Water-based medium-stripping non-silicon release agent, preparation method thereof and release film
Through the preparation of water-based medium-stripping non-silicon release agents, materials such as sodium dodecyl sulfonate and a persulfate initiator system are used to form an acrylate copolymer, which solves the problem of silicon in existing non-silicon release agents in electronic products. Fluorine sensitivity and environmental protection issues, achieving stable medium peeling effect and low-cost processing.
Patent Information
- Application Number
- CN202410828813.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-18
AI Technical Summary
Existing non-silicon release agents have problems with silicone and fluorine element sensitivity in the processing of electronic products. Solvent-based release agents have environmental and health hazards, and produce VOC and a large amount of organic solvents during the preparation process, polluting the environment and causing high costs.
Using a water-based medium-stripping non-silicon release agent, through the combination of sodium dodecyl sulfonate, polyoxyethylene octylphenol ether-10, lauryl methacrylate, hydroxyethyl methacrylate, initiator and curing agent, Combining the persulfate initiating system and the core-shell structure emulsion polymerization method, an acrylate binary copolymer is formed to achieve high-temperature coating film curing.
We provide an environmentally friendly, low-VOC non-silicon release film with stable mid-peeling effect, suitable for tape processing, reducing the aging creep rate and residual splicing rate, making it more cost-effective.
Smart Images

Figure BDA0004911245880000141
Abstract
Description
Technical Field
[0001] The invention relates to the field of release materials, and in particular to an aqueous medium-peeling non-silicon release agent, a preparation method thereof and a release film. Background Art
[0002] Release agent is a low-adhesion auxiliary coating used to protect pressure-sensitive adhesives. The special molecular structure of release agent has low surface free energy and critical surface tension, and materials with high surface energy such as pressure-sensitive adhesives are difficult to adhere. The release force range of silicone release materials is adjustable and has good durability. It has been widely used in pressure-sensitive tapes, waterproof materials and other fields. However, some electronic products are very sensitive to silicon and fluorine elements, which leads to poor processing and short circuits of electronic products. Non-silicone release materials are mainly light release and heavy release. During the unwinding process of the tape, the release layer needs to be peeled off in a layer on the back of the PET surface for easy unwinding. And most of them are solvent-based, and the volatile organic compounds they contain seriously endanger human physical and mental health and living environment. It has become a new development trend to replace traditional solvent-based non-silicone release agents with green and environmentally friendly water-based non-silicone release agents.
[0003] Patent CN 114014959B discloses a non-silicon release agent with adjustable release force and melting point and a preparation method thereof, wherein the non-silicon release agent is prepared by a nucleophilic addition reaction between octadecyl isocyanate and polyvinyl alcohol. The non-silicon release agent has a relatively light release force, which is not convenient for unwinding the tape in the later production and processing process, and a large amount of VOC is generated during the preparation and alcohol precipitation process.
[0004] Patent CN 116063886A discloses a high temperature resistant non-silicone release material, a non-silicone release film and a preparation method thereof. By adjusting the ratio of high molecular weight acrylic resin and low molecular weight acrylic resin, the non-silicone release film has the characteristics of medium peeling, good high temperature resistance, low aging climbing rate of the release film, and high aging residual rate. However, a large amount of organic solvents need to be consumed in the preparation and subsequent coating process, which pollutes the environment and is costly.
[0005] Therefore, it is necessary to improve the existing technology to provide a more reliable solution. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a water-based non-silicone release agent, a preparation method thereof and a release film in view of the deficiencies in the above-mentioned prior art.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: in the first aspect of the present invention, a water-based medium-peeling non-silicone release agent is provided, comprising the following raw material components by mass percentage: 0.1%-0.2% sodium dodecyl sulfate, 0.1%-0.4% polyoxyethylene octylphenol ether-10, 20%-35% lauryl methacrylate, 3%-10% hydroxyethyl methacrylate, 0.01%-0.05% initiator, 5%-10% curing agent, and 50%-60% deionized water.
[0008] Preferably, the initiator is a persulfate initiator.
[0009] Preferably, the initiator is ammonium persulfate.
[0010] Preferably, the curing agent is a water-based isocyanate curing agent.
[0011] Preferably, the water-based isocyanate curing agent is Wanhua Chemical Aquolin 278.
[0012] A second aspect of the present invention provides a method for preparing the aqueous medium-peeling non-silicone release agent as described above, comprising the following steps:
[0013] S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier;
[0014] Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, and dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution;
[0015] The initiator is divided into two parts: a first part initiator and a second part initiator;
[0016] Divide the deionized water into four parts: the first part of deionized water, the second part of deionized water, and the third part of deionized water;
[0017] S2, mixing the first part of the emulsifier and the first part of the deionized water uniformly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring uniformly to obtain a pre-emulsion, adding the first part of the initiator to the pre-emulsion after heating, and keeping the temperature to obtain a seed emulsion;
[0018] S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution;
[0019] Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A;
[0020] S4, simultaneously adding the initiator solution and the mixed solution A to the seed emulsion obtained in step S2, heating for reaction, adjusting the pH value, filtering the material, adding a curing agent and a third portion of deionized water to the obtained product, stirring, and obtaining the aqueous medium-peeling non-silicon release agent.
[0021] Preferably, the method for preparing the aqueous non-silicone release agent comprises the following steps:
[0022] S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier;
[0023] Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, and dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution;
[0024] The initiator is divided into two parts: a first part initiator and a second part initiator;
[0025] Divide the deionized water into three parts: a first part of deionized water, a second part of deionized water, and a third part of deionized water;
[0026] S2, mixing the first part of the emulsifier and the first part of the deionized water evenly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring for 1-4 hours to obtain a pre-emulsion, heating to 70-90° C., adding the first part of the initiator to the pre-emulsion, and keeping warm for 0.5-2 hours to obtain a seed emulsion;
[0027] S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution;
[0028] Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A;
[0029] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the dropwise addition within 1-4 hours. Keep the reaction at 70-90° C. for 1-4 hours, adjust the pH value to 8, filter the material, add the curing agent and the third part of deionized water to the obtained product, and stir for 0.5-2 hours to obtain the aqueous medium-peel non-silicon release agent.
[0030] Preferably, the method for preparing the aqueous non-silicone release agent comprises the following steps:
[0031] S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier;
[0032] Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution, wherein the mass ratio of the first part of the mixed monomer solution to the second part of the mixed monomer solution is 1:2;
[0033] The initiator is divided into two parts: a first part initiator and a second part initiator;
[0034] Divide the deionized water into four parts: the first part of deionized water, the second part of deionized water, and the third part of deionized water;
[0035] S2, mixing the first part of the emulsifier and the first part of the deionized water evenly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring for 2 hours to obtain a pre-emulsion, heating to 80° C., adding the first part of the initiator to the pre-emulsion, and keeping warm for 1 hour to obtain a seed emulsion;
[0036] S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution;
[0037] Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A;
[0038] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the dropwise addition within 2 hours. Keep the reaction at 80° C. for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add the curing agent and the third part of deionized water to the obtained product, and stir for 1 hour to obtain the aqueous medium-peel non-silicon release agent.
[0039] A third aspect of the present invention provides a release film, which is prepared by the following method: uniformly coating the above-mentioned aqueous medium-release non-silicon release agent on a base film, baking and curing, to obtain the release film.
[0040] Preferably, the release film is prepared by the following method: the aqueous medium-peeling non-silicon release agent as described above is uniformly coated on a PET base film with a coating thickness of 500 nm, and baked at 120° C. for 1 min to obtain the release film.
[0041] The beneficial effects of the present invention are:
[0042] The present invention provides a water-based medium-peeling non-silicon release agent, a preparation method thereof, and a release film based on the release agent. In the release agent formula of the present invention, an acrylate binary copolymer is formed by combining a persulfate initiation system with a core-shell structure emulsion polymerization method, and under high-temperature coating curing conditions, the -OH on the acrylic resin binary copolymer reacts with -NCO to cure into a film; the lauryl methacrylate chain in the release agent has a moderate length and imparts medium-peeling force to the release film. The non-silicon release film prepared by the present invention has excellent film surface performance and has a stable medium-peeling effect on the tape, and the preparation process of the present invention is more environmentally friendly and has a good market application prospect. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0044] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0045] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0046] The invention provides an aqueous medium-peeling non-silicon release agent, which comprises the following raw material components by mass percentage: 0.1%-0.2% of sodium dodecyl sulfonate, 0.1%-0.4% of polyoxyethylene octylphenol ether-10, 20%-35% of lauryl methacrylate, 3%-10% of hydroxyethyl methacrylate, 0.01%-0.05% of initiator, 5%-10% of curing agent and 50%-60% of deionized water.
[0047] In a preferred embodiment, the initiator is a persulfate initiator. In a further preferred embodiment, the initiator is ammonium persulfate.
[0048] In a preferred embodiment, the curing agent is a water-based isocyanate curing agent. In a further preferred embodiment, the water-based isocyanate curing agent is Wanhua Chemical Aquolin 278.
[0049] The present invention also provides a method for preparing the above aqueous medium-peeling non-silicone release agent, comprising the following steps:
[0050] S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier;
[0051] Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, and dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution;
[0052] The initiator is divided into two parts: a first part initiator and a second part initiator;
[0053] Divide the deionized water into three parts: a first part of deionized water, a second part of deionized water, and a third part of deionized water;
[0054] S2, mixing the first part of the emulsifier and the first part of the deionized water evenly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring for 1-4 hours to obtain a pre-emulsion, heating to 70-90° C., adding the first part of the initiator to the pre-emulsion, and keeping warm for 0.5-2 hours to obtain a seed emulsion;
[0055] S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution;
[0056] Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A;
[0057] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 1-4 hours. Keep the reaction at 70-90° C. for 1-4 hours, adjust the pH value to 8, filter the material, add the curing agent and the third part of deionized water to the obtained product, and stir for 0.5-2 hours to obtain a water-based medium-peel non-silicone release agent.
[0058] In a preferred embodiment, the method for preparing an aqueous medium-peelable non-silicone release agent comprises the following steps:
[0059] S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier;
[0060] Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution, wherein the mass ratio of the first part of the mixed monomer solution to the second part of the mixed monomer solution is 1:2;
[0061] The initiator is divided into two parts: a first part initiator and a second part initiator;
[0062] Divide the deionized water into four parts: the first part of deionized water, the second part of deionized water, and the third part of deionized water;
[0063] S2, mixing the first part of the emulsifier and the first part of the deionized water evenly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring for 2 hours to obtain a pre-emulsion, heating to 80° C., adding the first part of the initiator to the pre-emulsion, and keeping warm for 1 hour to obtain a seed emulsion;
[0064] S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution;
[0065] Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A;
[0066] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add the curing agent and the third part of deionized water to the obtained product, and stir for 1 hour to obtain a water-based medium-peel non-silicone release agent.
[0067] The present invention also provides a release film, which is prepared by the following method: the above-mentioned water-based medium-peeling non-silicon release agent is evenly coated on a base film, and the release film is baked and cured to obtain the release film.
[0068] In a preferred embodiment, the release film is prepared by the following method: the above aqueous medium-peel non-silicon release agent is evenly coated on the PET base film with a coating thickness of 500 nm, and baked at 120° C. for 1 min to obtain the release film.
[0069] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0070] The sources of the main raw materials involved in the following examples and comparative examples are as follows:
[0071] Sodium dodecyl sulfate and ammonium persulfate were purchased from Aladdin.
[0072] Polyoxyethylene octylphenol ether-10 (OP-10, Huayuan Chemical),
[0073] Lauryl methacrylate (LMA, BASF),
[0074] Hydroxyethyl methacrylate (HEMA, BASF),
[0075] Water-based isocyanate curing agent (Aquolin278, Wanhua Chemical),
[0076] Example 1
[0077] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0078] S1, take 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0079] 20 g of lauryl methacrylate and 4 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0080] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.2g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0081] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0082] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.2 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0083] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 4g of aqueous isocyanate curing agent and 67g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0084] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0085] Example 2
[0086] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0087] S1, take 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0088] 16 g of lauryl methacrylate and 8 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0089] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.2g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0090] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0091] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.2 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0092] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 4g of aqueous isocyanate curing agent and 67g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0093] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0094] Example 3
[0095] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0096] S1, take 0.1g sodium dodecyl sulfate and 0.1g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.1g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0097] 16 g of lauryl methacrylate and 8 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0098] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.1g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0099] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0100] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.1 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0101] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 4g of aqueous isocyanate curing agent and 67g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0102] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0103] Example 4
[0104] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0105] S1, take 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0106] 16 g of lauryl methacrylate and 8 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0107] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.2g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0108] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0109] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.2 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0110] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 5g of aqueous isocyanate curing agent and 72g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0111] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0112] Example 5
[0113] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0114] S1, take 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0115] 16 g of lauryl methacrylate and 8 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0116] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.2g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0117] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0118] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.2 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0119] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 6g of aqueous isocyanate curing agent and 77g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0120] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0121] Comparative Example 1
[0122] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0123] S1, take 0.1g sodium dodecyl sulfate and 0.3g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.3g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0124] 16 g of lauryl methacrylate and 8 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0125] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.3g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0126] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0127] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.3 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0128] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 6g of aqueous isocyanate curing agent and 77g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0129] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0130] Comparative Example 2
[0131] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0132] S1, take 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0133] 20 g of lauryl methacrylate and 4 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0134] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.2g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0135] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0136] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.2 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0137] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 1g of aqueous isocyanate curing agent and 52g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0138] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0139] Comparative Example 3
[0140] A water-based medium-peel non-silicone release agent, the preparation method of which comprises the following steps:
[0141] S1, take 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the first part of the emulsifier; take another 0.1g sodium dodecyl sulfate and 0.2g polyoxyethylene octylphenol ether-10 and mix them as the second part of the emulsifier;
[0142] 20 g of methyl methacrylate and 4 g of hydroxyethyl methacrylate were mixed to obtain a mixed monomer solution, and the obtained mixed monomer solution was divided into two parts: a first part of the mixed monomer solution of 8 g and a second part of the mixed monomer solution of 16 g;
[0143] S2, the first part of the emulsifier (0.1g sodium dodecyl sulfate, 0.2g polyoxyethylene octylphenol ether-10) and 30g deionized water were mixed evenly to obtain an emulsifier solution; 8g of the first part of the mixed monomer solution was added to the emulsifier solution, stirred for 2h to obtain a pre-emulsion, and 0.02g of ammonium persulfate initiator was added to the pre-emulsion after heating to 80°C, and kept warm for 1h to obtain a seed emulsion;
[0144] S3, 0.02 g of ammonium persulfate initiator is added into 15 g of deionized water to obtain an initiator solution;
[0145] 18 g of the second part of the mixed monomer solution and the second part of the emulsifier (0.1 g of sodium dodecyl sulfate and 0.2 g of polyoxyethylene octylphenol ether-10) were mixed evenly to obtain a mixed solution A;
[0146] S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the addition within 2 hours. Keep the reaction at 80°C for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add 4g of aqueous isocyanate curing agent and 67g of deionized water to the obtained product, and stir for 1 hour to prepare a stable emulsion, i.e., an aqueous medium-peel non-silicone release agent.
[0147] A release film is prepared by the following method: the above aqueous medium-peeling non-silicon release agent is evenly coated on a PET base film (thickness is 50 μm), the coating thickness is 500 nm, and then placed in an oven and baked at 120° C. for 1 min to obtain a release film.
[0148] The release films prepared in the examples and comparative examples were subjected to the following performance tests:
[0149] 20min, 24H release force test method: standard tape Nitto 31B is attached to the release surface, rolled back and forth twice with a 2kg roller (300mm / min), and then placed at room temperature (23±2℃, relative humidity 50%) for 20min and 24H, and then peeled 180° at 300mm / min with a universal tensile testing machine. Test 3 times and take the average value, which is recorded as the 20min, 24H release force.
[0150] 20H aging release force test method: Standard tape Nitto 31B is attached to the release surface, rolled back and forth twice with a 2kg roller (300mm / min), then placed in a 55℃ oven, aged for 20H, taken out and placed at room temperature for 2h, then peeled 180° at 300mm / min using a universal tensile testing machine, tested 3 times, and the average value was taken.
[0151] Residual test method: Standard tape Nitto 31B is attached to the release surface, and rolled back and forth twice with a 2kg roller (300mm / min), then placed in a 55℃ oven, aged for 20 hours, taken out and placed at room temperature for 2 hours, Nitto 31B on the test sample is peeled off and attached to a standard steel plate, and rolled back and forth twice with a 2kg roller, and the peeling force is tested after standing for 20 minutes, which is recorded as A1. Standard tape Nitto 31B is attached to a release standard steel plate, and rolled back and forth twice with a 2kg roller (300mm / min), and the peeling force is tested after standing for 20 minutes, which is recorded as A2.
[0152] Release film appearance: There is no rainbow or line defect on the surface of the release film, and the coating does not fall off after repeated rubbing by hand, which indicates that the release film has excellent appearance.
[0153] Residual SA%=(A1 / A2)×100%.
[0154] The test results are shown in Table 1 below:
[0155] Table 1
[0156]
[0157] Note: Comparative Examples 1 and 2 could not form release films that could be used for testing, so no relevant performance tests were conducted. The release film appearance was judged as follows: if there were no rainbow or line defects on the release film surface, and the coating did not fall off after multiple hand rubbing, the release film was judged to have excellent appearance.
[0158] According to the test results in Table 1, it can be seen that the release films prepared in Examples 1-5 have excellent comprehensive properties. In the examples, by using the method of acrylate core-shell emulsion polymerization, it is possible to have both medium peelability for the tape and low aging climb properties while avoiding the environmental hazards of organic solvents.
[0159] Comparison of the data of comparative example 3 with those of examples 1-5 shows that the long-chain acrylic resin can significantly reduce the release force of the release film, achieving the technical effect of mid-peeling, and the water-based isocyanate can achieve complete curing of the coating.
[0160] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A water-based non-silicone release agent, characterized in that: The invention comprises the following raw material components in percentage by mass: 0.1%-0.2% of sodium dodecyl sulfonate, 0.1%-0.4% of polyoxyethylene octylphenol ether-10, 20%-35% of lauryl methacrylate, 3%-10% of hydroxyethyl methacrylate, 0.01%-0.05% of initiator, 5%-10% of curing agent and 50%-60% of deionized water.
2. The water-based non-silicone release agent according to claim 1, characterized in that: The initiator is a persulfate initiator.
3. The aqueous non-silicone release agent according to claim 2, characterized in that: The initiator is ammonium persulfate.
4. The water-based non-silicone release agent according to claim 1, characterized in that: The curing agent is a water-based isocyanate curing agent.
5. The water-based non-silicone release agent according to claim 4, characterized in that: The water-based isocyanate curing agent is Wanhua Chemical Aquolin278.
6. A method for preparing a water-based non-silicone release agent as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier; Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, and dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution; The initiator is divided into two parts: a first part initiator and a second part initiator; Divide the deionized water into four parts: the first part of deionized water, the second part of deionized water, and the third part of deionized water; S2, mixing the first part of the emulsifier and the first part of the deionized water uniformly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring uniformly to obtain a pre-emulsion, adding the first part of the initiator to the pre-emulsion after heating, and keeping the temperature to obtain a seed emulsion; S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution; Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A; S4, simultaneously adding the initiator solution and the mixed solution A to the seed emulsion obtained in step S2, heating for reaction, adjusting the pH value, filtering the material, adding a curing agent and a third portion of deionized water to the obtained product, stirring, and obtaining the aqueous medium-peeling non-silicon release agent.
7. The method for preparing the aqueous medium-peeling non-silicone release agent according to claim 6, characterized in that: The following steps are involved: S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier; Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, and dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution; The initiator is divided into two parts: a first part initiator and a second part initiator; Divide the deionized water into three parts: a first part of deionized water, a second part of deionized water, and a third part of deionized water; S2, mixing the first part of the emulsifier and the first part of the deionized water evenly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring for 1-4 hours to obtain a pre-emulsion, heating to 70-90° C., adding the first part of the initiator to the pre-emulsion, and keeping warm for 0.5-2 hours to obtain a seed emulsion; S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution; Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A; S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the dropwise addition within 1-4 hours. Keep the reaction at 70-90° C. for 1-4 hours, adjust the pH value to 8, filter the material, add the curing agent and the third part of deionized water to the obtained product, and stir for 0.5-2 hours to obtain the aqueous medium-peel non-silicon release agent.
8. The method for preparing the aqueous medium-peeling non-silicone release agent according to claim 7, characterized in that: The following steps are involved: S1, taking part of sodium dodecyl sulfate and part of polyoxyethylene octylphenol ether-10 and mixing them as the first part of the emulsifier; mixing the remaining part of sodium dodecyl sulfate and the remaining part of polyoxyethylene octylphenol ether-10 as the second part of the emulsifier; Mixing lauryl methacrylate and hydroxyethyl methacrylate to obtain a mixed monomer solution, dividing the obtained mixed monomer solution into two parts: a first part of the mixed monomer solution and a second part of the mixed monomer solution, wherein the mass ratio of the first part of the mixed monomer solution to the second part of the mixed monomer solution is 1:2; The initiator is divided into two parts: a first part initiator and a second part initiator; Divide the deionized water into four parts: the first part of deionized water, the second part of deionized water, and the third part of deionized water; S2, mixing the first part of the emulsifier and the first part of the deionized water evenly to obtain an emulsifier solution; adding the first part of the mixed monomer solution to the emulsifier solution, stirring for 2 hours to obtain a pre-emulsion, heating to 80° C., adding the first part of the initiator to the pre-emulsion, and keeping warm for 1 hour to obtain a seed emulsion; S3, adding the second part of initiator to the second part of deionized water to obtain an initiator solution; Evenly mixing the second part of the mixed monomer solution and the second part of the emulsifier to obtain a mixed solution A; S4. Add the initiator solution and the mixed solution A to the seed emulsion obtained in step S2 simultaneously, and complete the dropwise addition within 2 hours. Keep the reaction at 80° C. for 2 hours, adjust the pH value to 8 with ammonia water, filter the material, add the curing agent and the third part of deionized water to the obtained product, and stir for 1 hour to obtain the aqueous medium-peel non-silicon release agent.
9. A release film, characterized in that: The release film is prepared by the following method: uniformly coating the water-based medium-peel non-silicon release agent as claimed in any one of claims 1 to 5 on a base film, baking and curing, and obtaining the release film.
10. The release film according to claim 9, characterized in that: The release film is prepared by the following method: the water-based medium-peel non-silicon release agent as described in any one of claims 1 to 5 is uniformly coated on a PET base film with a coating thickness of 500 nm, and baked at 120° C. for 1 min to obtain the release film.
Citation Information
Patent Citations
Environment-friendly emulsion type ultra-low peeling force protective film
CN110791222A
Acrylic acid type light-release-force release agent, release film and preparation method of acrylic acid type light-release-force release agent
CN116082938A
Waterborne acrylic low adhesion backsize and release coating compositions, methods of making the compositions, and sheet materials coated therewith
EP0448399A2
Resin composition for release film comprising itaconic acid ester with long alkyl side chain
KR1020140088431A
Waterborne (meth) acrylic latex polymers for release
US5516865A
Cited By
Environment-friendly water-based release agent, water-based release film and implementation method of water-based release film
CN119391244A