Bi-component polymer-based self-leveling plugging material as well as preparation method and application thereof
By optimizing raw material formulation and preparation methods, a two-component polymer-based self-leveling sealing material was developed, solving the problem of difficult balance between existing materials between multiple properties, and achieving high hardness, strength, flame retardancy and antibacterial The comprehensive performance improvement is suitable for high-demand applications in multiple industries.
Patent Information
- Application Number
- CN202411189969.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing self-leveling sealing materials are difficult to balance multiple key properties, and there are shortcomings in weather resistance, fire resistance, environmental protection, etc., which cannot meet the increasingly stringent application needs.
Develop a two-component polymer-based self-leveling sealing material, using poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, tributyl citrate by optimizing raw material formulation and preparation method. Esters, isobutylene sulfide and other components form materials with excellent comprehensive properties, including products with high hardness, strength, flame retardant and antibacterial properties.
It has achieved a balance of multiple performance indicators, met the needs of high-demand application occasions, improved the environmental protection performance and weather resistance of materials, broadened the scope of application, and was suitable for construction, electricity, chemical and other fields.
Smart Images

Figure CN119081459A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified organic materials, and in particular relates to an improved two-component polymer-based self-leveling plugging material and a preparation method and application thereof. Background Art
[0002] As an important functional material, self-leveling plugging materials have extensive and important applications in the fields of construction, electricity, chemical industry, aerospace, etc. This type of material is mainly used for sealing gaps, filling cavities, waterproofing and moisture-proofing, sound insulation and noise reduction, etc., which is of great significance to ensuring the quality and safety of projects. With the continuous advancement of industrial technology and the increasingly complex application environment, the performance requirements for self-leveling plugging materials are also constantly increasing, prompting the continued in-depth research on related issues.
[0003] The common self-leveling plugging materials on the market mainly include epoxy resins, polyurethanes, silicones, acrylates, etc. Although these materials have good performance in terms of sealing and fluidity, they still have some shortcomings and are difficult to meet the increasingly stringent application requirements:
[0004] 1. Epoxy resin materials:
[0005] Epoxy resin self-leveling plugging materials have excellent bonding strength and chemical resistance and are widely used in industrial floors, equipment foundations, etc. However, this type of material has the following problems:
[0006] (1) High hardness and brittleness, easy to crack in an environment with drastic temperature changes, affecting the sealing effect;
[0007] (2) Poor weather resistance, yellowing and powdering may occur when exposed to outdoor environment for a long time;
[0008] (3) A certain degree of shrinkage will occur during the curing process, resulting in stress between the substrate and the substrate, affecting the bonding effect;
[0009] (4) It is sensitive to moisture and the curing quality is difficult to guarantee in a humid environment.
[0010] 2. Polyurethane materials:
[0011] Polyurethane self-leveling sealing materials have good elasticity and wear resistance and are widely used in building joints, floors and other fields. However, this type of material also faces some challenges:
[0012] (1) Poor weather resistance and chemical resistance, especially prone to degradation under strong ultraviolet radiation and acid-base environment, with limited service life;
[0013] (2) It is easily affected by moisture and foaming occurs under humid conditions, affecting the sealing effect;
[0014] (3) Some polyurethane materials release a small amount of isocyanate during the curing process, which poses a potential risk to the environment and the health of construction workers;
[0015] (4) The temperature resistance is limited and it is easy to soften and deform in high temperature environment.
[0016] 3. Silicone materials:
[0017] Silicone self-leveling plugging materials have excellent weather resistance and good elasticity, and are widely used in building exterior walls, curtain walls and other fields. However, this type of material also has some limitations:
[0018] (1) Low strength, not suitable for load-bearing parts or applications requiring high strength;
[0019] (2) The bonding performance with some substrates is poor, and a primer is required for surface treatment;
[0020] (3) The curing speed is relatively slow, especially in low temperature or high humidity environment;
[0021] (4) Some silicone materials release a small amount of volatile organic compounds (VOCs) during the curing process, which affects the indoor air quality.
[0022] 4. Acrylic materials:
[0023] Acrylic self-leveling plugging materials have good weather resistance and fast curing properties, and are used in road markings, waterproof coatings and other fields. However, this type of material also faces some problems:
[0024] (1) Poor solvent resistance, easily corroded by organic solvents;
[0025] (2) Poor low temperature performance, becoming brittle and cracking in cold environments;
[0026] (3) Large shrinkage rate leads to stress concentration and cracking;
[0027] (4) Some acrylic materials will produce pungent odor during the curing process, affecting the construction environment.
[0028] In addition to the problems of the above materials, most self-leveling sealing materials currently have the following common problems:
[0029] Poor fire performance:
[0030] Many self-leveling sealing materials are prone to deformation, softening, or even burning in high temperature environments, and cannot meet the increasingly stringent fire protection requirements. Especially in some special places, such as power facilities, chemical plants, etc., the fire resistance of the material is directly related to the safety of the entire project. Existing self-leveling sealing materials often perform well in some aspects, but have obvious shortcomings in other aspects. For example, some materials have good sealing but poor weather resistance, and some materials have high strength but insufficient flexibility. How to strike a balance between multiple key performances and achieve a comprehensive improvement in comprehensive performance is a major difficulty in current research.
[0031] In view of the many problems and shortcomings of the above-mentioned existing technologies, the development of a new self-leveling plugging material with excellent comprehensive performance has important practical application value and far-reaching social significance. In particular, materials that have achieved breakthroughs in fire resistance, weather resistance, environmental protection, and intelligent responsiveness will effectively promote the technological upgrading and sustainable development of related industries. Summary of the invention
[0032] In view of the problems existing in the above-mentioned prior art, the present invention provides a two-component polymer-based self-leveling plugging material and its preparation method and application. A systematic study is conducted from aspects such as raw material selection, formula optimization, preparation method, and performance characterization to develop a two-component polymer-based self-leveling plugging material with excellent comprehensive performance. This material not only overcomes the shortcomings of the prior art and achieves breakthroughs in weather resistance, flame retardancy, and antibacterial properties, but also has broad application prospects and can effectively promote technological progress in related industries. The materials and preparation methods provided by the present invention have significant innovation and practicality, and are of great significance to promoting the development of polymer-based functional materials.
[0033] To solve the above problems, the present invention adopts the following technical solutions:
[0034] A two-component polymer-based self-leveling plugging material.
[0035] In parts by weight, it includes the following components:
[0036] Component A:
[0037] Poly(dimethylsiloxane): 55 parts to 72 parts;
[0038] N,N-dimethylformamide: 25-35 parts;
[0039] Acrylic acid: 5-10 parts;
[0040] Methoxy polyethylene glycol acrylate: 10 parts to 20 parts;
[0041] Component B:
[0042] Tributyl citrate: 1-3 parts;
[0043] Dioctyl phthalate: 5-10 parts;
[0044] Sulfurized isobutylene: 2-10 parts;
[0045] β-glycerophosphate: 1-3 parts;
[0046] Polyethylene glycol dioleate: 2 parts to 7 parts.
[0047] The present invention selects poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, methoxy polyethylene glycol acrylate as component A, tributyl citrate, dioctyl phthalate, isobutylene sulfide, β-glycerophosphoric acid, polyethylene glycol dioleate as component B. These raw materials have their own unique properties, and a polymer material with excellent performance can be obtained through synergistic action. The present invention optimizes the dosage ratio of each component through a large number of experiments. The dosage of poly(dimethylsiloxane) in component A is 55-72 parts, which can provide good weather resistance and flexibility; the dosage of N,N-dimethylformamide is 25-35 parts, which can promote the reaction; the dosage of acrylic acid is 5-10 parts, which can improve the polarity and adhesion of the material; the dosage of methoxy polyethylene glycol acrylate is 10-20 parts, which can improve the hydrophilicity and flexibility of the material. The dosage of each auxiliary agent in component B is also optimized, which can play multiple functions such as plasticization, flame retardancy, and antibacterial. At the same time, the dosage of dioctyl phthalate is usually 20-30 parts, and the addition of tributyl citrate can reduce the dosage of dioctyl phthalate and also achieve good results.
[0048] Preferably, the above-mentioned two-component polymer-based self-leveling plugging material,
[0049] In parts by weight, it includes the following components:
[0050] Component A:
[0051] Poly(dimethylsiloxane): 60 parts to 72 parts;
[0052] N,N-dimethylformamide: 30-35 parts;
[0053] Acrylic acid: 5-8 parts;
[0054] Methoxy polyethylene glycol acrylate: 15-20 parts;
[0055] Component B:
[0056] Tributyl citrate: 1-3 parts;
[0057] Dioctyl phthalate: 5-10 parts;
[0058] Sulfurized isobutylene: 2-6 parts;
[0059] β-glycerophosphate: 1-3 parts;
[0060] Polyethylene glycol dioleate: 2 parts to 7 parts.
[0061] Preferably, the above-mentioned two-component polymer-based self-leveling plugging material,
[0062] In parts by weight, it includes the following components:
[0063] Component A:
[0064] Poly(dimethylsiloxane): 66 parts;
[0065] N,N-dimethylformamide: 33 parts;
[0066] Acrylic acid: 7 parts;
[0067] Methoxy polyethylene glycol acrylate: 18 parts;
[0068] Component B:
[0069] Tributyl citrate: 2 parts;
[0070] Dioctyl phthalate: 8 parts;
[0071] Sulfurized isobutylene: 4 parts;
[0072] β-Glycerol phosphate: 2 parts;
[0073] Polyethylene glycol dioleate: 5 parts.
[0074] A method for preparing a two-component polymer-based self-leveling plugging material comprises the following steps:
[0075] (1) Weighing poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate, adding them to deionized water and mixing them evenly to obtain a premixture; wherein a catalyst is added to the obtained premixture, wherein the catalyst is one of dibutyltin dilaurate, triethylamine, benzoyl peroxide, and 1,8-diazabicyclo[5.4.0]undec-7-ene, and the amount of the catalyst is 0.12 times the mass of the premixture; the method for mixing evenly is ultrasonic water bath heating, wherein the power of the ultrasound is 100-200 W, and the temperature of the water bath heating is 65-80° C.;
[0076] (2) tributyl citrate, dioctyl phthalate, and polyethylene glycol dioleate are added to the premixture in sequence, and after stirring evenly, isobutylene sulfide and β-glycerophosphoric acid are added, and the mixture is transferred into a reaction kettle lined with polytetrafluoroethylene, air is removed, nitrogen is introduced as a protective gas, the temperature is raised to 110° C.-130° C., the reaction is continued for 6 h-12 h, and the mixture is washed 3 times with a modified cleaning solution, and then concentrated under reduced pressure, and filtered using a dialysis bag to obtain a product; wherein the stirring and mixing method is an oil bath, and the temperature of the oil bath is The temperature is 85-90°C, and the oil bath time is 1.5-3h. The modified cleaning solution is prepared by mixing the components in proportion by weight, and the ratio of anhydrous ethanol: acetone: trichloromethane: (3-aminopropyl) trimethoxysilane is (20-40): (3-8): (5-10): (7-18). The pressure parameter of the vacuum concentration is 2-5kPa, and the volume multiple of the vacuum concentration is 3 times to 5 times. The retention relative molecular mass of the dialysis bag is 8000-10000, and the filtration time is 2-4d.
[0077] In addition, the modified cleaning fluid, anhydrous ethanol: as the main component of the cleaning agent, it can dissolve and remove dirt and residues on the surface and inside of the material. Acetone: as an auxiliary component of the cleaning agent, it can dissolve and remove oily dirt on the surface and inside of the material. Chloroform: as an auxiliary component of the cleaning agent, it can dissolve and remove granular dirt on the surface and inside of the material. (3-Aminopropyl) trimethoxysilane: as an auxiliary component of the cleaning agent, it can improve the cleanliness and smoothness of the material surface. Dimethoxypropane: as an auxiliary component of the cleaning agent, it can improve the cleanliness and smoothness of the material surface. In general, the cleaning agent can effectively remove dirt and residues on the surface and inside of the material through the mechanisms of dissolution, emulsification, dispersion and surface activity, improve the cleanliness and smoothness of the material, and facilitate subsequent processing and application.
[0078] The use of the two-component polymer-based self-leveling plugging material as described above in the preparation of fireproof components.
[0079] The present invention adopts a preparation method of premixing-polycondensation reaction-washing-drying. First, the raw materials of component A are mixed uniformly to obtain a premixture, and then the auxiliary agent of component B is added, and a polycondensation reaction is carried out under specific conditions, and the target product is obtained after washing and drying. The method is simple and controllable, and the product quality is stable. The two-component polymer-based self-leveling plugging material prepared by the present invention has excellent comprehensive performance, a Shore hardness of up to 92-96, a tensile strength of 74-80MPa, and a compressive strength of 1.08-1.10MPa. At the same time, it has excellent weather resistance, flame retardancy and antibacterial properties, and can meet a variety of application requirements. The material prepared by the present invention can be widely used in the fields of construction, electric power, chemical industry, etc., and is particularly suitable for occasions with high requirements for fire resistance. The material can be used for sealing gaps, filling cavities, waterproofing and moisture-proofing, sound insulation and noise reduction, etc., which greatly broadens the application range of polymer-based self-leveling plugging materials.
[0080] In addition, the main chemical reactions occurring between the components are as follows:
[0081] Free radical polymerization: Under the action of the crosslinking agent β-glycerophosphate, monomers containing carbon-carbon double bonds such as acrylic acid, methoxy polyethylene glycol acrylate, and isobutylene sulfide can undergo free radical polymerization to form a polymer backbone. Among them, acrylic acid and methoxy polyethylene glycol acrylate can form random copolymers, while isobutylene sulfide mainly forms homopolymers.
[0082] Siloxane polycondensation reaction: Polydimethylsiloxane can undergo polycondensation reaction at high temperature (90℃-120℃) under nitrogen conditions to form a cross-linked network structure. This reaction occurs during the polymer molding process and improves the mechanical properties and heat resistance of the material.
[0083] Esterification / etherification reaction: The carboxyl group in the acrylic acid molecule undergoes an esterification reaction with the hydroxyl group in the methoxy polyethylene glycol acrylate or polyethylene glycol dioleate molecule; at the same time, the carboxyl group in the acrylic acid also undergoes an etherification reaction with the hydroxyl group in the polyethylene glycol chain segment. These reactions help to increase the branching degree and molecular weight of the polymer.
[0084] Hydrogen bonding: Carboxyl, hydroxyl and other groups contained in molecules such as acrylic acid and β-glycerophosphate can form intermolecular or intramolecular hydrogen bonds, affecting the solubility, crystallinity and other properties of the polymer.
[0085] Compatibility: Non-polar components such as isobutylene sulfide can form a homogeneous blend with polydimethylsiloxane to improve the flexibility of the material; while polar components such as N,N-dimethylformamide and acrylic acid help to improve the compatibility of the system.
[0086] Plasticizing effect: Plasticizers such as dioctyl phthalate and tributyl citrate can be inserted between polymer molecular chains, reducing intermolecular forces and improving the flexibility and ductility of the material.
[0087] Compared with the prior art, the present invention has the following beneficial effects:
[0088] Excellent comprehensive performance: The two-component polymer-based self-leveling plugging material developed by the present invention performs well in multiple performance indicators such as hardness, strength, flame retardancy, and temperature resistance, achieving a balance of multiple key performances and meeting the needs of high-demand applications. Improved environmental performance: The present invention adopts environmentally friendly plasticizer tributyl citrate to replace the traditional phthalate plasticizer, reducing the environmental risk of the material. At the same time, the release of volatile organic compounds is reduced by optimizing the formula, thereby improving the environmental performance of the material. Improved weather resistance: The introduction of sulfided isobutylene and β-glycerophosphate can improve the material's UV resistance and hydrolysis stability, improve the material's weather resistance in outdoor environments, and extend its service life. Optimized bonding performance: The introduction of acrylic acid monomers improves the polarity of the material, improves the bonding force with a variety of substrates, and ensures a good plugging effect. Methoxy polyethylene glycol acrylate plays a role in optimizing the interface, further enhancing the bonding performance of the material. Improved processing performance: The use of N, N-dimethylformamide as a reaction solvent reduces the viscosity of the system, improves the compatibility of the raw materials, and is conducive to the polymerization reaction. The optimized preparation method improves production efficiency and reduces costs. Broadened scope of application: The excellent comprehensive performance enables the two-component polymer-based self-leveling plugging material of the present invention to be widely used in multiple fields such as construction, electricity, chemical industry, aerospace, etc., and is especially suitable for occasions with high requirements for fire resistance. By optimizing the material formula and preparation method, the present invention improves the environmental protection, weather resistance, adhesion, etc. of the material while ensuring excellent comprehensive performance, thereby broadening the scope of application and showing significant technical advantages and application value. Compared with the existing technology, it has obvious innovation and advancement. BRIEF DESCRIPTION OF THE DRAWINGS
[0089] Figure 1 This is a physical picture of the two-component polymer-based self-leveling plugging material prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0090] The present invention is further described in conjunction with specific embodiments.
[0091] The CAS numbers, manufacturers, etc. of the chemical reagents used in the examples and comparative examples of the present invention, and other reagents not mentioned were purchased from Sinopharm Chemical Reagent Co., Ltd., and the information is as follows:
[0092]
[0093]
[0094] Example 1
[0095] Two-component polymer-based self-leveling plugging material.
[0096] In parts by weight, it includes the following components:
[0097] Component A:
[0098] Poly(dimethylsiloxane): 55 parts;
[0099] N,N-dimethylformamide: 35 parts;
[0100] Acrylic acid: 5 parts;
[0101] Methoxy polyethylene glycol acrylate: 20 parts;
[0102] Component B:
[0103] Tributyl citrate: 1 part;
[0104] Dioctyl phthalate: 10 parts;
[0105] Sulfurized isobutylene: 2 parts;
[0106] β-Glycerol phosphate: 3 parts;
[0107] Polyethylene glycol dioleate: 2 parts.
[0108] The above-mentioned two-component polymer-based self-leveling plugging material,
[0109] The parameters of poly(dimethylsiloxane) are as follows:
[0110] Density: 0.96g / cm 3 , viscosity: 800000cSt.
[0111] The above-mentioned two-component polymer-based self-leveling plugging material,
[0112] The parameters of N,N-dimethylformamide are as follows:
[0113] Density: 0.944 g / cm 3 , viscosity: 0.92mPa·s.
[0114] The above-mentioned two-component polymer-based self-leveling plugging material,
[0115] The parameters of acrylic acid are as follows:
[0116] Density: 1.051 g / cm 3 , viscosity: 1.25mPa·s.
[0117] The above-mentioned two-component polymer-based self-leveling plugging material,
[0118] The parameters of methoxy polyethylene glycol acrylate are as follows:
[0119] Density: 1.08 g / mL, molecular weight: ~2000 g / mol.
[0120] The above-mentioned two-component polymer-based self-leveling plugging material,
[0121] The parameters of tributyl citrate are as follows: density is 1.042g / cm 3 , boiling point is 170℃, viscosity is 37.6mPa.s;
[0122] The parameters of dioctyl phthalate are as follows: density is 0.98g / cm 3 , viscosity is 79mPa·s;
[0123] The parameters of sulfided isobutylene are as follows: density is 0.917 g / cm 3 , the glass transition temperature is -76°C;
[0124] The parameters of β-glycerophosphate are as follows: appearance is white crystalline powder;
[0125] The parameters of polyethylene glycol dioleate are as follows: the appearance is amber oily liquid, and the HLB value is 8.
[0126] A method for preparing a two-component polymer-based self-leveling plugging material comprises the following steps:
[0127] (1) Weighing poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate, adding them to deionized water 20 times the total mass of the above substances (i.e., poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate) and mixing them evenly to obtain a premixture; wherein a catalyst is added to the obtained premixture, wherein the catalyst is dibutyltin dilaurate, and the amount of the catalyst is 0.12 times the mass of the premixture; the method for mixing evenly is ultrasonic water bath heating, wherein the ultrasonic power is 100 W, and the water bath heating temperature is 80° C.;
[0128] (2) tributyl citrate, dioctyl phthalate and polyethylene glycol dioleate are added to the premixture in sequence, stirred evenly, and then isobutylene sulfide and β-glycerophosphoric acid are added, and the mixture is transferred into a reactor lined with polytetrafluoroethylene, air is removed, nitrogen is introduced as a protective gas, the temperature is raised to 110° C., the reaction is continued for 12 hours, and the mixture is washed three times with a modified cleaning solution, and then concentrated under reduced pressure, and filtered using a dialysis bag to obtain a product; wherein the stirring and mixing method is an oil bath, wherein the temperature of the oil bath is 85° C., and the oil bath time is 3 hours; the modified cleaning solution is a mixture of components in parts by weight, wherein the ratio of anhydrous ethanol: acetone: trichloromethane: (3-aminopropyl) trimethoxysilane is 20:8:5:18; the pressure parameter of the reduced pressure concentration is 2 kPa, and the volume multiple of the reduced pressure concentration is 5 times; the cutoff relative molecular mass of the dialysis bag is 8000, and the filtration time is 4 days.
[0129] Example 2
[0130] Two-component polymer-based self-leveling plugging material.
[0131] In parts by weight, it includes the following components:
[0132] Component A:
[0133] Poly(dimethylsiloxane): 72 parts;
[0134] N,N-dimethylformamide: 25 parts;
[0135] Acrylic acid: 10 parts;
[0136] Methoxy polyethylene glycol acrylate: 10 parts;
[0137] Component B:
[0138] Tributyl citrate: 3 parts;
[0139] Dioctyl phthalate: 5 parts;
[0140] Sulfurized isobutylene: 10 parts;
[0141] β-Glycerol phosphate: 1 part;
[0142] Polyethylene glycol dioleate: 7 parts.
[0143] The above-mentioned two-component polymer-based self-leveling plugging material,
[0144] The parameters of poly(dimethylsiloxane) are as follows:
[0145] Density: 0.96g / cm 3 , viscosity: 800000cSt.
[0146] The above-mentioned two-component polymer-based self-leveling plugging material,
[0147] The parameters of N,N-dimethylformamide are as follows:
[0148] Density: 0.944 g / cm 3 , viscosity: 0.92mPa·s.
[0149] The above-mentioned two-component polymer-based self-leveling plugging material,
[0150] The parameters of acrylic acid are as follows:
[0151] Density: 1.051 g / cm 3 , viscosity: 1.25mPa·s.
[0152] The above-mentioned two-component polymer-based self-leveling plugging material,
[0153] The parameters of methoxy polyethylene glycol acrylate are as follows:
[0154] Density: 1.08 g / mL, molecular weight: ~2000 g / mol.
[0155] The above-mentioned two-component polymer-based self-leveling plugging material,
[0156] The parameters of tributyl citrate are as follows: density is 1.042g / cm 3 , boiling point is 170℃, viscosity is 37.6mPa.s;
[0157] The parameters of dioctyl phthalate are as follows: density is 0.98g / cm 3 , viscosity is 79mPa·s;
[0158] The parameters of sulfided isobutylene are as follows: density is 0.917 g / cm 3 , the glass transition temperature is -76°C;
[0159] The parameters of β-glycerophosphate are as follows: appearance is white crystalline powder;
[0160] The parameters of polyethylene glycol dioleate are as follows: the appearance is amber oily liquid, and the HLB value is 10.
[0161] A method for preparing a two-component polymer-based self-leveling plugging material comprises the following steps:
[0162] (1) Weighing poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate, adding them to deionized water 30 times the total mass of the above substances (i.e., poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate) and mixing them evenly to obtain a premixture; wherein a catalyst is added to the obtained premixture, wherein the catalyst is triethylamine, and the amount of the catalyst is 0.12 times the mass of the premixture; the method for mixing evenly is ultrasonic water bath heating, wherein the ultrasonic power is 200 W, and the water bath heating temperature is 65° C.;
[0163] (2) tributyl citrate, dioctyl phthalate and polyethylene glycol dioleate are added to the premixture in sequence, stirred evenly, and then isobutylene sulfide and β-glycerophosphoric acid are added, and the mixture is transferred into a reactor lined with polytetrafluoroethylene, air is removed, nitrogen is introduced as a protective gas, the temperature is raised to 130° C., the reaction is continued for 6 hours, and the mixture is washed 3 times with a modified cleaning solution, and then concentrated under reduced pressure, and filtered using a dialysis bag to obtain a product; wherein the stirring and mixing method is an oil bath, wherein the temperature of the oil bath is 90° C., and the time of the oil bath is 1.5 hours; the modified cleaning solution is a mixture of components in parts by weight, wherein the ratio of anhydrous ethanol: acetone: trichloromethane: (3-aminopropyl) trimethoxysilane is 40:3:10:7; the pressure parameter of the reduced pressure concentration is 5 kPa, and the volume multiple of the reduced pressure concentration is 3 times; the cutoff relative molecular mass of the dialysis bag is 10,000, and the filtration time is 2 days.
[0164] Example 3
[0165] Two-component polymer-based self-leveling plugging material.
[0166] In parts by weight, it includes the following components:
[0167] Component A:
[0168] Poly(dimethylsiloxane): 60 parts;
[0169] N,N-dimethylformamide: 35 parts;
[0170] Acrylic acid: 5 parts;
[0171] Methoxy polyethylene glycol acrylate: 20 parts;
[0172] Component B:
[0173] Tributyl citrate: 1 part;
[0174] Dioctyl phthalate: 10 parts;
[0175] Sulfurized isobutylene: 2 parts;
[0176] β-Glycerol phosphate: 3 parts;
[0177] Polyethylene glycol dioleate: 2 parts.
[0178] The above-mentioned two-component polymer-based self-leveling plugging material,
[0179] The parameters of poly(dimethylsiloxane) are as follows:
[0180] Density: 0.96g / cm 3 , viscosity: 800000cSt.
[0181] The above-mentioned two-component polymer-based self-leveling plugging material,
[0182] The parameters of N,N-dimethylformamide are as follows:
[0183] Density: 0.944 g / cm 3 , viscosity: 0.92mPa·s.
[0184] The above-mentioned two-component polymer-based self-leveling plugging material,
[0185] The parameters of acrylic acid are as follows:
[0186] Density: 1.051 g / cm 3 , viscosity: 1.25mPa·s.
[0187] The above-mentioned two-component polymer-based self-leveling plugging material,
[0188] The parameters of methoxy polyethylene glycol acrylate are as follows:
[0189] Density: 1.08 g / mL, molecular weight: ~2000 g / mol.
[0190] The above-mentioned two-component polymer-based self-leveling plugging material,
[0191] The parameters of tributyl citrate are as follows: density is 1.042g / cm 3 , boiling point is 170°C, viscosity is 37.6mPa·s;
[0192] The parameters of dioctyl phthalate are as follows: density is 0.98g / cm 3 , viscosity is 79mPa·s;
[0193] The parameters of sulfided isobutylene are as follows: density is 0.917 g / cm 3 , the glass transition temperature is -76°C;
[0194] The parameters of β-glycerophosphate are as follows: appearance is white crystalline powder;
[0195] The parameters of polyethylene glycol dioleate are as follows: the appearance is amber oily liquid, and the HLB value is 8.
[0196] A method for preparing a two-component polymer-based self-leveling plugging material comprises the following steps:
[0197] (1) Weighing poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate, adding them to deionized water 22 times the total mass of the above substances (i.e., poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate) and mixing them evenly to obtain a premixture; wherein a catalyst is added to the obtained premixture, wherein the catalyst is benzoyl peroxide, and the amount of the catalyst is 0.12 times the mass of the premixture; the method for mixing evenly is ultrasonic water bath heating, wherein the ultrasonic power is 100 W, and the water bath heating temperature is 65° C.;
[0198] (2) tributyl citrate, dioctyl phthalate and polyethylene glycol dioleate are added to the premixture in sequence, stirred evenly, and then isobutylene sulfide and β-glycerophosphoric acid are added, and the mixture is transferred into a reactor lined with polytetrafluoroethylene, air is removed, nitrogen is introduced as a protective gas, the temperature is raised to 110° C., the reaction is continued for 6 hours, and the mixture is washed 3 times with a modified cleaning solution, and then concentrated under reduced pressure, and filtered using a dialysis bag to obtain a product; wherein the stirring and mixing method is an oil bath, wherein the temperature of the oil bath is 85° C., and the oil bath time is 1.5 hours; the modified cleaning solution is a mixture of components in parts by weight, wherein the ratio of anhydrous ethanol: acetone: trichloromethane: (3-aminopropyl) trimethoxysilane is 20:3:5:7; the pressure parameter of the reduced pressure concentration is 2 kPa, and the volume multiple of the reduced pressure concentration is 3 times; the cutoff relative molecular mass of the dialysis bag is 8000, and the filtration time is 2 days.
[0199] Example 4
[0200] Two-component polymer-based self-leveling plugging material.
[0201] In parts by weight, it includes the following components:
[0202] Component A:
[0203] Poly(dimethylsiloxane): 72 parts;
[0204] N,N-dimethylformamide: 30 parts;
[0205] Acrylic acid: 8 parts;
[0206] Methoxy polyethylene glycol acrylate: 15 parts;
[0207] Component B:
[0208] Tributyl citrate: 3 parts;
[0209] Dioctyl phthalate: 5 parts;
[0210] Sulfurized isobutylene: 6 parts;
[0211] β-Glycerol phosphate: 1 part;
[0212] Polyethylene glycol dioleate: 7 parts.
[0213] The above-mentioned two-component polymer-based self-leveling plugging material,
[0214] The parameters of poly(dimethylsiloxane) are as follows:
[0215] Density: 0.96g / cm 3 , viscosity: 800000cSt.
[0216] The above-mentioned two-component polymer-based self-leveling plugging material,
[0217] The parameters of N,N-dimethylformamide are as follows:
[0218] Density: 0.944 g / cm 3 , viscosity: 0.92mPa·s.
[0219] The above-mentioned two-component polymer-based self-leveling plugging material,
[0220] The parameters of acrylic acid are as follows:
[0221] Density: 1.051 g / cm 3 , viscosity: 1.25mPa·s.
[0222] The above-mentioned two-component polymer-based self-leveling plugging material,
[0223] The parameters of methoxy polyethylene glycol acrylate are as follows:
[0224] Density: 1.08 g / mL, molecular weight: ~2000 g / mol.
[0225] The above-mentioned two-component polymer-based self-leveling plugging material,
[0226] The parameters of tributyl citrate are as follows: density is 1.042g / cm 3 , boiling point is 170°C, viscosity is 37.6mPa·s;
[0227] The parameters of dioctyl phthalate are as follows: density is 0.98g / cm 3 , viscosity is 79mPa·s;
[0228] The parameters of sulfided isobutylene are as follows: density is 0.917 g / cm 3 , the glass transition temperature is -76°C;
[0229] The parameters of β-glycerophosphate are as follows: appearance is white crystalline powder;
[0230] The parameters of polyethylene glycol dioleate are as follows: the appearance is an amber oily liquid, and the HLB value is 8-10.
[0231] A method for preparing a two-component polymer-based self-leveling plugging material comprises the following steps:
[0232] (1) Weighing poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate, adding them to deionized water 27 times the total mass of the above substances (i.e., poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate) and mixing them evenly to obtain a premixture; wherein a catalyst is added to the obtained premixture, wherein the catalyst is 1,8-diazabicyclo[5.4.0]undec-7-ene, and the amount of the catalyst is 0.12 times the mass of the premixture; the method for mixing evenly is ultrasonic water bath heating, wherein the ultrasonic power is 200 W, and the water bath heating temperature is 80° C.;
[0233] (2) tributyl citrate, dioctyl phthalate and polyethylene glycol dioleate are added to the premixture in sequence, stirred evenly, and then isobutylene sulfide and β-glycerophosphoric acid are added, and the mixture is transferred into a reactor lined with polytetrafluoroethylene, air is removed, nitrogen is introduced as a protective gas, the temperature is raised to 130° C., the reaction is continued for 12 hours, and the mixture is washed three times with a modified cleaning solution, and then concentrated under reduced pressure, and filtered using a dialysis bag to obtain a product; wherein the stirring and mixing method is an oil bath, wherein the temperature of the oil bath is 90° C., and the oil bath time is 3 hours; the modified cleaning solution is a mixture of components in parts by weight, wherein the ratio of anhydrous ethanol: acetone: trichloromethane: (3-aminopropyl) trimethoxysilane is 40:8:10:18; the pressure parameter of the reduced pressure concentration is 5 kPa, and the volume multiple of the reduced pressure concentration is 5 times; the cutoff relative molecular mass of the dialysis bag is 10,000, and the filtration time is 4 days.
[0234] Example 5
[0235] Two-component polymer-based self-leveling plugging material.
[0236] In parts by weight, it includes the following components:
[0237] Component A:
[0238] Poly(dimethylsiloxane): 66 parts;
[0239] N,N-dimethylformamide: 33 parts;
[0240] Acrylic acid: 7 parts;
[0241] Methoxy polyethylene glycol acrylate: 18 parts;
[0242] Component B:
[0243] Tributyl citrate: 2 parts;
[0244] Dioctyl phthalate: 8 parts;
[0245] Sulfurized isobutylene: 4 parts;
[0246] β-Glycerol phosphate: 2 parts;
[0247] Polyethylene glycol dioleate: 5 parts.
[0248] The above-mentioned two-component polymer-based self-leveling plugging material,
[0249] The parameters of poly(dimethylsiloxane) are as follows:
[0250] Density: 0.96g / cm 3 , viscosity: 800000cSt.
[0251] The above-mentioned two-component polymer-based self-leveling plugging material,
[0252] The parameters of N,N-dimethylformamide are as follows:
[0253] Density: 0.944 g / cm 3 , viscosity: 0.92mPa·s.
[0254] The above-mentioned two-component polymer-based self-leveling plugging material,
[0255] The parameters of acrylic acid are as follows:
[0256] Density: 1.051 g / cm 3 , viscosity: 1.25mPa·s.
[0257] The above-mentioned two-component polymer-based self-leveling plugging material,
[0258] The parameters of methoxy polyethylene glycol acrylate are as follows:
[0259] Density: 1.08 g / mL, molecular weight: ~2000 g / mol.
[0260] The above-mentioned two-component polymer-based self-leveling plugging material,
[0261] The parameters of tributyl citrate are as follows: density is 1.042g / cm 3 , boiling point is 170°C, viscosity is 37.6mPa·s;
[0262] The parameters of dioctyl phthalate are as follows: density is 0.98g / cm 3 , viscosity is 79mPa·s;
[0263] The parameters of sulfided isobutylene are as follows: density is 0.917 g / cm 3 , the glass transition temperature is -76°C;
[0264] The parameters of β-glycerophosphate are as follows: appearance is white crystalline powder;
[0265] The parameters of polyethylene glycol dioleate are as follows: the appearance is an amber oily liquid, and the HLB value is 8-10.
[0266] A method for preparing a two-component polymer-based self-leveling plugging material comprises the following steps:
[0267] (1) Weighing poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate, adding them to deionized water 25 times the total mass of the above substances (i.e., poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate) and mixing them evenly to obtain a premixture; wherein a catalyst is added to the obtained premixture, wherein the catalyst is dibutyltin dilaurate, and the amount of the catalyst is 0.12 times the mass of the premixture; the method for mixing evenly is ultrasonic water bath heating, wherein the ultrasonic power is 150 W, and the water bath heating temperature is 74° C.;
[0268] (2) tributyl citrate, dioctyl phthalate and polyethylene glycol dioleate are added to the premixture in sequence, stirred evenly, and then isobutylene sulfide and β-glycerophosphoric acid are added, and the mixture is transferred into a reactor lined with polytetrafluoroethylene, air is removed, nitrogen is introduced as a protective gas, the temperature is raised to 120° C., the reaction is continued for 9 hours, and the mixture is washed 3 times with a modified cleaning solution, and then concentrated under reduced pressure, and filtered using a dialysis bag to obtain a product; wherein the stirring and mixing method is an oil bath, wherein the temperature of the oil bath is 88° C., and the oil bath time is 2 hours; the modified cleaning solution is a mixture of components in parts by weight, wherein the ratio of anhydrous ethanol: acetone: trichloromethane: (3-aminopropyl) trimethoxysilane is 30:5:8:13; the pressure parameter of the reduced pressure concentration is 4 kPa, and the volume multiple of the reduced pressure concentration is 4 times; the cutoff relative molecular mass of the dialysis bag is 10,000, and the filtration time is 3 days.
[0269] Comparative Example 1
[0270] The two-component polymer-based self-leveling plugging material is based on Example 5, except that N,N-dimethylformamide is removed.
[0271] Comparative Example 2
[0272] The two-component polymer-based self-leveling plugging material is based on Example 5, except that acrylic acid is removed.
[0273] Comparative Example 3
[0274] The two-component polymer-based self-leveling plugging material is based on Example 5, but differs in that methoxy polyethylene glycol acrylate is removed.
[0275] Comparative Example 4
[0276] The two-component polymer-based self-leveling plugging material is based on Example 5, but differs in that tributyl citrate is removed.
[0277] Comparative Example 5
[0278] The two-component polymer-based self-leveling plugging material is based on Example 5, but differs in that the sulfided isobutylene is removed.
[0279] Test Case
[0280] The plugging materials prepared in Examples 1-5 and Comparative Examples 1-5 were selected and the following performance tests were performed:
[0281] The sample size was set to 150 mm × 10 mm × 10 mm.
[0282] The tensile strength is tested according to the standard GB / T528-1998; the Shore A hardness is tested according to the standard GB / T531-1992; the compressive strength is tested according to the standard GB / T 8813-2008; the oxygen index is tested according to the standard GB / T2406-1993; high temperature and low temperature resistance test: placed at 250℃ and -40℃ for detection changes.
[0283] Table 1 Test results of Examples 1-5
[0284]
[0285] As shown in Table 1, the test results of Examples 1-5 show that these two-component polymer-based self-leveling plugging materials show excellent performance in multiple performance indicators: Shore hardness: The Shore hardness of all embodiments is between 92 and 96, indicating that the material has high hardness and good mechanical properties. Tensile strength: The tensile strength is between 74.2MPa and 80.5MPa, showing the high strength characteristics of the material. Oxygen index: The oxygen index is between 32.2% and 34.5%, indicating that the material has good flame retardant properties. High and low temperature resistance: There is no deformation at 250°C and -40°C, showing the excellent temperature resistance of the material. Compressive strength: The compressive strength is between 1.08MPa and 1.10MPa, which further proves the high strength characteristics of the material. These results show that the developed two-component polymer-based self-leveling plugging material performs well in hardness, strength, flame retardancy and temperature resistance, and is suitable for high-demand applications.
[0286] Table 2 Comparative Examples 1-5 Test Results
[0287]
[0288] As shown in Table 2, N,N-dimethylformamide is removed in Comparative Example 1. DMF is a polar non-protonic solvent that can dissolve polymer raw materials such as poly (dimethylsiloxane), acrylic acid, methoxy polyethylene glycol acrylate, etc., reduce the viscosity of the system, and facilitate the polymerization reaction. The end with a positive charge in the DMF molecule is surrounded by a methyl group to form a steric hindrance, so that negative ions cannot approach and can only associate with positive ions. This effect makes many ionic reactions such as nucleophilic substitution easier to carry out in DMF than in protic solvents. DMF can stabilize the active species such as free radicals and negative ions generated during the reaction, extend their lifespan, and thus improve the reaction efficiency. DMF can dissolve a variety of organic and inorganic compounds, can increase the solubility of the polymer product in the system, prevent it from precipitating, and facilitate the polymerization reaction. Therefore, after removing DMF in Comparative Example 1, due to the lack of a suitable solvent, the polymer raw material cannot be completely dissolved, the system viscosity is too high, which is not conducive to monomer diffusion and polymerization reaction. At the same time, the stabilizing effect of DMF on ions and free radicals is lost, the concentration of active species decreases, and the polymerization efficiency decreases. This ultimately leads to incomplete polymerization and reduced product performance. It can be seen that DMF plays a vital role in this system.
[0289] Acrylic acid is removed in Comparative Example 2. Acrylic acid molecules contain active carbon-carbon double bonds and carboxyl groups, and free radical polymerization can occur under the action of initiators. Acrylic acid can be copolymerized with other monomers such as methoxy polyethylene glycol acrylate to form a polymer with acrylic acid structural units. The carboxyl group in the acrylic acid molecule is a polar group, and the introduction of acrylic acid units can increase the polarity of the polymer molecule. The increase in polarity is conducive to improving the hydrophilicity of the material, improving the adhesion to the substrate, and improving the blocking performance. Adjusting the mechanical properties of the polymer: Acrylic acid polymers have a certain rigidity, and the introduction of an appropriate amount of acrylic acid units can adjust the hardness and strength of the polymer. Too much acrylic acid will cause the polymer to be too hard and the flexibility to decrease. It can be seen from the test results of Comparative Example 2 that after removing acrylic acid, the Shore hardness, tensile strength, and compressive strength of the material are all reduced, and deformation occurs at high and low temperatures, indicating that acrylic acid plays an important role in maintaining the mechanical properties of the material. At the same time, the oxygen index is also significantly reduced, which is due to the decrease in polarity causing the dispersion of flame retardant elements to deteriorate. In summary, acrylic acid plays an important role in two-component polymer-based self-leveling plugging materials by participating in polymerization reactions, improving material polarity, and adjusting mechanical properties. An appropriate amount of acrylic acid can improve the material's plugging performance and comprehensive mechanical properties, and is an indispensable key component in the formula.
[0290] Methoxy polyethylene glycol acrylate is removed in Comparative Example 3. The mechanism of action of methoxy polyethylene glycol acrylate in a two-component polymer-based self-leveling plugging material is as follows: Participation in free radical polymerization: Methoxy polyethylene glycol acrylate molecules contain active carbon-carbon double bonds, which can undergo free radical polymerization under the action of an initiator. It can be copolymerized with other monomers such as acrylic acid to form a polymer with a polyethylene glycol segment. Improving the hydrophilicity and flexibility of the material: Methoxy polyethylene glycol acrylate molecules contain hydrophilic polyethylene glycol segments, and the introduction of this component can improve the hydrophilicity of the polymer molecule. At the same time, the polyethylene glycol segment has good flexibility, which can improve the flexibility and ductility of the material. Improving ionic conductivity: The polyethylene glycol segment can promote the migration and conduction of lithium ions, etc., and improve the ionic conductivity of the material. This is conducive to improving the conductive properties of the material. From the test results of Comparative Example 3, it can be seen that after removing methoxy polyethylene glycol acrylate, the Shore hardness of the material increases, indicating that the hardness of the material increases and the flexibility decreases. At the same time, the tensile strength and compressive strength also decreased, indicating that the mechanical properties of the material have deteriorated. This is due to the loss of the contribution of the polyethylene glycol segment to the flexibility of the material. In summary, methoxy polyethylene glycol acrylate plays an important role in two-component polymer-based self-leveling plugging materials by participating in polymerization reactions, improving the hydrophilicity and flexibility of the material, and improving ionic conductivity. The introduction of this component in an appropriate amount can optimize the comprehensive performance of the material and is an indispensable key component in the formula.
[0291] Tributyl citrate is removed in Comparative Example 4. The mechanism of action of tributyl citrate in a two-component polymer-based self-leveling plugging material is as follows: Plasticizing effect: tributyl citrate is an environmentally friendly plasticizer that can increase the flexibility and activity of polymer molecular chains. It can be inserted between polymer molecular chains to reduce intermolecular forces, thereby improving the flexibility of the material. Reduce the glass transition temperature: tributyl citrate can reduce the glass transition temperature (Tg) of the polymer. The reduction in Tg means that the material can move the molecular chain at a lower temperature, showing better flexibility. Improve elongation at break: Adding tributyl citrate can significantly improve the elongation at break of the polymer. This is because tributyl citrate increases the sliding and orientation of the molecular chain, allowing the material to withstand greater deformation without breaking. From the test results of Comparative Example 4, it can be seen that after removing tributyl citrate, the Shore hardness of the material increases, indicating that the material becomes harder and the flexibility decreases. At the same time, deformation occurs at high and low temperatures, indicating that the temperature resistance of the material deteriorates after losing tributyl citrate. In summary, tributyl citrate plays a key toughening role in two-component polymer-based self-leveling plugging materials through mechanisms such as plasticization, lowering glass transition temperature, and increasing elongation at break. Adding tributyl citrate in an appropriate amount can optimize the flexibility and temperature resistance of the material, and is an indispensable key component in the formula.
[0292] In comparative example 5, isobutylene sulfide is removed. The mechanism of action of isobutylene sulfide in the two-component polymer-based self-leveling plugging material is as follows: Participate in free radical polymerization: isobutylene sulfide molecules contain unsaturated double bonds, and free radical polymerization can occur under the action of initiators. It can be copolymerized with other monomers such as acrylic acid, methoxy polyethylene glycol acrylate, etc. to form a polymer with isobutylene sulfide structural units. Improve the strength and toughness of the material: isobutylene sulfide polymers have excellent strength and toughness. The introduction of an appropriate amount of isobutylene sulfide units can improve the tensile strength, compressive strength and other mechanical properties of the polymer. This is due to the flexibility and entanglement of the isobutylene sulfide molecular chain. Give the material antibacterial properties: isobutylene sulfide molecules contain sulfur atoms and have a certain antibacterial effect. Introducing it into a polymer can give the material antibacterial properties and improve the hygienic safety of the material. Improve the compatibility of the material: isobutylene sulfide can form a homogeneous blend with a variety of polymers such as natural rubber, butyl rubber, etc. Adding isobutylene sulfide helps to improve the compatibility between the components of the plugging material and obtain a product with better performance. From the test results of Comparative Example 5, it can be seen that after removing isobutylene sulfide, the tensile strength and compressive strength of the material are reduced, and deformation occurs at high and low temperatures, indicating that isobutylene sulfide plays an important role in maintaining the mechanical properties and temperature resistance of the material. At the same time, the oxygen index is also significantly reduced, which is due to the loss of the antibacterial effect of isobutylene sulfide. In summary, isobutylene sulfide plays an irreplaceable role in two-component polymer-based self-leveling plugging materials by participating in polymerization, improving material toughness, imparting antibacterial properties, and improving compatibility. The appropriate amount of introduction of isobutylene sulfide can comprehensively improve the comprehensive performance of the material and is a key component in the formula.
[0293] The above content is a further detailed description of the present invention in combination with specific implementation methods. It cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the scope of protection determined by the claims submitted for the present invention.
Claims
1. A two-component polymer-based self-leveling plugging material, Features: In parts by weight, it includes the following components: Component A: Poly(dimethylsiloxane): 55 parts to 72 parts; N,N-dimethylformamide: 25-35 parts; Acrylic acid: 5-10 parts; Methoxy polyethylene glycol acrylate: 10 parts to 20 parts; Component B: Tributyl citrate: 1-3 parts; Dioctyl phthalate: 5-10 parts; Sulfurized isobutylene: 2-10 parts; β-glycerophosphate: 1-3 parts; Polyethylene glycol dioleate: 2 parts to 7 parts.
2. The two-component polymer-based self-leveling plugging material according to claim 1, Features: In parts by weight, it includes the following components: Component A: Poly(dimethylsiloxane): 60 parts to 72 parts; N,N-dimethylformamide: 30-35 parts; Acrylic acid: 5-8 parts; Methoxy polyethylene glycol acrylate: 15-20 parts; Component B: Tributyl citrate: 1-3 parts; Dioctyl phthalate: 5-10 parts; Sulfurized isobutylene: 2-6 parts; β-glycerophosphate: 1-3 parts; Polyethylene glycol dioleate: 2 parts to 7 parts.
3. The two-component polymer-based self-leveling plugging material according to claim 2, Features: In parts by weight, it includes the following components: Component A: Poly(dimethylsiloxane): 66 parts; N,N-dimethylformamide: 33 parts; Acrylic acid: 7 parts; Methoxy polyethylene glycol acrylate: 18 parts; Component B: Tributyl citrate: 2 parts; Dioctyl phthalate: 8 parts; Sulfurized isobutylene: 4 parts; β-Glycerol phosphate: 2 parts; Polyethylene glycol dioleate: 5 parts.
4. A method for preparing a two-component polymer-based self-leveling plugging material according to any one of claims 1 to 3, Features: The steps include: (1) Weighing poly(dimethylsiloxane), N,N-dimethylformamide, acrylic acid, and methoxy polyethylene glycol acrylate, adding them to deionized water and mixing them evenly to obtain a premixture; (2) tributyl citrate, dioctyl phthalate, and polyethylene glycol dioleate are added to the premixture in sequence, and after stirring evenly, isobutylene sulfide and β-glycerophosphoric acid are added, and the mixture is transferred into a reaction kettle lined with polytetrafluoroethylene, air is removed, nitrogen is introduced as a protective gas, the temperature is raised to 110° C.-130° C., the reaction is continued for 6 h-12 h, and the mixture is washed 3 times with a modified cleaning solution, and then concentrated under reduced pressure, and filtered using a dialysis bag to obtain a product.
5. The method for preparing the two-component polymer-based self-leveling plugging material according to claim 4, Features: Adding a catalyst to the premixture obtained in step (1), wherein the catalyst is one of dibutyltin dilaurate, triethylamine, benzoyl peroxide, and 1,8-diazabicyclo[5.4.0]undec-7-ene, and the amount of the catalyst is 0.12 times the mass of the premixture; The method for uniform mixing in step (1) is ultrasonic water bath heating, wherein the power of the ultrasound is 100-200W, and the temperature of the water bath heating is 65-80°C.
6. The method for preparing the two-component polymer-based self-leveling plugging material according to claim 4, Features: The stirring and mixing method in step (2) is oil bath, wherein the temperature of the oil bath is 85-90° C., and the time of the oil bath is 1.5-3 h.
7. The method for preparing the two-component polymer-based self-leveling plugging material according to claim 4, Features: The modified cleaning solution in step (2) is prepared by mixing the components in proportion by weight, wherein the ratio of anhydrous ethanol: acetone: trichloromethane: (3-aminopropyl) trimethoxysilane is (20-40): (3-8): (5-10): (7-18).
8. The method for preparing the two-component polymer-based self-leveling plugging material according to claim 4, Features: The pressure parameter of the reduced pressure concentration in step (2) is 2-5 kPa, and the volume multiple of the reduced pressure concentration is 3-5 times; In step (2), the cut-off relative molecular mass of the dialysis bag is 8000-10000, and the filtration time is 2-4 days.
9. Use of the two-component polymer-based self-leveling plugging material according to any one of claims 1 to 3 in the preparation of fireproof components.