Molybdenum trioxide two-dimensional crystal material and preparation method and application thereof

By forming atomic steps on a C-plane sapphire substrate and performing physical vapor deposition, highly directional two-dimensional molybdenum trioxide crystals were prepared, which solved the problems of complex preparation and difficult morphology control of two-dimensional molybdenum trioxide crystals in the existing technology. problem, realizing efficient mid-infrared optical metalens imaging applications.

CN118792735APending Publication Date: 2024-10-18CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410858904.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the existing technology, the preparation method of two-dimensional molybdenum trioxide crystal is relatively complex, lacks morphology control, and is difficult to achieve efficient light field compression and light focusing.

Method used

A C-face sapphire substrate is used for heat treatment to form atomic steps, and a two-dimensional molybdenum trioxide crystal is prepared by physical vapor deposition. 60% to 70% of the (001) crystal faces are parallel to the direction of the atomic steps, and 30% to 40% of the crystal faces The included angle is 60°C, and the included angle of the cone is 15~25°, forming a large-area, ultra-thin conical molybdenum trioxide crystal.

Benefits of technology

Pure ultra-thin two-dimensional cone-shaped molybdenum trioxide crystals have been successfully prepared for use in mid-infrared optical metalens imaging. They are low-cost, simple to operate, comply with environmental protection requirements, and have good prospects for mid-infrared optical metalens imaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792735A_ABST
    Figure CN118792735A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor materials, and particularly discloses a molybdenum trioxide two-dimensional crystal material and a preparation method and application thereof. According to the material, C-plane sapphire subjected to heat treatment serves as a growth substrate, pure large-area ultrathin two-dimensional conical molybdenum trioxide crystals are successfully prepared through a physical vapor deposition method, the crystals are directionally arranged along atomic steps on the surface of the C-plane sapphire substrate, the crystal face (001) of 60%-70% of the molybdenum trioxide conical crystals is parallel to the direction of the atomic steps, and the crystal face (002) of the molybdenum trioxide conical crystals is parallel to the direction of the atomic steps. The included angle between the (001) crystal face of the 30%-40% molybdenum trioxide conical crystal and the atomic step direction is 60 DEG C, and the conical included angle ranges from 15 degrees to 25 degrees. The cost of the required raw materials is low, the process operation is simple, the environmental protection requirement is met, and the application prospect of the material in mid-infrared optical super-lens imaging is considerable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semiconductor materials, and specifically relates to a two-dimensional molybdenum trioxide crystal material and a preparation method and application thereof. Background Art

[0002] The enhancement of the interaction between light and matter has many application prospects in the fields of nanolasers, nanobiosensors and enhanced optical nonlinearity. Two-dimensional molybdenum trioxide supports natural in-plane hyperbolic phonon polaritons, which can compress mid-infrared light to the nanoscale.

[0003] In the existing technology, there are not many methods for preparing two-dimensional molybdenum trioxide crystals because the crystal growth conditions of transition metal oxides are more complicated than those of transition metal chalcogenides. Most of the published research work does not involve the morphology control of two-dimensional molybdenum trioxide. In order to pursue more extreme light field compression, how to make conical two-dimensional molybdenum trioxide and efficiently focus light to the top of the cone is a technical problem that researchers urgently need to solve. Summary of the invention

[0004] The purpose of the present invention is to provide a two-dimensional crystalline material of molybdenum trioxide and a preparation method and application thereof in view of the above-mentioned deficiencies in the prior art.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] The first purpose of the present invention is to provide a two-dimensional molybdenum trioxide crystal material, which has atomic steps and multiple molybdenum trioxide conical crystals arranged along the atomic steps on the surface of a C-plane sapphire substrate, wherein 60% to 70% of the (001) crystal planes of the molybdenum trioxide conical crystals are parallel to the direction of the atomic steps, and 30% to 40% of the (001) crystal planes of the molybdenum trioxide conical crystals are at an angle of 60° to the direction of the atomic steps, and the cone angle is between 15 and 25°.

[0007] Furthermore, the molybdenum trioxide two-dimensional crystal material has a length of 1000 to 5000 μm and a width of 200 to 1000 μm.

[0008] Furthermore, the thickness of the two-dimensional molybdenum trioxide crystal is between 15 and 20 nm.

[0009] The second object of the present invention is to provide a method for preparing the above-mentioned molybdenum trioxide two-dimensional crystalline material, comprising the following steps:

[0010] S1, gasifying the molybdenum oxide precursor compound to form molybdenum trioxide vapor;

[0011] S2. Using C-plane sapphire as a growth substrate, in a mixed gas of argon and oxygen, cool and deposit molybdenum trioxide vapor on the C-plane sapphire, wherein the surface of the C-plane sapphire has a plurality of atomic steps.

[0012] Furthermore, in step S1, the molybdenum oxide precursor compound includes any one of metallic molybdenum, molybdenum oxide, and molybdate.

[0013] Furthermore, in step S2, the C-plane sapphire is heat-treated so that its surface has a plurality of atomic steps.

[0014] Furthermore, in step S2, the gas flow ratio of argon gas to oxygen gas is (3-6):1.

[0015] Furthermore, the molybdenum oxide precursor compound is molybdenum trioxide.

[0016] Furthermore, the temperature of the gasification is 750-800°C, and the temperature of the cooling deposition is 500-600°C.

[0017] The third object of the present invention is to provide the application of the above-mentioned molybdenum trioxide two-dimensional crystal material in the preparation of mid-infrared optical superlens imaging products.

[0018] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0019] (1) The present invention provides a two-dimensional molybdenum trioxide crystal material, a preparation method and an application thereof. Using heat-treated C-face sapphire as a growth substrate, a pure, large-area, ultra-thin two-dimensional conical molybdenum trioxide crystal is successfully prepared by a physical vapor deposition method, and the atomic steps along the surface of the C-face sapphire substrate are oriented and arranged, wherein 60% to 70% of the (001) crystal planes of the molybdenum trioxide conical crystals are parallel to the direction of the atomic steps, and 30% to 40% of the (001) crystal planes of the molybdenum trioxide conical crystals are at an angle of 60° to the direction of the atomic steps, and the cone angle is between 15 and 25°.

[0020] (2) The raw material cost required by the present invention is low, the process operation is simple, and it meets environmental protection requirements. In addition, the application prospect of the material in mid-infrared optical superlens imaging is promising. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram of the process flow of the molybdenum trioxide two-dimensional crystal material provided by the present invention;

[0022] Figure 2 A surface atomic force microscope (AFM) image of the C-plane sapphire substrate after heat treatment provided by the present invention;

[0023] Figure 3An optical photograph of a two-dimensional conical molybdenum trioxide single crystal provided by the present invention;

[0024] Figure 4 A high-resolution transmission electron microscope image of a two-dimensional molybdenum trioxide single crystal provided by the present invention;

[0025] Figure 5 The selected area electron diffraction pattern of the two-dimensional tapered molybdenum trioxide single crystal provided by the present invention;

[0026] Figure 6 The X-ray photoelectron spectrum of the two-dimensional conical molybdenum trioxide single crystal provided by the present invention;

[0027] Figure 7 This is a near-field optical imaging diagram of the two-dimensional conical molybdenum trioxide single crystal provided by the present invention under mid-infrared light excitation. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention are further described in detail below in conjunction with specific examples and drawings. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.

[0029] refer to Figure 1 , which is a schematic diagram of the process flow of preparing highly oriented molybdenum trioxide two-dimensional crystalline materials according to the present invention, specifically: prepare a multi-temperature zone tubular furnace, which includes a high temperature zone and a low temperature zone, weigh molybdenum oxide precursor compound powder and place it in a quartz boat, move the quartz boat into the high temperature zone of the tubular furnace, move the C-face sapphire substrate into the low temperature zone of the tubular furnace, and the quartz boat is 25 cm away from the C-face sapphire substrate, then, introduce Ar / O2 mixed gas, calcine in the high temperature zone to gasify the molybdenum oxide precursor compound to form molybdenum trioxide vapor, and in the low temperature zone, cool and deposit the molybdenum trioxide vapor on the C-face sapphire.

[0030] In a specific implementation scheme, the C-face sapphire is heat-treated and has multiple atomic steps on its surface. For example, a clean C-face sapphire substrate is kept at 1000°C for 200 minutes and then naturally cooled to room temperature. The average height of the atomic steps after heat treatment is 1nm, and the distance between the atomic steps is 100-200nm.

[0031] In a specific embodiment, the molybdenum oxide precursor compound is not particularly limited as long as it is a precursor compound for forming the molybdenum trioxide two-dimensional crystalline material of the present invention.

[0032] The molybdenum oxide precursor compound is not particularly limited as long as it is a compound that forms molybdenum trioxide vapor by calcination, and can be selected from: metal molybdenum, molybdenum trioxide, molybdenum dioxide, molybdenum sulfide, phosphomolybdic acid, silicomolybdic acid, aluminum molybdate, silicon molybdate, magnesium molybdate, sodium molybdate, titanium molybdate, iron molybdate, potassium molybdate, zinc molybdate, boron molybdate, lithium molybdate, cobalt molybdate, nickel molybdate, manganese molybdate, chromium molybdate, cesium molybdate, barium molybdate, strontium molybdate, yttrium molybdate, zirconium molybdate. These molybdenum oxide precursor compounds can be used alone or in combination of two or more. These molybdenum oxide precursor compounds can be used alone or in combination of two or more.

[0033] A preferred molybdenum oxide precursor compound may be commercially available molybdenum trioxide.

[0034] The calcination temperature used to gasify the molybdenum oxide precursor compound to form molybdenum trioxide vapor also depends on the decomposable temperature of the specific molybdenum oxide precursor compound selected. For example, when using a molybdenum compound as a molybdenum oxide precursor compound, the calcination temperature is preferably 500° C. to 1600° C. When molybdenum trioxide is selected, the calcination temperature can be 750° C. to 800° C.

[0035] The temperature for cooling and depositing molybdenum trioxide vapor on C-plane sapphire is preferably 500-600°C.

[0036] The specific implementation method is described below. The molybdenum trioxide powder used in the embodiment is commercially available with a purity of 99.99%, and is orthorhombic molybdenum trioxide.

[0037] Example 1

[0038] A method for preparing a conical two-dimensional molybdenum trioxide crystal comprises the following steps:

[0039] (1) The C-side sapphire substrate was ultrasonicated with acetone, anhydrous ethanol, and deionized water for 20 min respectively and then dried with a N2 gun;

[0040] (2) placing a clean C-plane sapphire substrate in a single-temperature zone tube furnace and keeping it at 1000°C for 200 min, and then cooling it naturally to room temperature after the end of the heat preservation;

[0041] (3) placing commercial molybdenum trioxide powder and annealed C-plane sapphire substrate in the high temperature zone and low temperature zone of a multi-temperature zone tube furnace respectively;

[0042] (4) The temperature of the high temperature zone in step (3) is set to 780° C., and the temperature of the low temperature zone is set to 580° C.;

[0043] (5) Maintain the argon gas flow rate in the multi-temperature zone tubular furnace at 48 sccm and the oxygen gas flow rate at 12 sccm.

[0044] (6) The heating time in step (3) and step (4) is controlled to be 78 minutes, and the insulation time after heating to the set temperature is 20 minutes. After the insulation is completed, it is naturally cooled to room temperature to obtain a two-dimensional molybdenum trioxide crystalline material.

[0045] Example 2

[0046] A method for preparing a conical two-dimensional molybdenum trioxide crystal comprises the following steps:

[0047] (1) The C-side sapphire substrate was ultrasonicated with acetone, anhydrous ethanol, and deionized water for 20 min respectively and then dried with a N2 gun;

[0048] (2) placing a clean C-plane sapphire substrate in a single-temperature zone tube furnace and keeping it at 1000°C for 200 min, and then cooling it naturally to room temperature after the end of the heat preservation;

[0049] (3) placing commercial molybdenum trioxide powder and annealed C-plane sapphire substrate in the high temperature zone and low temperature zone of a multi-temperature zone tube furnace respectively;

[0050] (4) The temperature of the high temperature zone in step (3) is set to 780° C., and the temperature of the low temperature zone is set to 540° C.;

[0051] (5) Maintain the argon gas flow rate in the multi-temperature zone tubular furnace at 36 sccm and the oxygen gas flow rate at 24 sccm.

[0052] (6) The heating time in step (3) and step (4) is controlled to be 78 minutes, and the insulation time after heating to the set temperature is 60 minutes. After the insulation is completed, it is naturally cooled to room temperature to obtain a two-dimensional molybdenum trioxide crystalline material.

[0053] Example 3

[0054] A method for preparing a conical two-dimensional molybdenum trioxide crystal comprises the following steps:

[0055] (1) The C-side sapphire substrate was ultrasonicated with acetone, anhydrous ethanol, and deionized water for 20 min respectively and then dried with a N2 gun;

[0056] (2) placing a clean C-plane sapphire substrate in a single-temperature zone tube furnace and keeping it at 1000°C for 200 min, and then cooling it naturally to room temperature after the end of the heat preservation;

[0057] (3) placing commercial molybdenum trioxide powder and annealed C-plane sapphire substrate in the high temperature zone and low temperature zone of a multi-temperature zone tube furnace respectively;

[0058] (4) The temperature of the high temperature zone in step (3) is set to 780° C., and the temperature of the low temperature zone is set to 600° C.;

[0059] (5) Maintain the argon gas flow rate in the multi-temperature zone tubular furnace at 16 sccm and the oxygen gas flow rate at 4 sccm.

[0060] (6) The heating time in step (3) and step (4) is controlled to be 156 min, and the insulation time after reaching the set temperature is 30 min. After the insulation is completed, it is naturally cooled to room temperature to obtain a two-dimensional molybdenum trioxide crystalline material.

[0061] Example 4

[0062] A method for preparing a conical two-dimensional molybdenum trioxide crystal comprises the following steps:

[0063] (1) The C-side sapphire substrate was ultrasonicated with acetone, anhydrous ethanol, and deionized water for 20 min respectively and then dried with a N2 gun;

[0064] (2) placing a clean C-plane sapphire substrate in a single-temperature zone tube furnace and keeping it at 1100°C for 200 min, and then cooling it naturally to room temperature after the end of the heat preservation;

[0065] (3) placing commercial molybdenum trioxide powder and annealed C-plane sapphire substrate in the high temperature zone and low temperature zone of a multi-temperature zone tube furnace respectively;

[0066] (4) The temperature of the high temperature zone in step (3) is set to 760° C., and the temperature of the low temperature zone is set to 580° C.;

[0067] (5) Maintain the argon gas flow rate in the multi-temperature zone tubular furnace at 48 sccm and the oxygen gas flow rate at 12 sccm.

[0068] (6) The heating time in step (3) and step (4) is controlled to be 78 minutes, and the insulation time after reaching the set temperature is 120 minutes. After the insulation is completed, it is naturally cooled to room temperature to obtain a two-dimensional molybdenum trioxide crystalline material.

[0069] Example 5

[0070] A method for preparing a conical two-dimensional molybdenum trioxide crystal comprises the following steps:

[0071] (1) The C-side sapphire substrate was ultrasonicated with acetone, anhydrous ethanol, and deionized water for 20 min respectively and then dried with a N2 gun;

[0072] (2) placing a clean C-plane sapphire substrate in a single-temperature zone tube furnace and keeping it at 1140°C for 300 min, and then cooling it naturally to room temperature after the end of the heat preservation;

[0073] (3) placing commercial molybdenum trioxide powder and annealed C-plane sapphire substrate in the high temperature zone and low temperature zone of a multi-temperature zone tube furnace respectively;

[0074] (4) The temperature of the high temperature zone in step (3) is set to 780° C., and the temperature of the low temperature zone is set to 600° C.;

[0075] (5) Maintain the argon gas flow rate in the multi-temperature zone tubular furnace at 48 sccm and the oxygen gas flow rate at 12 sccm.

[0076] (6) The heating time in step (3) and step (4) is controlled to be 156 min, and the insulation time after reaching the set temperature is 60 min. After the insulation is completed, it is naturally cooled to room temperature to obtain a two-dimensional molybdenum trioxide crystalline material.

[0077] In order to better illustrate the performance of the molybdenum trioxide two-dimensional crystalline material prepared by the present invention, the applicant conducted the following research:

[0078] Example 1-Example 5 have similar structures and properties. The prepared molybdenum trioxide two-dimensional crystalline material has atomic steps on the surface of the C-plane sapphire substrate and multiple molybdenum trioxide conical crystals arranged along the atomic steps, wherein 60% to 70% of the molybdenum trioxide conical crystals have (001) crystal planes parallel to the atomic step direction, and 30% to 40% of the molybdenum trioxide conical crystals have an angle of 60° with the (001) crystal plane and the atomic step direction. The cone angle is between 15 and 25°. The molybdenum trioxide two-dimensional crystalline material has a length of 1000-5000μm, a width of 200-1000μm, and a thickness of 15 to 20nm.

[0079] The following is described using Example 1 as an example:

[0080] refer to Figure 2 , is the AFM morphology of the C-plane sapphire substrate surface after heat treatment. It can be seen from the image that parallel atomic-level steps are formed on the C-plane sapphire surface after annealing. The step height is about 1nm, and the spacing between the steps is 100-200nm, which provides lower energy nucleation sites for the subsequent nucleation of two-dimensional molybdenum trioxide.

[0081] refer to Figure 3 , is an optical photograph of a two-dimensional molybdenum trioxide cone crystal prepared in Example 1. It can be seen from Figure a that the molybdenum trioxide cone crystal is oriented along the atomic step height. According to statistics, 60% to 70% of the molybdenum trioxide cone crystals have (001) crystal planes parallel to the atomic step direction, and 30% to 40% of the molybdenum trioxide cone crystals have an angle of 60° with the atomic step direction. Figure b is a partial enlarged view of the molybdenum oxide cone crystal, and a cone-shaped morphology is formed at the tip of the crystal. The length of the molybdenum trioxide two-dimensional crystal material is 1000-5000μm and the width is 200-1000μm. Figures c and d are enlarged views of the tip of the crystal, and the cone angle is between 15 and 25°.

[0082] refer to Figure 4 , which is a high-resolution transmission electron microscope image of a two-dimensional molybdenum trioxide pyramidal crystal. The lattice constants along the

[100] and

[001] directions are consistent with the standard lattice constants, indicating that the prepared two-dimensional molybdenum trioxide has a high degree of crystallinity.

[0083] refer to Figure 5 Figures ad in the figure are selected area electron diffraction obtained from different areas of the two-dimensional molybdenum trioxide conical crystal prepared in Example 1. Maintaining the same direction indicates the single crystal nature of the conical two-dimensional molybdenum trioxide.

[0084] refer to Figure 6 , is a high-resolution X-ray photoelectron spectrum of the two-dimensional molybdenum trioxide single crystal prepared in Example 1. It can be seen that the prepared crystal has fewer defects and good crystallinity.

[0085] In order to better illustrate that the molybdenum trioxide two-dimensional crystal material prepared by the present invention has excellent mid-infrared optical superlens imaging performance, the applicant conducted the following research:

[0086] Example 6

[0087] 0.1g of raw material MoO3 powder was placed in a corundum crucible and placed upstream of a dual-temperature zone tube furnace, with the sintering temperature set to 770°C and the holding time set to 1h; a C-face sapphire substrate after high-temperature annealing was placed downstream, with the sintering temperature set to 560°C and the holding time set to 1h. After the reaction was completed, a two-dimensional conical molybdenum trioxide flake was obtained on the C-face sapphire substrate.

[0088] Figure 7 This is a near-field optical imaging image of the two-dimensional conical molybdenum trioxide single crystal prepared in Example 6 under mid-infrared light excitation. In the light field characterization mode, there is a highly localized light field at the tip of the cone. The near-field amplitude at the localized location is extracted. The "near-field hotspot" excited at 11.24 microns is only 35nm, which is 1 / 10 of the natural space excitation light volume. -8 It is expected to realize ultra-thin, high-transmission-density two-dimensional transition metal oxide multifunctional optical resonant devices, providing advanced solutions for mid-infrared optical sensing, superlens imaging, and on-chip integration.

[0089] In the absence of conflict, the above embodiments and features in the embodiments may be combined with each other.

[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A two-dimensional molybdenum trioxide crystalline material, characterized in that: The surface of the C-plane sapphire substrate is provided with atomic steps and a plurality of molybdenum trioxide pyramidal crystals arranged along the atomic steps, wherein 60% to 70% of the molybdenum trioxide pyramidal crystals have (001) crystal planes parallel to the atomic step direction, and 30% to 40% of the molybdenum trioxide pyramidal crystals have an angle of 60° with the atomic step direction, and the pyramidal angle is between 15 and 25°.

2. The molybdenum trioxide two-dimensional crystalline material according to claim 1, characterized in that The length of the molybdenum trioxide cone crystal is 1000-5000 μm, and the width is 200-1000 μm.

3. The molybdenum trioxide two-dimensional crystalline material according to claim 1, characterized in that The thickness is 15 to 20 nm.

4. A method for preparing the two-dimensional molybdenum trioxide crystalline material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, gasifying the molybdenum oxide precursor compound to form molybdenum trioxide vapor; S2. Using C-plane sapphire as a growth substrate, in a mixed gas of argon and oxygen, cool and deposit molybdenum trioxide vapor on the C-plane sapphire, wherein the surface of the C-plane sapphire has a plurality of atomic steps.

5. The preparation method according to claim 4, characterized in that: In step S1, the molybdenum oxide precursor compound includes any one of metallic molybdenum, molybdenum oxide, and molybdate.

6. The preparation method according to claim 4, characterized in that: In step S2, the C-plane sapphire is heat-treated so that its surface has a plurality of atomic steps.

7. The preparation method according to claim 5, characterized in that: In step S2, the gas flow ratio of argon gas to oxygen gas is (3-6):

1.

8. The preparation method according to claim 7, characterized in that: The molybdenum oxide precursor compound is molybdenum trioxide.

9. The preparation method according to claim 8, characterized in that: The temperature of the gasification is 750-800°C, and the temperature of the cooling deposition is 500-600°C.

10. Use of the molybdenum trioxide two-dimensional crystal material as described in any one of claims 1 to 3 in the preparation of mid-infrared optical superlens imaging products.

Citation Information

Cited By

  • Alpha-Al2Mo3O12 nanosheet as well as preparation method and application thereof

    CN119776988A

  • Dielectric film manufacturing method, dielectric film and two-dimensional field effect transistor

    CN121335177A

  • Method for manufacturing dielectric thin film, dielectric thin film, and two-dimensional field effect transistor

    CN121335177B

  • Wafer-level aluminum molybdate film, preparation method and packaging method thereof, and semiconductor device

    CN122803758A