P(AM-MAPTAC-TEMAc6)-10 represent hydrophobic flocculants with hydrophobicity of 7.5% and 10%, respectively.

[0092] It can be seen that with the increase of the amount of P(AM-MAPTAC-TEMAc6), the adsorption amount basically shows a linear increase trend, which means that the adsorption capacity of P(AM-MAPTAC-TEMAc6) on the kaolinite surface is continuously enhanced. This shows that when the amount of P(AM-MAPTAC) is greater than 0.36 mg / g, the adsorption amount decreases due to the electrostatic repulsion between the molecular chains. After the introduction of the hydrophobic monomer, the adsorption amount of P(AM-MAPTAC-TEMAc6) did not decrease significantly. The carbon fluorine chain causes the molecular chain to associate, forming a network structure that is easier to capture solid particles in the colloidal suspension and produces a lower supernatant turbidity. When the dosage is less than 0.03 mg / g, the charge density of P(AM-MAPTAC)-20 is low, and aggregation and sedimentation are difficult; P(AM-MAPTAC-TEMAc6)-7.5 and P(AM-MAPTAC-TEMAc6)-10 are adsorbed on kaolinite particles, and the hydrophobic structural units on them can enhance the bridging mechanism of the hydrophobic flocculant through association, significantly reducing the turbidity of the supernatant, showing excellent turbidity removal efficiency. When the dosage is greater than 0.03 mg / g, the turbidity produced by P(AM-MAPTAC-TEMAc6) is less than that of commercially available polyacrylamide flocculants and P(AM-MAPTAC), further indicating that it has the highest turbidity removal efficiency, and both P-MAPTAC and P-TEMAc6 structures are conducive to the sedimentation of suspended particles.

[0093] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A hydrophobic flocculant, comprising an adsorption structural unit and a hydrophobic structural unit embedded in a polyacrylamide molecular chain, characterized in that: The cationic monomer constituting the adsorption structural unit is methacrylamidopropyltrimethylammonium chloride, and the hydrophobic monomer constituting the hydrophobic structural unit is perfluorohexylethyl methacrylate.

2. The hydrophobic flocculant according to claim 1, characterized in that The copolymer has a cationic degree of 10-50% and a hydrophobic degree of 2.5-17.5%.

3. The method for preparing a hydrophobic flocculant according to any one of claims 1 to 2, characterized in that: The copolymer is polymerized by using acrylamide as the main chain monomer, methacrylamidopropyltrimethylammonium chloride as the cationic monomer, and perfluorohexylethyl methacrylate as the hydrophobic monomer through low-pressure ultraviolet initiation.

4. The preparation method according to claim 3, characterized in that: The specific steps include: S1. Mix a certain amount of hydrophobic monomer, surfactant and deionized water, adjust the pH of the reaction system to 2.5-5.5, and obtain a transparent solution after sufficient dispersion, which is liquid A; S2, adding a certain amount of acrylamide monomer, cationic monomer and solubilizer to liquid A, introducing nitrogen protection throughout the process, and fully mixing at room temperature to obtain liquid B; S3, adding a certain amount of photoinitiator to liquid B, after fully mixing, transferring the mixed liquid to a light irradiation reaction device; S4, irradiating with a low-pressure ultraviolet lamp for a certain period of time, and curing at room temperature for 2 to 4 hours to obtain a gelatinous substance C; S5, transferring the colloid C into a mixture of ethanol and acetone, and chopping it into pieces, so as to fully wash it to obtain a solid D; S6. Dry the solid D for 24 hours and grind it to obtain a finished flocculant.

5. The preparation method according to claim 4, characterized in that: The surfactant in step S1 is hexadecyltrimethylammonium bromide, the solubilizer in step S2 is urea, and the photoinitiator in step S3 is one of azobisisobutylamidine hydrochloride, azobisisopropylimidazoline hydrochloride, azobiscyanovaleric acid, azobisimidazoline propane, and irgacure2959.

6. The preparation method according to claim 4, characterized in that: In step S2, the total monomer mass of the hydrophobic monomer, acrylamide monomer and cationic monomer accounts for 15-45% of the mass of liquid B, the molar mass of the cationic monomer accounts for 10-50% of the total monomers, and the molar mass ratio of the acrylamide monomer to the hydrophobic monomer is (7.75-6.25):(0.25-1.75).

7. The preparation method according to claim 6, characterized in that: The amount of surfactant used in step S1 is 1.3-5.3% of the total monomer mass fraction, the amount of solubilizer used in step S2 is 0.1-0.7% of the total monomer mass fraction, and the amount of photoinitiator used in step S3 is 0.01-0.07% of the total monomer mass fraction.

8. The preparation method according to claim 4, characterized in that: The low-pressure ultraviolet lamp in step S4 is 24W or 48W, the radiation wavelength is 253.7nm, and the light radiation reaction time is 2-8h.

9. Use of the hydrophobic flocculant according to any one of claims 1 to 2 in wastewater treatment.

Citation Information

Patent Citations

  • Novel hydrophobically modified cationic polymers and personal care compositions thereof

    CN101484129A

  • Preparation method of hydrophobic modified cationic polyacrylamide flocculant

    CN103319652A

  • Aqueous solution polymerization preparation method of methacrylamidopropyltrimethylammonium chloride and acrylamide copolymer

    CN105111366A

  • Cationic functional fluorine-containing polymer and preparation method thereof

    CN105985495A

  • Quaternary ammonium cationic type water-borne fluorine containing polyacrylate and emulsion and preparation of emulsion

    CN106749878A