Preparation method of solar cell and solar cell
Laser electroplating technology is used to deposit local metal ions at the grid line slots of solar cells, which solves the problems of low deposition rate and poor aspect ratio in the copper electroplating process, and improves the conversion efficiency of the cell and the pull-off force of the electrode.
Patent Information
- Application Number
- CN202410862627.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-15
AI Technical Summary
When preparing solar cell electrodes in the prior art, the copper electroplating process results in a low metal copper deposition rate, low production efficiency, poor electrode aspect ratio, and insufficient pull-off force, which affects the battery conversion efficiency.
Laser plating technology is used to locally deposit metal ions at the grid grooves of the battery substrate. Laser irradiation is used to accelerate the deposition speed, limit the lateral growth of the electrode, improve the aspect ratio and density, and enhance the pull-off force.
The production efficiency and the contact performance and mechanical properties of the electrodes are improved, and the battery conversion efficiency is enhanced.
Smart Images

Figure CN118773702A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of photovoltaic technology, and in particular to a method for preparing a solar cell and a solar cell. Background Art
[0002] When preparing the electrodes of solar cells, the related technology uses the copper electroplating process to prepare electrodes on both sides of the battery substrate at the same time. However, the current density used for electroplating should not be too large, resulting in a low rate of metal copper deposition and low production efficiency. In addition, the electrodes prepared by the copper electroplating process grow laterally and have large grain sizes, resulting in poor electrode aspect ratio and poor electrode pull-off force. Summary of the invention
[0003] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes a method for preparing a solar cell and a solar cell, which can improve production efficiency, increase electrode pull-off force, and increase electrode aspect ratio, thereby improving cell conversion efficiency.
[0004] In a first aspect, the present application provides a method for preparing a solar cell, comprising:
[0005] forming a first gate line groove on a first side of the battery substrate;
[0006] The second side of the battery substrate is electrically connected to the cathode of the electroplating device, and the first side and the second side of the battery substrate are arranged opposite to each other;
[0007] A first electroplating solution is dripped onto a first side of the battery substrate, and the first electroplating solution is filled into the first gate line groove, and an anode of the electroplating device is immersed in the first electroplating solution;
[0008] The first gate line groove is irradiated with a first laser to form a first electrode on a first side of the battery substrate, and the first electrode is filled in the first gate line groove.
[0009] According to the preparation method of solar cells of the present application, by adopting laser electroplating electrodes, the local metal ion deposition rate can be accelerated, the production efficiency can be improved, and the laser irradiation area can be limited so that the laser can be accurately irradiated to the gate line groove, thereby limiting the lateral growth of the electrode, improving the electrode aspect ratio, and reducing light shielding, thereby improving the battery conversion efficiency. Laser irradiation can also improve the density of the electrode, thereby increasing the pull-off force of the electrode, and further improving the contact performance and mechanical properties of the electrode.
[0010] According to one embodiment of the present application, a plurality of the first grid line grooves are formed on the first side of the battery substrate;
[0011] The step of irradiating the first gate line groove with a first laser to form a first electrode on a first side of the battery substrate includes:
[0012] Splitting a single laser beam into a plurality of first laser beams corresponding to a plurality of the first gate line grooves respectively;
[0013] The first laser is used to irradiate the corresponding first gate line groove and scan back and forth along the length direction of the corresponding first gate line groove to form a first electrode on the first side of the battery substrate.
[0014] According to one embodiment of the present application, the current density of the first electroplating solution is 2A / dm 2 and / or,
[0015] The first laser meets at least one of the following characteristics: wavelength of 532nm; spot diameter of 6μm; irradiation power density of 800W / cm 2 ; Movement speed is 20000mm / s; Frequency is 100KHz; Irradiation time is 60s.
[0016] According to one embodiment of the present application, before dripping the first electroplating solution on the first side of the battery substrate, the method further includes:
[0017] A second electroplating solution is dripped onto the first side of the battery substrate, and the second electroplating solution is filled into the first gate line groove, and the anode of the electroplating device is immersed in the second electroplating solution;
[0018] irradiating the first gate line groove with a second laser to form a first seed layer at the bottom of the first gate line groove;
[0019] The second electroplating solution on the first side of the battery substrate is cleaned.
[0020] According to one embodiment of the present application, the current density of the second electroplating solution is 2A / dm 2 and / or,
[0021] The second laser meets at least one of the following characteristics: wavelength of 532nm; spot diameter of 6μm; irradiation power density of 500W / cm 2 ; Movement speed is 20000mm / s; Frequency is 100KHz; Irradiation time is 20s.
[0022] According to one embodiment of the present application, the method further includes:
[0023] forming a second gate line groove on a second side of the battery substrate;
[0024] electrically connecting the first side of the battery substrate to the cathode of the electroplating device;
[0025] A third electroplating solution is dripped onto the second side of the battery substrate, and the third electroplating solution is filled in the second gate line groove, and the anode of the electroplating device is immersed in the third electroplating solution;
[0026] The second gate line groove is irradiated with a third laser to form a second electrode on the second side of the battery substrate, and the second electrode is filled in the second gate line groove.
[0027] According to one embodiment of the present application, before dripping the third electroplating solution on the second side of the battery substrate, the method further includes:
[0028] A fourth electroplating solution is dripped onto the second side of the battery substrate, and the fourth electroplating solution is filled into the second gate line groove, and the anode of the electroplating device is immersed in the fourth electroplating solution;
[0029] irradiating the second gate line groove with a fourth laser to form a second seed layer at the bottom of the second gate line groove;
[0030] The fourth electroplating solution on the second side of the substrate is cleaned.
[0031] According to one embodiment of the present application, the method further includes:
[0032] The battery substrate having the first electrode and the second electrode is immersed in a chemical plating solution to form a first protective layer on a surface of the first electrode and a second protective layer on a surface of the second electrode.
[0033] According to one embodiment of the present application, the step of electrically connecting the second side of the battery substrate to the cathode of the electroplating device includes:
[0034] A conductive electrode electrically connected to the battery substrate is formed on the second side of the battery substrate, and the conductive electrode corresponds to the cathode position of the electroplating device;
[0035] The conductive electrode is placed in contact with the cathode.
[0036] In a second aspect, the present application provides a solar cell, which is prepared by the method for preparing a solar cell as described in the first aspect above.
[0037] The above one or more technical solutions in the embodiments of the present application have at least one of the following technical effects:
[0038] By using laser electroplating electrodes, the local metal ion deposition rate can be accelerated, the production efficiency can be improved, and the laser irradiation area can be limited so that the laser can be accurately irradiated to the gate line groove, limiting the lateral growth of the electrode, increasing the electrode aspect ratio, and reducing light shielding, thereby improving the battery conversion efficiency. Laser irradiation can also increase the density of the electrode, thereby increasing the electrode pull-off force, and further improving the contact performance and mechanical properties of the electrode.
[0039] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0041] Figure 1 This is one of the flow diagrams of the method for preparing a solar cell provided in an embodiment of the present application;
[0042] Figure 2 is a schematic structural diagram of an electroplating device in a method for preparing a solar cell provided in an embodiment of the present application;
[0043] Figure 3 is a schematic diagram of the structure of a solar cell provided in an embodiment of the present application;
[0044] Figure 4 This is the second schematic flow chart of the method for preparing a solar cell provided in an embodiment of the present application. DETAILED DESCRIPTION
[0045] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0046] The following describes a method for preparing a solar cell and a solar cell provided in an embodiment of the present application with reference to the accompanying drawings.
[0047] Figure 1 A schematic diagram of a process for preparing a solar cell provided in an embodiment of the present application, wherein the solar cell may be a TOPCON solar cell or other types of solar cells, which are not specifically limited here.
[0048] like Figure 1 As shown, the method for preparing a solar cell provided in the embodiment of the present application includes steps 110 to 140.
[0049] Step 110: forming a first gate line groove on a first side of a battery substrate.
[0050] First, a cell substrate is formed. The cell substrate is a solar cell without electrodes. In the case where the solar cell is a TOPCON solar cell, Figure 3 As shown, the battery substrate 1 may include a silicon substrate 11, a first passivation layer 12, a tunneling oxide layer 13, a polysilicon layer 14 and a second passivation layer 15. The size of the battery substrate 1 may be 210 mm×182 mm.
[0051] The silicon substrate 11 has a front side and a back side. The front side of the silicon substrate 11 is the light-receiving side of the solar cell (i.e., the side of the solar cell exposed to ultraviolet light). The back side of the silicon substrate 11 is the backlight side of the solar cell. The front side and the back side of the silicon substrate 11 are arranged opposite to each other. The first passivation layer 12 is located on the front side of the silicon substrate 11. The first passivation layer 12 may include at least one of aluminum oxide film, silicon nitride, silicon oxynitride, and silicon oxide. The tunneling oxide layer 13 is located on the back side of the silicon substrate 11. The tunneling oxide layer 13 may include silicon oxide, etc. The polysilicon layer 14 is located on the side of the tunneling oxide layer 13 away from the silicon substrate 11. The tunneling oxide layer 13 and the polysilicon layer 14 may constitute a tunneling oxide layer passivation contact (TOPCon) structure to achieve selective carrier transmission and have excellent passivation quality and contact performance. The second passivation layer 15 is located on the side of the polysilicon layer 14 away from the tunneling oxide layer 13. The second passivation layer 15 may include at least one of aluminum oxide film, silicon nitride, silicon oxynitride, and silicon oxide, etc.
[0052] The battery substrate 1 has a first side and a second side, and the first side and the second side of the battery substrate 1 are arranged opposite to each other. One of the first side and the second side of the battery substrate 1 is the side of the battery substrate 1 close to the first passivation layer 12, and the other side is the side of the battery substrate 1 close to the second passivation layer 15, that is, the first side of the battery substrate 1 is the side of the battery substrate 1 close to the first passivation layer 12, and the second side of the battery substrate 1 is the side of the battery substrate 1 close to the second passivation layer 15; or, the second side of the battery substrate 1 is the side of the battery substrate 1 close to the first passivation layer 15, and the first side of the battery substrate 1 is the side of the battery substrate 1 close to the second passivation layer 15.
[0053] A first gate line groove is formed on the first side of the battery substrate 1. The first gate line groove is used for electrically connecting the first electrode formed subsequently with the battery substrate. The first gate line groove penetrates the first passivation layer or the second passivation layer along the thickness direction of the battery substrate.
[0054] When forming the first gate line groove, a laser may be used to irradiate the first side of the battery substrate according to the pre-designed first electrode pattern, so as to etch the first gate line groove on the first side of the battery substrate.
[0055] For example, the first side of the battery substrate is a side of the battery substrate close to the first passivation layer. An ultraviolet picosecond laser (wavelength of 355 nm) is used to irradiate the first side of the battery substrate with laser to etch the first passivation layer to form a first gate line groove penetrating the first passivation layer, wherein the first gate line groove exposes the silicon substrate. The width of the first gate line groove may be 10 μm.
[0056] Step 120: electrically connect the second side of the battery substrate to the cathode of the electroplating device, and the first side and the second side of the battery substrate are arranged opposite to each other.
[0057] Combination Figure 2 As shown, the electroplating device may include a cathode 10, and the cathode 10 may include two cathode contacts or two cathode rollers arranged in parallel. During the electrode preparation process, the battery substrate 1 may be located on the cathode 10, and the second side of the battery substrate 1 is arranged toward the cathode 10, so that the battery substrate 1 is electrically connected to the cathode 10. In the case where the cathode 10 includes a cathode roller, the cathode roller may roll along the transmission direction of the battery substrate, so that the battery substrate can prepare the electrode while being transported.
[0058] There are many ways to electrically connect the battery substrate 1 and the cathode 10 .
[0059] In some embodiments, after forming the first gate line groove on the first side of the battery substrate, a groove penetrating the passivation layer may be formed on the second side of the battery substrate, and the position of the groove corresponds to the position of the cathode 10. After the battery substrate is placed on the cathode 10, the cathode 10 is electrically connected to the battery substrate through the groove on the second side of the battery substrate.
[0060] In some embodiments, the step 120 of electrically connecting the second side of the battery substrate to the cathode of the electroplating device includes:
[0061] Forming a conductive electrode electrically connected to the battery substrate on the second side of the battery substrate, wherein the conductive electrode corresponds to the cathode position of the electroplating device;
[0062] A conductive electrode is placed in contact with the cathode.
[0063] A conductive electrode is formed on the second side of the battery substrate, and the conductive electrode penetrates the passivation layer on the second side of the battery substrate along the thickness direction of the battery substrate to be electrically connected to the battery substrate. Moreover, the conductive electrode corresponds to the position of the cathode 10, so that when the battery substrate is located on the cathode 10, the conductive electrode on the second side of the battery substrate contacts the cathode 10, so that the battery substrate is electrically connected to the cathode 10 through the conductive electrode.
[0064] For example, the second side of the battery substrate is the side of the battery substrate close to the second passivation layer. A screen printing process is used to form a conductive electrode on the side of the second passivation layer away from the silicon substrate, and the conductive electrode penetrates the second passivation layer along the thickness direction to connect with the polysilicon layer, thereby achieving electrical connection between the conductive electrode and the battery substrate. The conductive electrode can also be used as a partial electrode on the second side of the battery substrate.
[0065] It should be noted that, when the cathode 10 includes a cathode roller, the conductive electrode may extend along the transport direction of the battery substrate and penetrate the battery substrate, so that the battery substrate maintains electrical connection with the cathode 10 when being transported on the cathode 10 .
[0066] In this embodiment, a conductive electrode is disposed on the second side of the battery substrate, so that the battery substrate is electrically connected to the cathode 10 through the conductive electrode, thereby improving the conduction effect between the battery substrate and the cathode 10 .
[0067] In some embodiments, before electrically connecting the second side of the cell substrate to the cathode of the electroplating device in step 120, the method for preparing a solar cell may further include:
[0068] The battery substrate is pretreated to remove impurities on the surface of the battery substrate and the passivation layer is hydrophilic.
[0069] Step 130 : dripping a first electroplating solution onto a first side of the battery substrate, filling the first gate line groove with the first electroplating solution, and immersing an anode of an electroplating device into the first electroplating solution.
[0070] Combination Figure 2 As shown, when the battery substrate 1 is located on the cathode 10, the second side of the battery substrate 1 is arranged toward the cathode 10 (i.e., the second side of the battery substrate 1 faces downward), and the first side of the battery substrate 1 is arranged away from the cathode 10 (i.e., the first side of the battery substrate 1 faces upward). The first electroplating solution 40 is dripped onto the first side of the battery substrate 1 to ensure that the first electroplating solution 40 covers the first side of the battery substrate 1 and fills the first grid line groove, but does not overflow the first side of the battery substrate 1. The first electroplating solution 40 contains metal ions that form the first electrode, such as copper ions.
[0071] Combination Figure 2 As shown, the electroplating device further includes an anode 20, which is located above the cathode 10. After the battery substrate 1 is located on the cathode 10, the battery substrate 1 is located between the cathode 10 and the anode 20. The anode 20 includes two anode contacts, and after the first side of the battery substrate 1 is dripped with the first electroplating solution, the two anode contacts of the anode 20 are immersed in the first electroplating solution.
[0072] Step 140: Use a first laser to irradiate the first gate line groove to form a first electrode on the first side of the battery substrate, and the first electrode fills the first gate line groove.
[0073] Combination Figure 2 and Figure 3 As shown, the electroplating device may further include a laser 30, which is located above the anode 20. The first laser emitted by the laser 30 accurately irradiates the area where the first grid line groove is located, and the spot diameter of the first laser does not exceed the width of the first grid line groove. The metal ions in the first electroplating solution 40 are quickly deposited in the first laser irradiation area (i.e., the area where the first grid line groove is located) to form a first electrode 21 at the first grid line groove. The first electrode 21 is located on the first side of the battery substrate 1 and filled in the first grid line groove. The first electrode 21 may include a copper electrode, etc.
[0074] For example, the first side of the battery substrate is the side of the battery substrate close to the first passivation layer. The current density of the first electroplating solution can be 2A / dm 2 The first laser meets at least one of the following characteristics: the wavelength is 532nm, the laser emitting the first laser is a green picosecond laser; the spot diameter is 6μm; the irradiation power density is 800W / cm 2 ; The movement speed is 20000 mm / s; The frequency is 100 KHz; The irradiation time is 60 seconds, that is, the electroplating time is 60 seconds. The thickness of the first electrode is 13 μm, and the width of the first electrode does not exceed 16 μm.
[0075] After forming the first electrode, the first electroplating solution dripped on the first side of the battery substrate may be cleaned and rinsed clean for subsequent processes.
[0076] The metallization of solar cells affects the cost and conversion efficiency of the cells, and ultimately affects the choice of cell path. Cell metallization is one of the important links in the production of solar cells. Through contact and non-contact technologies, metallized electrodes are prepared on the front and back of solar cells to form a tight and efficient ohmic contact between the electrodes and the cells, and to guide the photogenerated carriers out of the cells. Metallization is related to the production cost and conversion efficiency of the cells, and ultimately affects the choice of future cell paths. Therefore, the optimization of the metallization process has not only become a key area for various battery manufacturers to achieve their cost reduction plans, but also a focus of the industry.
[0077] As a non-contact metallization technology, the electroplating copper process is the most effective attempt to break through the screen printing technology. The biggest advantage of the electroplating copper process is that copper replaces all metal silver pastes, which fundamentally solves the problem of high material costs. At the same time, copper electroplating can achieve double-sided metallization at the same time, improving production efficiency. However, due to the requirements of the bonding strength of the copper plating layer and the seed layer, the current density used for electroplating should not be too large, resulting in low metallization capacity, thereby weakening the feasibility of large-scale mass production of electroplated copper. Moreover, the electroplating copper process needs to be matched with a graphical front-end process. The graphical process uses a mask with a certain thickness as a barrier to constrain the morphology of the electroplated copper metal electrode and increase the aspect ratio of the gate line, but the cost of the thick mask is relatively high, and the related subsequent processing is also relatively complicated.
[0078] Based on this, the present embodiment adopts laser electroplating of the first electrode, which can accelerate the metal ion deposition speed at the first gate line groove, improve the preparation efficiency of the first electrode, and thus improve the production efficiency; limit the spot diameter of the first laser, so that the first laser can be accurately irradiated to the first gate line groove, limit the lateral growth of the first electrode, and improve the aspect ratio of the first electrode on the basis of the patterning of the thin mask, reduce light shielding, and thus improve the battery conversion efficiency; laser irradiation can refine the grain size of the first electrode, improve the density of the first electrode, and improve the pull-off force of the first electrode, thereby improving the contact performance and mechanical properties of the first electrode.
[0079] In some embodiments, when a plurality of first electrodes need to be prepared on the first side of the battery substrate, a plurality of first gateline grooves may be formed on the first side of the battery substrate in step 110. The step 140 of irradiating the first gateline grooves with a first laser to form the first electrode on the first side of the battery substrate includes:
[0080] Splitting a single laser beam into a plurality of first laser beams corresponding to the plurality of first grid line grooves respectively;
[0081] A first laser is used to irradiate the corresponding first gate line groove and scan back and forth along the length direction of the corresponding first gate line groove to form a first electrode on the first side of the battery substrate.
[0082] The laser emitted by the laser is a single laser beam, and a beam splitter is used to split the single laser beam into multiple first laser beams, and the multiple first laser beams can be arranged in one-to-one correspondence with the multiple first grid line grooves.
[0083] Multiple beams of first laser light are irradiated to multiple first grid line grooves one by one, and the spot diameter of each beam of first laser light does not exceed the width of the corresponding first grid line groove. Each beam of first laser light scans back and forth along the length direction of the corresponding first grid line groove, so that the metal ions in the first electroplating solution are quickly deposited at each first grid line groove, thereby forming a first electrode at each first grid line groove.
[0084] In this embodiment, multiple beams of first laser light are used to irradiate multiple first gate line grooves correspondingly, so as to form first electrodes at the multiple first gate line grooves simultaneously, thereby further improving the preparation efficiency of the first electrodes.
[0085] In some embodiments, before dripping the first electroplating solution on the first side of the cell substrate in step 130, the method for preparing a solar cell further includes:
[0086] The second electroplating solution is dripped onto the first side of the battery substrate, and the second electroplating solution is filled into the first grid line groove, and the anode of the electroplating device is immersed in the second electroplating solution;
[0087] irradiating the first gate line groove with a second laser to form a first seed layer at the bottom of the first gate line groove;
[0088] The second electroplating solution on the first side of the cell substrate is cleaned.
[0089] After the second side of the battery substrate is electrically connected to the cathode 10 of the electroplating device, the second electroplating solution can be firstly dripped onto the first side of the battery substrate 1 to ensure that the second electroplating solution covers the first side of the battery substrate 1 and fills the first grid line groove, but does not overflow the first side of the battery substrate 1. The second electroplating solution contains metal ions, such as nickel ions, that form the first seed layer.
[0090] After the first side of the battery substrate 1 is dripped with the second electroplating solution, the anode 20 is immersed in the second electroplating solution. The second laser emitted by the laser 30 accurately irradiates the area where the first grid line groove is located, and the spot diameter of the second laser does not exceed the width of the first grid line groove. Figure 3 As shown, metal ions in the second electroplating solution are rapidly deposited in the second laser irradiation area (ie, the area where the first gate line groove is located) to form a dense first seed layer 22 at the bottom of the first gate line groove. The first seed layer 22 may include a nickel seed layer or the like.
[0091] For example, the first side of the battery substrate is the side of the battery substrate close to the first passivation layer. The current density of the second electroplating solution can be 2A / dm 2 The second laser meets at least one of the following characteristics: the wavelength is 532nm, the laser emitting the second laser is a green picosecond laser; the spot diameter is 6μm; the irradiation power density is 500W / cm 2 ; Movement speed is 20000mm / s; Frequency is 100KHz; Irradiation time is 20s, that is, electroplating time is 20s.
[0092] After forming the first seed layer, the second electroplating solution dripped on the first side of the battery substrate can be cleaned and rinsed clean to facilitate the subsequent process of preparing the first electrode.
[0093] In this embodiment, the first seed layer 22 is first formed at the bottom of the first gate line groove, and then the first electrode 21 is formed, which can improve the conductivity of the first electrode 21 and prevent copper in the first electrode 21 from diffusing into the silicon substrate 11, further increasing the pull-off force of the first electrode 21.
[0094] In some embodiments, when a plurality of first grid line grooves are formed on the first side of the battery substrate, a beam splitter is used to split a single laser beam emitted by the laser into a plurality of second laser beams, and the plurality of second laser beams can be arranged in one-to-one correspondence with the plurality of first grid line grooves. The plurality of second laser beams are irradiated to the plurality of first grid line grooves in one-to-one correspondence, and the spot diameter of each second laser beam does not exceed the width of the corresponding first grid line groove. Each second laser beam scans back and forth along the length direction of the corresponding first grid line groove, so that the metal ions in the second electroplating solution are quickly deposited at each first grid line groove, thereby forming a first seed layer at the bottom of each first grid line groove.
[0095] In this embodiment, multiple beams of second laser light are used to irradiate multiple first gate line grooves correspondingly, so as to form the first seed layer at the multiple first gate line grooves at the same time, thereby improving the preparation efficiency of the first seed layer.
[0096] In some embodiments, the method for preparing a solar cell further includes:
[0097] forming a second grid line groove on a second side of the battery substrate;
[0098] electrically connecting the first side of the battery substrate to a cathode of an electroplating device;
[0099] The third electroplating solution is dripped onto the second side of the battery substrate, and the third electroplating solution is filled into the second grid line groove, and the anode of the electroplating device is immersed in the third electroplating solution;
[0100] The second gate line groove is irradiated with a third laser to form a second electrode on the second side of the battery substrate, and the second electrode is filled in the second gate line groove.
[0101] After forming the first electrode on the first side of the battery substrate, the second electrode can be formed on the second side of the battery substrate. In the process of preparing the second electrode, a second grid line groove is first formed on the second side of the battery substrate. The second grid line groove is used for electrically connecting the second electrode formed subsequently to the battery substrate. The second grid line groove penetrates the first passivation layer or the second passivation layer along the thickness direction of the battery substrate.
[0102] When forming the second gate line groove, the second side of the battery substrate may be irradiated with laser by a laser according to the pre-designed second electrode pattern, so as to etch the second gate line groove on the second side of the battery substrate.
[0103] For example, the second side of the battery substrate is a side of the battery substrate close to the second passivation layer. An ultraviolet picosecond laser (wavelength of 355 nm) is used to irradiate the second side of the battery substrate with laser to etch the second passivation layer to form a second gate line groove penetrating the second passivation layer, wherein the second gate line groove exposes the polysilicon layer. The width of the second gate line groove may be 40 μm.
[0104] In some embodiments, the step of forming a second gate line groove may be performed before step 120. For example, a first gate line groove may be formed on the first side of the battery substrate, and then a second gate line groove may be formed on the second side of the battery substrate. The second side of the battery substrate is then electrically connected to the cathode of the electroplating device.
[0105] After forming the second gate line groove, the battery substrate 1 having the first electrode 21 (and the first seed layer 22) can be placed on the cathode 10, with the first side of the battery substrate 1 facing the cathode 10 (i.e., the first side of the battery substrate 1 faces downward), and the first electrode 21 on the first side of the battery substrate 1 contacts the cathode 10, thereby realizing electrical connection between the battery substrate 1 and the cathode 10.
[0106] The second side of the battery substrate 1 is arranged away from the cathode 10 (i.e., the second side of the battery substrate 1 faces upward). The third electroplating solution is dripped onto the second side of the battery substrate 1 to ensure that the third electroplating solution covers the second side of the battery substrate 1 and fills the second grid line groove, but does not overflow the second side of the battery substrate 1. The third electroplating solution contains metal ions, such as copper ions, that form the second electrode. After the third electroplating solution is dripped onto the second side of the battery substrate 1, the anode 20 is immersed in the third electroplating solution.
[0107] The third laser emitted by the laser 30 accurately irradiates the area where the second grid line groove is located, and the spot diameter of the third laser does not exceed the width of the second grid line groove. Figure 3 As shown, the metal ions in the third electroplating solution are quickly deposited in the third laser irradiation area (i.e., the area where the second gate line groove is located) to form a second electrode 31 at the second gate line groove. The second electrode 31 is located on the second side of the battery substrate 1 and filled in the second gate line groove. The second electrode 31 may include a copper electrode, etc.
[0108] For example, the second side of the battery substrate is the side of the battery substrate close to the second passivation layer. The current density of the third electroplating solution can be 2A / dm 2 The third laser meets at least one of the following characteristics: the wavelength is 532nm, the laser emitting the third laser is a green picosecond laser; the spot diameter is 30μm (the third laser may also include multiple beams, and the spot diameter of each beam is 6μm); the irradiation power density is 800W / cm 2; The movement speed is 20000 mm / s; The frequency is 100 KHz; The irradiation time is 60 seconds, that is, the electroplating time is 60 seconds. The thickness of the second electrode is 13 μm, and the width of the second electrode does not exceed 45 μm.
[0109] After forming the second electrode, the third electroplating solution dripped on the second side of the battery substrate may be cleaned and rinsed clean for subsequent processes.
[0110] This embodiment uses laser electroplating for the second electrode, which can speed up the metal ion deposition rate at the second gate line groove, improve the preparation efficiency of the second electrode, and thus improve the production efficiency; limit the spot diameter of the third laser so that the third laser can be accurately irradiated to the second gate line groove, limit the lateral growth of the second electrode, increase the aspect ratio of the second electrode, reduce light shielding, and thus improve the battery conversion efficiency; laser irradiation can refine the grain size of the second electrode and increase the pull-off force of the second electrode.
[0111] In some embodiments, when a plurality of second electrodes need to be prepared on the second side of the battery substrate, a plurality of second gate line grooves can be first formed on the second side of the battery substrate. A beam splitter is used to split a single laser beam emitted by the laser into a plurality of third laser beams, and each second gate line groove is arranged corresponding to at least one third laser beam.
[0112] Each third laser beam is irradiated to the corresponding second grid line groove, and the spot diameter of the laser beam irradiated to each second grid line groove does not exceed the width of the second grid line groove. Each third laser beam is scanned back and forth along the length direction of the corresponding second grid line groove, so that the metal ions in the third electroplating solution are quickly deposited at each second grid line groove, thereby forming a second electrode at each second grid line groove.
[0113] In this embodiment, multiple beams of third laser light are used to irradiate multiple second gate line grooves correspondingly, so as to simultaneously form second electrodes at multiple second gate line grooves, thereby further improving the preparation efficiency of the second electrodes.
[0114] In some embodiments, before dripping the third electroplating solution on the second side of the cell substrate, the method for preparing a solar cell further includes:
[0115] The fourth electroplating solution is dripped onto the second side of the battery substrate, and the fourth electroplating solution is filled into the second grid line groove, and the anode of the electroplating device is immersed in the fourth electroplating solution;
[0116] irradiating the second gate line groove with a fourth laser to form a second seed layer at the bottom of the second gate line groove;
[0117] The fourth electroplating solution is cleaned from the second side of the substrate.
[0118] After the first side of the battery substrate is electrically connected to the cathode 10 of the electroplating device, the fourth electroplating solution can be firstly dripped onto the second side of the battery substrate 1 to ensure that the fourth electroplating solution covers the second side of the battery substrate 1 and fills the second gate line groove, but does not overflow the second side of the battery substrate 1. The fourth electroplating solution contains metal ions, such as nickel ions, that form the second seed layer.
[0119] After the fourth electroplating solution is dripped onto the second side of the battery substrate 1, the anode 20 is immersed in the fourth electroplating solution. The fourth laser emitted by the laser 30 is precisely irradiated on the area where the second grid line groove is located, and the spot diameter of the fourth laser does not exceed the width of the second grid line groove. Figure 3 As shown, metal ions in the fourth electroplating solution are rapidly deposited in the fourth laser irradiation area (ie, the area where the second gate line groove is located) to form a dense second seed layer 32 at the bottom of the second gate line groove. The second seed layer 32 may include a nickel seed layer or the like.
[0120] For example, the second side of the battery substrate is the side of the battery substrate close to the second passivation layer. The current density of the fourth electroplating solution may be 2A / dm 2 The fourth laser meets at least one of the following characteristics: the wavelength is 532nm, the laser emitting the fourth laser is a green picosecond laser; the spot diameter is 30μm (the fourth laser may also include multiple beams, and the spot diameter of each beam is 6μm); the irradiation power density is 500W / cm 2 ; Movement speed is 20000mm / s; Frequency is 100KHz; Irradiation time is 20s, that is, electroplating time is 20s.
[0121] After the second seed layer is formed, the fourth electroplating solution dripped on the second side of the battery substrate may be cleaned and rinsed clean to facilitate the subsequent process of preparing the second electrode.
[0122] In this embodiment, a second seed layer is first formed at the bottom of the second gate line groove, and then a second electrode is formed, which can improve the conductivity of the second electrode and prevent copper in the second electrode from diffusing into the silicon substrate, thereby further increasing the pull-off force of the second electrode.
[0123] In some embodiments, when a plurality of second grid line grooves are formed on the second side of the battery substrate, a beam splitter is used to split a single laser beam emitted by the laser into a plurality of fourth laser beams, and each second grid line groove is provided corresponding to at least one fourth laser beam. The plurality of fourth laser beams are irradiated to the plurality of second grid line grooves correspondingly, and the spot diameter of the laser beam irradiated to each second grid line groove does not exceed the width of the second grid line groove. Each fourth laser beam scans back and forth along the length direction of the corresponding second grid line groove, so that the metal ions in the fourth electroplating solution are quickly deposited at each second grid line groove, thereby forming a second seed layer at the bottom of each second grid line groove.
[0124] In this embodiment, multiple beams of fourth laser light are used to irradiate multiple second gate line grooves correspondingly, so as to simultaneously form the second seed layer at the multiple second gate line grooves, thereby improving the preparation efficiency of the second seed layer.
[0125] In some embodiments, the method for preparing a solar cell further includes:
[0126] The battery substrate having the first electrode and the second electrode is immersed in a chemical plating solution to form a first protective layer on the surface of the first electrode and a second protective layer on the surface of the second electrode.
[0127] Combination Figure 3 As shown, after preparing the first electrode 21 on the first side of the battery substrate 1 and preparing the second electrode 31 on the second side of the battery substrate 1, the battery substrate 1 having the first electrode 21 and the second electrode 31 can be immersed in a chemical plating solution for a period of time to deposit a first protective layer 23 on the surface of the first electrode 21 and a second protective layer 33 on the surface of the second electrode 31.
[0128] The chemical plating solution may be a silver plating solution, the duration may be 30 seconds, the thickness of the first protective layer 23 and the second protective layer 33 may both be about 1 μm, and the first protective layer 23 and the second protective layer 33 may both include silver or the like.
[0129] After the first protective layer 23 and the second protective layer 33 are formed, the cell substrate is taken out and dried to obtain a solar cell.
[0130] like Figure 4 As shown, the embodiment of the present application also provides a method for preparing a solar cell, including steps 211 to 228.
[0131] Step 211 : forming a first gate line groove on a first side of a battery substrate, and forming a second gate line groove on a second side of the battery substrate.
[0132] Step 212: forming a conductive electrode electrically connected to the battery substrate on the second side of the battery substrate, wherein the conductive electrode corresponds to the position of the cathode of the electroplating device.
[0133] Step 213: pre-treat the battery substrate.
[0134] Step 214: Place the battery substrate on the cathode of the electroplating device so that the conductive electrode contacts the cathode of the electroplating device.
[0135] Step 215 , dripping the second electroplating solution onto the first side of the battery substrate, ensuring that the second electroplating solution covers the first side of the battery substrate but does not overflow, and immersing the anode of the electroplating device in the second electroplating solution.
[0136] Step 216 , using a second laser to irradiate the first gate line groove, and the second laser scans back and forth along the length direction of the first gate line groove to form a first seed layer at the bottom of the first gate line groove.
[0137] Step 217: Rinse the second electroplating solution on the first side of the battery substrate.
[0138] Step 218: drip the first electroplating solution onto the first side of the battery substrate, ensure that the first electroplating solution covers the first side of the battery substrate but does not overflow, and immerse the anode of the electroplating device in the first electroplating solution.
[0139] Step 219: irradiate the first gate line groove with a first laser, and scan the first laser back and forth along the length direction of the first gate line groove to form a first electrode on the first side of the battery substrate, and the first electrode fills the first gate line groove.
[0140] Step 220: Rinse the first electroplating solution on the first side of the battery substrate.
[0141] Step 221, place the battery substrate back on the cathode of the electroplating device so that the first electrode is in contact with the cathode of the electroplating device.
[0142] Step 222: drip the fourth electroplating solution onto the second side of the battery substrate, ensure that the fourth electroplating solution covers the second side of the battery substrate but does not overflow, and immerse the anode of the electroplating device in the fourth electroplating solution.
[0143] Step 223 , using a fourth laser to irradiate the second gate line groove, and the fourth laser scans back and forth along the length direction of the second gate line groove to form a second seed layer at the bottom of the second gate line groove.
[0144] Step 224: Rinse the fourth electroplating solution on the second side of the battery substrate.
[0145] Step 225 , dripping the third electroplating solution onto the second side of the battery substrate, ensuring that the third electroplating solution covers the second side of the battery substrate but does not overflow, and immersing the anode of the electroplating device into the third electroplating solution.
[0146] Step 226: Use a third laser to irradiate the second gate line groove, and the third laser scans back and forth along the length direction of the second gate line groove to form a second electrode on the second side of the battery substrate, and the second electrode fills the second gate line groove.
[0147] Step 227: Rinse the third electroplating solution on the second side of the battery substrate.
[0148] Step 228: Immerse the battery substrate in a chemical plating solution to form a first protective layer on the surface of the first electrode and a second protective layer on the surface of the second electrode.
[0149] According to the method for preparing solar cells provided in the embodiments of the present application, by adopting laser electroplating electrodes, the local metal ion deposition rate can be accelerated, the production efficiency can be improved, and the laser irradiation area can be limited so that the laser can be accurately irradiated to the gate line groove, thereby limiting the lateral growth of the electrode, improving the electrode aspect ratio, and reducing light shielding, thereby improving the battery conversion efficiency. In addition, laser irradiation can increase the density of the electrode, thereby increasing the pull-off force of the electrode, and further improving the contact performance and mechanical properties of the electrode.
[0150] Correspondingly, an embodiment of the present application also provides a solar cell.
[0151] The solar cell is prepared by using the method for preparing the solar cell in the above embodiment.
[0152] like Figure 3 As shown, the battery substrate 1 may include a silicon substrate 11, a first passivation layer 12, a tunneling oxide layer 13, a polysilicon layer 14 and a second passivation layer 15. The silicon substrate 11 has a front side and a back side, and the front side of the silicon substrate 11 is the light-receiving side of the solar cell (i.e., the side of the solar cell exposed to ultraviolet light). The back side of the silicon substrate 11 is the backlight side of the solar cell, and the front side and the back side of the silicon substrate 11 are arranged opposite to each other. The first passivation layer 12 is located on the front side of the silicon substrate 11, and the first passivation layer 12 may include at least one of aluminum oxide film, silicon nitride, silicon oxynitride and silicon oxide. The tunneling oxide layer 13 is located on the back side of the silicon substrate 11, and the tunneling oxide layer 13 may include silicon oxide. The polysilicon layer 14 is located on the side of the tunneling oxide layer 13 away from the silicon substrate 11. The tunneling oxide layer 13 and the polysilicon layer 14 may form a tunneling oxide layer passivation contact (TOPCon) structure to achieve selective carrier transmission, and have excellent passivation quality and contact performance. The second passivation layer 15 is located on a side of the polysilicon layer 14 away from the tunnel oxide layer 13 . The second passivation layer 15 may include at least one of aluminum oxide film, silicon nitride, silicon oxynitride, silicon oxide, and the like.
[0153] The battery substrate 1 has a first side and a second side, and the first side and the second side of the battery substrate 1 are arranged opposite to each other. One of the first side and the second side of the battery substrate 1 is a side of the battery substrate 1 close to the first passivation layer 12, and the other side is a side of the battery substrate 1 close to the second passivation layer 15.
[0154] The electrodes include a first electrode 21 and a second electrode 31. The first electrode 21 is located on a first side of the battery substrate 1 and is electrically connected to the battery substrate 1. The second electrode 31 is located on a second side of the battery substrate 1 and is electrically connected to the battery substrate 1.
[0155] For example, the first side of the battery substrate 1 is the side of the battery substrate 1 close to the first passivation layer 12, and the second side of the battery substrate 1 is the side of the battery substrate 1 close to the second passivation layer 15. The first electrode 21 is located on the side of the first passivation layer 12 away from the silicon substrate 11, and penetrates the first passivation layer 12 to connect with the silicon substrate 11. The second electrode 31 is located on the side of the second passivation layer 15 away from the silicon substrate 11, and penetrates the second passivation layer 15 to connect with the polysilicon layer 14.
[0156] In some embodiments, the solar cell may further include a first seed layer 22 and a second seed layer 32 , wherein the first seed layer 22 is located between the first electrode 21 and the silicon substrate 11 , and the second seed layer 32 is located between the second electrode 31 and the polysilicon layer 14 .
[0157] In some embodiments, the solar cell may further include a first protective layer 23 and a second protective layer 33 , wherein the first protective layer 23 covers the first electrode 21 , and the second protective layer 33 covers the second electrode 31 .
[0158] According to the solar cell provided in the embodiment of the present application, by adopting laser electroplating electrodes, the local metal ion deposition rate can be accelerated, the production efficiency can be improved, and the laser irradiation area can be limited so that the laser can be accurately irradiated to the gate line groove, thereby limiting the lateral growth of the electrode, improving the electrode aspect ratio, and reducing light shielding, thereby improving the battery conversion efficiency. Laser irradiation can also increase the density of the electrode, thereby increasing the pull-off force of the electrode, and further improving the contact performance and mechanical properties of the electrode.
[0159] Correspondingly, an embodiment of the present application further provides a photovoltaic assembly, comprising the solar cell in the above embodiment.
[0160] The photovoltaic module of the present application includes the solar cell provided by the present application, and thus has at least the same advantages as the above-mentioned solar cell.
[0161] Correspondingly, an embodiment of the present application also provides an electrical device, including the above-mentioned photovoltaic component.
[0162] The electrical device of the present application includes the photovoltaic module provided by the present application, and thus has at least the same advantages as the above-mentioned photovoltaic module.
[0163] The terms "first", "second", etc. in the specification and claims of this application are used to distinguish similar objects, and are not used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable under appropriate circumstances, so that the embodiments of the present application can be implemented in an order other than those illustrated or described herein, and the objects distinguished by "first", "second", etc. are generally of the same type, and the number of objects is not limited. For example, the first object can be one or more.
[0164] In the description of the present application, “plurality” means two or more.
[0165] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0166] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A method for preparing a solar cell, characterized in that: include: forming a first gate line groove on a first side of the battery substrate; The second side of the battery substrate is electrically connected to the cathode of the electroplating device, and the first side and the second side of the battery substrate are arranged opposite to each other; A first electroplating solution is dripped onto a first side of the battery substrate, and the first electroplating solution is filled into the first gate line groove, and an anode of the electroplating device is immersed in the first electroplating solution; The first gate line groove is irradiated with a first laser to form a first electrode on a first side of the battery substrate, and the first electrode is filled in the first gate line groove.
2. The method for preparing a solar cell according to claim 1, characterized in that: A plurality of first gate line grooves are formed on the first side of the battery substrate; The step of irradiating the first gate line groove with a first laser to form a first electrode on a first side of the battery substrate includes: Splitting a single laser beam into a plurality of first laser beams corresponding to a plurality of the first gate line grooves respectively; The first laser is used to irradiate the corresponding first gate line groove and scan back and forth along the length direction of the corresponding first gate line groove to form a first electrode on the first side of the battery substrate.
3. The method for preparing a solar cell according to claim 1, characterized in that: The current density of the first electroplating solution is 2A / dm 2 and / or, The first laser meets at least one of the following characteristics: wavelength of 532nm; spot diameter of 6μm; irradiation power density of 800W / cm 2 ; Movement speed is 20000mm / s; Frequency is 100KHz; Irradiation time is 60s.
4. The method for preparing a solar cell according to claim 1, characterized in that: Before dripping the first electroplating solution on the first side of the battery substrate, the method further includes: A second electroplating solution is dripped onto the first side of the battery substrate, and the second electroplating solution is filled into the first gate line groove, and the anode of the electroplating device is immersed in the second electroplating solution; irradiating the first gate line groove with a second laser to form a first seed layer at the bottom of the first gate line groove; The second electroplating solution on the first side of the battery substrate is cleaned.
5. The method for preparing a solar cell according to claim 4, characterized in that: The current density of the second electroplating solution is 2A / dm 2 and / or, The second laser meets at least one of the following characteristics: wavelength of 532nm; spot diameter of 6μm; irradiation power density of 500W / cm 2 ; Movement speed is 20000mm / s; Frequency is 100KHz; Irradiation time is 20s.
6. The method for preparing a solar cell according to claim 1, characterized in that: The method further comprises: forming a second gate line groove on a second side of the battery substrate; electrically connecting the first side of the battery substrate to the cathode of the electroplating device; A third electroplating solution is dripped onto the second side of the battery substrate, and the third electroplating solution is filled in the second gate line groove, and the anode of the electroplating device is immersed in the third electroplating solution; The second gate line groove is irradiated with a third laser to form a second electrode on the second side of the battery substrate, and the second electrode is filled in the second gate line groove.
7. The method for preparing a solar cell according to claim 6, characterized in that: Before dripping the third electroplating solution on the second side of the battery substrate, the method further includes: A fourth electroplating solution is dripped onto the second side of the battery substrate, and the fourth electroplating solution is filled into the second gate line groove, and the anode of the electroplating device is immersed in the fourth electroplating solution; irradiating the second gate line groove with a fourth laser to form a second seed layer at the bottom of the second gate line groove; The fourth electroplating solution on the second side of the substrate is cleaned.
8. The method for preparing a solar cell according to claim 6, characterized in that: The method further comprises: The battery substrate having the first electrode and the second electrode is immersed in a chemical plating solution to form a first protective layer on a surface of the first electrode and a second protective layer on a surface of the second electrode.
9. The method for preparing a solar cell according to claim 1, characterized in that: The step of electrically connecting the second side of the battery substrate to the cathode of the electroplating device comprises: A conductive electrode electrically connected to the battery substrate is formed on the second side of the battery substrate, and the conductive electrode corresponds to the cathode position of the electroplating device; The conductive electrode is placed in contact with the cathode.
10. A solar cell, characterized in that: The solar cell is prepared by the method for preparing the solar cell according to any one of claims 1 to 9.