Cardanol-blocked polyisocyanate emulsion, preparation method thereof, and application thereof in waterproof finishing of fabrics

By blocking the polyisocyanate water dispersible emulsion by cashew phenol, the problem of unstable VOC and water dispersion of textile waterproofing agents is solved, fiber adhesion and waterproofing performance are improved, efficient waterproofing efficiency and curing effect are achieved, and waterproofing agents are reduced. Dosage avoids hard feel and white marks.

CN118792880BActive Publication Date: 2024-11-12GUANGDONG INNOVATIVE FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411253591.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing textile waterproofing agents have problems such as VOC, unstable water dispersion, low adhesion and peel strength to fibers, and low unsealing and crosslinking efficiency, resulting in poor waterproofing efficiency and curing performance.

Method used

Polyisocyanate water dispersible emulsion blocked with cashew phenol, diisocyanate addition condensation under nitrogen protection, alkaline ionic liquid catalyst and acid stop agent, combined with internal emulsifier and external emulsifier, and obtained by phase transfer emulsification. Stable nanoscale aqueous dispersion.

Benefits of technology

The cashew phenol blocked polyisocyanate emulsion is achieved without VOC and has good water dispersion stability, which improves fiber adhesion and peel strength, improves waterproof performance and durability, reduces the amount of waterproofing agent, and solves the problem of hard feel and white marks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
  • Figure 6L4JK154K9Q8YNR0SVSGOMDESN5REY2PI2YPV3TF
    Figure 6L4JK154K9Q8YNR0SVSGOMDESN5REY2PI2YPV3TF
Patent Text Reader

Abstract

The invention provides a cardanol-blocked polyisocyanate emulsion and a preparation method thereof and an application thereof in fabric waterproof finishing, belonging to the technical field of textile printing and dyeing, wherein the preparation method comprises the following steps: (1) adding and condensing diisocyanate under the catalytic action of alkaline ionic liquid, and when the conversion rate reaches 30-50%, terminating the condensation reaction to obtain polyisocyanate; (2) first blocking the NCO part in the polyisocyanate with an internal emulsifier and a catalyst, and then blocking all the remaining NCO with cardanol, cooling and discharging, and obtaining cardanol-blocked polyisocyanate; (3) mixing the cardanol-blocked polyisocyanate, an external emulsifier, and glacial acetic acid, slowly adding water at the same temperature and emulsifying by a phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion. The cardanol-blocked polyisocyanate emulsion of the present invention has a simple preparation process and excellent comprehensive performance for waterproof finishing working fluid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile printing and dyeing, and particularly relates to a cardanol-blocked polyisocyanate emulsion and a preparation method thereof and application thereof in waterproof finishing of fabrics. Background Art

[0002] With economic development and social progress, people pay more and more attention to the functionality of fiber textiles, such as waterproof, oil-proof, fire-proof, and radiation-proof properties. Early waterproofing agents had the disadvantages of poor washability, poor hand feel, odor, and potential formaldehyde release after being applied to fabrics. Until the emergence of fluorocarbon waterproofing agents (C8), they were widely used in the waterproof, oil-proof and anti-fouling finishing of fabrics, which depends on the ultra-low surface energy (17-18mN / m) of the side group of the main chain - C8 fluorocarbon chain. However, ecological studies have shown that the C8 fluorocarbon waterproofing agent for textiles will be accompanied by the production and use of PFOA and PFOS by-products, which are difficult to degrade, bioaccumulate, and carcinogenic. The ecological protection of textiles has prompted people to develop fluorocarbon waterproofing agents below C6 and fluorine-free waterproofing agents. The waterproof and oil-proof grades of fluorocarbon waterproofing agents below C6 can only reach the level of C8 with a higher dosage, and the washing durability is worse than that of C8. Similarly, the dosage of fluorine-free waterproofing agents must be increased to achieve the waterproof grade of C8 fluorocarbon, but the washing durability still cannot meet customer requirements. Therefore, how to improve the waterproof performance and washing durability of fluorocarbon waterproofing agents below C6 and fluorine-free waterproofing agents on fabrics are two problems currently existing in fabric waterproofing finishing.

[0003] At present, in order to solve the above two problems, on the one hand, starting from molecular design, changing the structure of the key components of the waterproofing agent to regulate the waterproofness and washing durability of the fabric. On the other hand, starting from the design of the working solution formula, adding a cross-linking agent, changing the binding mode of the waterproofing agent on the fabric, in order to reduce the amount of waterproof finishing agent (increasing efficiency) and improve the washing durability of the finishing (curing). Obviously, molecular design can fundamentally solve the problem, but it is difficult, has a long development cycle and high cost; while the working solution formula design belongs to the compounding technology, which has the advantages of low difficulty, short time and quick effect.

[0004] Early waterproofing agents (including fluorine-containing and fluorine-free) used urea-formaldehyde resin or melamine-formaldehyde resin for crosslinking and fixing. Since this type of aldehyde resin crosslinking agent has a small amount of free formaldehyde or formaldehyde release, it has been replaced by blocked polyisocyanate emulsion (patents CN103668957B, CN115819723A, CN114729100A). The key factors affecting the synergistic and curing performance of blocked polyisocyanate emulsion for waterproof finishing include polyisocyanate structure, blocking agent, water dispersion state, etc.

[0005] Commonly used blocking agents include methyl ethyl ketone oxime, sodium bisulfite, 3,5-dimethylpyrazole, etc. The blocked products are mostly solid at room temperature, and direct emulsification is very difficult. Generally, a large amount of solvents and emulsifiers must be added to obtain a more uniform emulsion, but the particle size is large (micrometer level), and it is easy to stratify during storage. As a result, the price of such crosslinking agents of blocked polyisocyanate emulsions is high, the storage stability is poor, and they cannot be made into an integrated auxiliary agent with waterproofing agent emulsions. They are extremely inconvenient to use. Volatile organic compounds (VOCs) such as solvents and blocking agents are generated during heating and baking, affecting the production environment and safety. Phenol was the earliest blocking agent used for isocyanates, but its unblocking temperature is too high (>180°C), and the product is solid at room temperature. After unblocking, the phenol volatiles are too toxic and cannot be used as fabric finishing crosslinking agents. Summary of the invention

[0006] In view of the problems of poor waterproofing synergy and curing performance caused by factors such as the presence of VOC, unstable water dispersibility, low adhesion and peel strength to fibers, low unblocking and crosslinking efficiency, etc. in the blocked polyisocyanate emulsion used in the prior art to improve the performance of waterproof agents, the purpose of the present invention is to provide a water-dispersible emulsion of cardanol blocked polyisocyanate that is free of VOC, has good water dispersion stability, and has high adhesion and peel strength to fibers to solve the existing problems.

[0007] To achieve the above object, the present invention provides the following technical solutions: In a first aspect, the present invention provides a method for preparing a cardanol-blocked polyisocyanate emulsion, comprising the following steps:

[0008] (1) Under nitrogen protection, at 35-65° C. and with mechanical stirring, 200.0 g of diisocyanate is subjected to addition condensation under the action of 0.5-2.0 g of alkaline ionic liquid catalyst. After 3 hours, the NCO mass percentage of the system is measured. When the conversion rate reaches 30-50%, an acid terminator in an amount equal to the molar number of the alkaline ionic liquid catalyst is added to terminate the condensation reaction, the temperature is lowered, solid impurities are removed by filtration, and unreacted monomers are removed by molecular distillation to obtain polyisocyanate;

[0009] (2) 40.0 g of the polyisocyanate obtained in step (1) was added to a reaction kettle. Under nitrogen protection, a temperature of 50-90° C. and mechanical stirring, an internal emulsifier and 2-3 drops of a catalyst, bismuth neodecanoate, were first added to partially block the NCO in the polyisocyanate. The blocking rate was controlled to 8%-18% by adjusting the amount of the internal emulsifier added. Cardanol was then added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., a cardanol-blocked polyisocyanate;

[0010] (3) At room temperature, 40.0 g of the cardanol-blocked polyisocyanate prepared in step (2), 2.0-6.0 g of an external emulsifier, and 2.0 g of glacial acetic acid were uniformly mixed, and water at the same temperature was slowly added thereto. The mixture was emulsified by a phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion having a mass percentage concentration of 35%-45%.

[0011] Furthermore, in step (1), the diisocyanate is selected from one or more of aliphatic diisocyanates and cycloaliphatic diisocyanates.

[0012] Furthermore, the diisocyanate is selected from one or more of isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), and 4,4'-dicyclohexylmethane diisocyanate (HMDI).

[0013] Furthermore, in the step (1), the average molecular functionality of the polyisocyanate is greater than 3.3 and less than 4.5.

[0014] Considering the performance and raw material cost, the diisocyanate is 1,6-hexamethylene diisocyanate, which is provided by Wanhua Chemical Group Co., Ltd.

[0015] Polyisocyanates mainly include dimers, trimers, adducts of polyols and diisocyanates, adducts of modified castor oil and diisocyanates, etc. From the perspective of cost and waterproof finishing applications, it is better to use trimer blockers as waterproof crosslinking agents. Trimers can be trimers of a single diisocyanate or trimers of two different diisocyanates. Among them, the most commonly used is HDI (1,6-hexamethylene diisocyanate) trimer. HDI trimer has the characteristics of low viscosity, low chroma, low vapor pressure, yellowing resistance, high thermal stability (isocyanurate ring), anti-bacterial and corrosion resistance.

[0016] HDI reacts at a certain temperature in the presence of a trimer catalyst. When the desired conversion rate is reached, a terminator is added to deactivate the catalyst, and the free monomer is removed under reduced pressure to obtain a trimer containing an isocyanate heterocyclic structure. For example, in the HDI trimer product synthesized using a quaternary ammonium base (an important catalyst for HDI trimerization) as a catalyst, the mass fractions of trimer, polymer, dimer and HDI monomer in the product are 62%~64%, 29%~31%, 2%~3% and 2%~3%, respectively. Therefore, the structure and properties of the HDI trimer product mainly depend on the catalyst.

[0017] Furthermore, the alkaline ionic liquid catalyst in step (1) is an imidazole-based ionic liquid, and the chemical structure is shown in formula (I); (I); In formula (I), there are two substituents on the imidazolium cation group, R1=C n H 2n-1, n = 1, 2; R2 = C m H 2m-1 , 1 < m < 10; anion A - is 2-(carbamoyl)-benzoate (CAB) or phthalimide-N-oxyl anion (PIO); wherein, the structural formula of 2-(carbamoyl)-benzoate is: ; the structural formula of phthalimide-N-oxyl anion is: .

[0018] Furthermore, for the two substituents on the imidazole cation group in the basic ionic liquid catalyst, n = 1 in R1 and m = 2, 4 in R2.

[0019] Ionic Liquids (IL for short) is a new type of "green solvent". It is a salt compound composed of organic cations and inorganic / organic anions and is in a liquid state at room temperature or near room temperature. Ionic liquids have excellent physical and chemical characteristics, such as no vapor pressure at room temperature, good thermal stability and conductivity, and can be recycled and reused, etc., and are widely used in fields such as synthesis, analysis, catalysis and separation.

[0020] The present invention uses imidazolium ionic liquid as the HDI trimerization catalyst, which is based on the molecular interaction between the aromatic imidazole ring (electron-donating) and the six-membered cyanuric acid ring of the HDI trimer (electron-withdrawing) and the basicity brought by the tertiary amine formed by another N of the imidazole ring.

[0021] The described basic ionic liquid catalyst is prepared in the laboratory, and the specific preparation method is as follows: The preparation method of [1-butyl-3-methylimidazole][PIO] is: In a 100 mL three-necked round-bottom flask equipped with a reflux condenser, magnetic stirring and a thermometer, add 3.14 g of N-hydroxyphthalimide (98%, CAS: 524-38-9, Macklin reagent) and 13.1 g of an ethanol solution of 1-butyl-3-methylimidazole hydroxide (22.5%, CAS: 528818-81-7, Macklin reagent), stir at room temperature for 5 min, then add 30 mL of absolute ethanol, heat up to 70 °C and keep the reaction for 30 min, cool to room temperature, precipitate red-brown crystals, filter under reduced pressure, collect the red-brown crystals, and after vacuum drying, obtain the ionic liquid catalyst.

[0022] The preparation method of [1-butyl-3-methylimidazole][CAB] is as follows: in a 100 mL three-necked round-bottom flask equipped with a reflux condenser, a magnetic stirrer and a thermometer, 2.83 g of phthalimide (98%, CAS: 85-41-6, MacLean's reagent) and 13.1 g of an ethanol solution of 1-butyl-3-methylimidazole hydroxide (22.5%, CAS: 528818-81-7, MacLean's reagent) are added, stirred at room temperature for 5 minutes, and then 15 mL of deionized water is added, the temperature is raised to 80° C. and the reaction is kept for 6 hours. After cooling, the volatile substances are removed by a rotary evaporator, and the obtained yellow viscous liquid is placed in an environment of 0-5° C. for natural crystallization, and the white crystals are collected by vacuum filtration. After vacuum drying, an ionic liquid catalyst is obtained.

[0023] Furthermore, in step (1), the acid terminator is selected from one or more of diethyl sulfate, methyl p-toluenesulfonate, and phosphoric acid.

[0024] The cardanol-blocked polyisocyanate emulsion prepared by the present invention is used as a crosslinking agent in fabric finishing, which is safe and non-toxic. The cardanol-blocked polyisocyanate emulsion of the present invention has a phenolic hydroxyl group on the benzene ring of the cardanol, and the benzene ring of the cardanol also has a C15 long-chain alkyl group, which has a large steric hindrance, has the characteristics of low viscosity and strong hydrophobicity. Thermal analysis shows that the unblocking temperature of the cardanol-blocked isocyanate prepared by the present invention is 120-150° C. The cardanol polyisocyanate blocker prepared by the present invention has strong hydrophobicity, low melting point and viscosity, but high cohesive energy and strong adhesion, which can improve the adhesion and film-forming flexibility of waterproof polymer particles on fibers; the cardanol polyisocyanate blocker is essentially that the active isocyanate (-NCO) functional group is temporarily blocked by the cardanol (phenolic hydroxyl group), and the active isocyanate is released by heat treatment and baking, and cross-linking and curing occur, so as to achieve the purpose of durable waterproof performance, improve the performance of friction or repeated washing, and maintain the texture of the fabric to avoid the poor appearance of white marks.

[0025] Furthermore, in step (2), the structure of cardanol is as shown in formula (II), wherein n=0, 1, 2 or 3; (II).

[0026] Furthermore, in step (2), the cardanol is selected from one or more of cardanol NX-2026, cardanol NX-2025, and cardanol NX-2023, all of which are purchased from Cardolite Corporation.

[0027] From the composition point of view, cardanol NX-2026, cardanol NX-2025, and cardanol NX-2023 are all mixtures: the side chain can be a monoene, a diene, or a triene. The main components of cardanol NX-2026, cardanol NX-2025, and cardanol NX-2023 are shown in formula (III): (III).

[0028] Formula (III) indicates that the main components of the three types of cardanols are cardanols with a diene structure as the side group, and the content thereof is greater than or equal to 96%. From the perspective of physicochemical properties, cardanol NX-2026, cardanol NX-2025, and cardanol NX-2023 are all low-viscosity fluids at room temperature, and are reddish brown or yellowish brown in color. The cardanol polyisocyanate blocker prepared by the three types of cardanols produced by Cardolite Company in the present invention can be compounded with a waterproofing agent to improve the wearing performance of the fabric after waterproofing.

[0029] In order to facilitate the application in the finishing process, the blocked polyisocyanate must be made into a water dispersion with small particle size and narrow distribution by an appropriate emulsification process. The type and amount of the blocking agent of the polyisocyanate, the type and amount of the internal and external emulsifiers, the emulsification temperature, the emulsification method, the pH value and other parameters all have an important influence on the particle size and distribution of the emulsion, thereby ensuring the stability of the product storage and application performance.

[0030] Furthermore, in step (2), the internal emulsifier is polyethylene glycol monomethyl ether (MPEG).

[0031] Furthermore, the polyethylene glycol monomethyl ether is selected from one or more of MPEG-350 (average molecular weight 350 g / mol), MPEG-550, and MPEG-750, all of which are provided by Jiangsu Haian Petrochemical Plant. Furthermore, in step (3), the external emulsifier is selected from a nonionic surfactant.

[0032] Furthermore, the HLB value of the external emulsifier in step (3) is 14-16.

[0033] Furthermore, the external emulsifier is selected from one or more of Peregal O-20, AEO-15, Tween-80, and E-1340 (isomeric tridecanol polyoxyethylene ether), all of which are provided by Jiangsu Haian Petrochemical Plant.

[0034] In a second aspect, the present invention provides a cardanol-blocked polyisocyanate emulsion prepared by the above-mentioned preparation method.

[0035] In a third aspect, the present invention also provides the use of the cardanol-blocked polyisocyanate emulsion in waterproof finishing of textiles.

[0036] Furthermore, the cardanol-blocked polyisocyanate emulsion is used for waterproof finishing of textiles containing fluorine-containing waterproofing agents or fluorine-free waterproofing agents.

[0037] Furthermore, the fluorine-containing waterproofing agent is a C6 fluorine waterproofing agent.

[0038] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0039] (1) The present invention uses alkaline ionic liquid to catalyze the nucleophilic addition condensation of diisocyanate to produce trimer. The characteristic is that the low-activity diisocyanate, such as HDI, has a higher trimer conversion rate at a lower temperature, which is beneficial to the blocking reaction and emulsification processing, and it is easier to obtain a stable nano-scale water dispersion, and improve its adhesion to fabric fibers and affinity for waterproofing agent particles. Compared with existing quaternary ammonium salt catalysts, it has the characteristics of low melting point and viscosity, reusability, low reaction temperature, controllable rate, low polymer content in the product, narrow molecular weight distribution, and low viscosity, which is beneficial to subsequent blocking and emulsification, and it is particularly easy to obtain a nano-scale water dispersion. When used together with a waterproofing agent, it significantly improves the waterproof grade and durability of the fabric;

[0040] (2) The cardanol-blocked polyisocyanate emulsion prepared by the present invention is a waterproof synergistic curing agent. When used in the finishing process of C6 fluorine waterproofing agent fabric, the C6 fluorine waterproofing agent can achieve the waterproof and oil-proof performance and durability of C8 fluorine waterproofing agent at a lower dosage, thereby reducing the harm of C6 fluorine to the environment; when used in the finishing process of fluorine-free waterproofing agent fabric, the dosage of waterproofing agent can be reduced to achieve a high waterproof grade and durability, thereby saving resources and costs;

[0041] (3) Compared with the existing commercial blocked polyisocyanate emulsion (micron-scale water dispersion), the cardanol-blocked polyisocyanate emulsion prepared by the present invention is a nano-scale water dispersion, the colloid particles are positively charged in water, the particle charge density is higher, the surface energy is higher, the diffusion and penetration are stronger, and the conventional fiber (negatively charged on the surface in water) has better adhesion, and can penetrate into the fabric and yarn faster. Therefore, when used for fabric waterproof finishing (fluorine-containing and fluorine-free), the nano-colloid particles have strong adsorption on the waterproofing agent particles in the working liquid; during padding, the adsorption amount of the waterproofing agent on the fabric is increased; during heat treatment, since the blocker, the waterproofing agent and the fiber are distributed and combined at the nanometer level, as long as the cardanol is unblocked from the polyisocyanate blocker, the curing and cross-linking reaction can occur. Therefore, after the heat treatment is completed, the waterproofing agent molecules (such as C18 long chains) on the fiber are regularly arranged, and the roughness of the fiber surface is greater. The cardanol of the present invention can be inserted into the amorphous area formed by the waterproofing agent molecules to soften the film. The technical solution proposed by the present invention can not only solve the problem that the existing waterproofing agent (C6 and fluorine-free) has a high dosage and a short effect, but also effectively solve the problem that the textiles in the prior art have a hard feel and white marks (hand scratches) on the fabric surface;

[0042] (4) The diisocyanate, cardanol, internal emulsifier and external emulsifier used in the present invention are all derived from bio-based materials, the catalyst does not contain toxic heavy metal elements, and the product is green and environmentally friendly. The preparation method and product proposed in the present invention do not use any non-aqueous solvents, have no VOC emissions, and do not contain alkylphenol polyoxyethylene ether compounds (APEO) and phosphorus chemicals, which ensures the production and application of the waterproof synergistic curing agent and the ecological and environmental protection of textiles;

[0043] (5) The preparation method of the present invention is simple and easy to operate. The synthesis and emulsification of polyisocyanate and cardanol blocked polyisocyanate belong to conventional preparation methods and can be produced on a large scale. The product cost is low, which is conducive to large-scale production and use. DETAILED DESCRIPTION

[0044] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0046] The preparation method of the catalyst used in the following examples is as follows: The preparation method of [1-butyl-3-methylimidazole][PIO] is as follows: In a 100mL three-necked round-bottom flask equipped with a reflux condenser, a magnetic stirrer and a thermometer, 3.14g of N-hydroxyphthalimide (98%, CAS: 524-38-9, MacLean's reagent) and 13.1g of an ethanol solution of 1-butyl-3-methylimidazole hydroxide (22.5%, CAS: 528818-81-7, MacLean's reagent) were added and stirred at room temperature for 5 minutes, and then 30mL of anhydrous ethanol was added, the temperature was raised to 70°C and the reaction was kept warm for 30 minutes, and then cooled to room temperature to precipitate reddish-brown crystals, and the reddish-brown crystals were collected by vacuum filtration and vacuum drying to obtain an ionic liquid catalyst.

[0047] The preparation method of [1-butyl-3-methylimidazole][CAB] is as follows: in a 100 mL three-necked round-bottom flask equipped with a reflux condenser, a magnetic stirrer and a thermometer, 2.83 g of phthalimide (98%, CAS: 85-41-6, MacLean's reagent) and 13.1 g of an ethanol solution of 1-butyl-3-methylimidazole hydroxide (22.5%, CAS: 528818-81-7, MacLean's reagent) are added, stirred at room temperature for 5 minutes, and then 15 mL of deionized water is added, the temperature is raised to 80° C. and the reaction is kept for 6 hours. After cooling, the volatile substances are removed by a rotary evaporator, and the obtained yellow viscous liquid is placed in an environment of 0-5° C. for natural crystallization, and the white crystals are collected by vacuum filtration. After vacuum drying, an ionic liquid catalyst is obtained.

[0048] Example 1

[0049] This embodiment provides a cardanol-blocked polyisocyanate emulsion, and the preparation method thereof comprises the following steps:

[0050] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.8g alkaline ionic liquid [1-methyl-3-ethylimidazole] [CAB] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 30%, 1.0g diethyl sulfate was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by molecular distillation to obtain polyisocyanate. The test showed that the number average molecular weight of the polyisocyanate was 620 and the NCO mass percentage was 23.4%;

[0051] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 14.0 g of MPEG-350 (average molecular weight of 350 g / mol) was first added to partially block the NCO in the polyisocyanate. When the blocking rate reached 17.95%, 57.9 g of cardanol NX-2026 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0052] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 4.0 g of external emulsifier O-20, and 2.0 g of glacial acetic acid were mixed evenly, and 54.0 g of water at the same temperature was slowly added. The mixture was emulsified by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0053] Example 2

[0054] This embodiment provides a cardanol blocked polyisocyanate emulsion, and the preparation method thereof comprises the following steps:

[0055] (1) Under nitrogen protection, at 35°C and with mechanical stirring, 200.0g of IPDI was subjected to addition condensation with 2.0g of alkaline ionic liquid [1-methyl-3-butylimidazole][CAB] as a catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 50%, 0.5g of diethyl sulfate and 0.38g of phosphoric acid were immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were removed by filtration, and unreacted monomers were removed by molecular distillation to obtain polyisocyanate. The test showed that the number average molecular weight of the polyisocyanate was 760 and the NCO mass percentage was 18.3%;

[0056] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 90°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 10.5 g of MPEG-750 (average molecular weight of 750 g / mol) was first added to block the NCO part of the polyisocyanate. When the blocking rate reached 8.0%, 51.0 g of cardanol NX-2026 was added to block all the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0057] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 1.0 g of external emulsifiers AEO-15 and O-20, and 2.0 g of glacial acetic acid were mixed evenly, and then 60.0 g of water at the same temperature was slowly added thereto for emulsification by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 35%.

[0058] Example 3

[0059] This embodiment provides a cardanol blocked polyisocyanate emulsion, and the preparation method thereof comprises the following steps:

[0060] (1) Under nitrogen protection, at 65°C and mechanical stirring, 200.0g HMDI was subjected to addition condensation under the action of 0.5g alkaline ionic liquid [1-methyl-3-ethylimidazole] [PIO] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 40%, 0.14g diethyl sulfate and 0.17g methyl p-toluenesulfonate were immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by molecular distillation to obtain polyisocyanate. The test showed that the number average molecular weight of the polyisocyanate was 830 and the NCO mass percentage was 15.2%;

[0061] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 50°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 10.0 g of MPEG-550 (average molecular weight of 550 g / mol) was first added to partially block the NCO in the polyisocyanate. When the blocking rate reached 12.56%, 40.0 g of cardanol NX-2023 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0062] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 6.0 g of external emulsifier Tween-80, and 2.0 g of glacial acetic acid were mixed evenly, and then 41.0 g of water at the same temperature was slowly added thereto for emulsification by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 45%.

[0063] Example 4

[0064] This embodiment provides a cardanol blocked polyisocyanate emulsion, and the preparation method thereof comprises the following steps:

[0065] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.6g alkaline ionic liquid [1-methyl-3-butylimidazole] [PIO] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 45%, 1.0g methyl p-toluenesulfonate was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by molecular distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 630 and the NCO mass percentage was 22.8%;

[0066] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 12.0 g of MPEG-550 (average molecular weight of 550 g / mol) was first added to block the NCO part of the polyisocyanate. When the blocking rate reached 15.79%, 22.0 g of cardanol NX-2026 and 35.0 g of cardanol NX-2023 were added to block all the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0067] (3) At room temperature, 40 g of the cardanol-blocked polyisocyanate, 13405.0 g of the external emulsifier, and 2.0 g of glacial acetic acid in (2) were mixed evenly, and then 53.0 g of water at the same temperature was slowly added thereto for emulsification by a phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0068] Example 5

[0069] This embodiment provides a cardanol blocked polyisocyanate emulsion, and the preparation method thereof comprises the following steps:

[0070] (1) Under nitrogen protection, at 40°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.0g alkaline ionic liquid [1-methyl-3-ethylimidazole] [CAB] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 40%, 0.42g phosphoric acid was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by molecular distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 620 and the NCO mass percentage was 23.2%;

[0071] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 70°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 12.0 g of MPEG-550 (average molecular weight of 550 g / mol) was first added to block the NCO part of the polyisocyanate. When the blocking rate reached 15.52%, 24.0 g of cardanol NX-2025 and 35.0 g of cardanol NX-2026 were added to block all the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0072] (3) At room temperature, 40 g of the cardanol-blocked polyisocyanate in (2), 3.0 g of the external emulsifier AEO-15, and 2.0 g of glacial acetic acid were mixed evenly, and then 55.0 g of water at the same temperature was slowly added thereto for emulsification by a phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0073] Example 6

[0074] This embodiment provides a cardanol blocked polyisocyanate emulsion, and the preparation method thereof comprises the following steps:

[0075] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.0g alkaline ionic liquid [1-methyl-3-ethylimidazole] [CAB] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 40%, 0.42g phosphoric acid was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by molecular distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 620 and the NCO mass percentage was 23.2%;

[0076] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 14.0 g of MPEG-750 (average molecular weight of 750 g / mol) was first added to partially block the NCO in the polyisocyanate. When the blocking rate reached 11.31%, 63.0 g of cardanol NX-2026 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate.

[0077] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 6.0 g of external emulsifier Tween-80, and 2.0 g of glacial acetic acid were mixed evenly, and then 52.0 g of water at the same temperature was slowly added thereto for emulsification by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0078] Among them, the toluene-di-n-butylamine titration method is used to test the -NCO content of the polyisocyanate system in the embodiment of the present invention, and HG / T2409-1992 "Determination of the content of isocyanate groups in polyurethane prepolymers" is used as a reference. The molecular weight of polyisocyanates is tested by gel permeation chromatography (GPC) method (instrument: waters1515 gel permeation chromatograph, carrier gas: tetrahydrofuran, flow rate: 0.6mL / min, sample concentration: 1.0wt.%, injection volume: 20μL, temperature: 40°C, detection method: differential refractometer). The method for testing the complete closure of -NCO in the closed system: take 1-2 drops of the product, add it to 10mL acetone to dissolve, then add a few drops of aniline and shake it. If precipitation or turbidity is observed, it indicates that it is not completely closed, otherwise it is completely closed. Phase inversion emulsification is to first dissolve the emulsifier in the oil and heat it into a liquid, then slowly add warm water while stirring vigorously. The added water begins to disperse in the oil in the form of fine particles, forming a W / O type; as water continues to be added, the emulsion becomes thinner, and finally the viscosity drops sharply, and the phase turns into an O / W emulsion, which is an emulsification method.

[0079] Comparative Example 1

[0080] This comparative example provides a cardanol-blocked polyisocyanate emulsion, and a preparation method thereof, comprising the following steps:

[0081] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation with 1.8g conventional catalyst tetramethylammonium n-octanoate. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 30%, 1.28g diethyl sulfate was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by reduced pressure distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 790 and the NCO mass percentage was 20.9%;

[0082] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-necked reactor. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 12.5 g of MPEG-350 (average molecular weight of 350 g / mol) was first added to partially block the NCO in the polyisocyanate. When the blocking rate reached 17.94%, 51.5 g of cardanol NX-2026 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0083] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 4.0 g of external emulsifier O-20, and 2.0 g of glacial acetic acid were mixed evenly, and then 54.0 g of water at the same temperature was slowly added thereto for emulsification by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0084] Comparative Example 2

[0085] This comparative example provides a cardanol-blocked polyisocyanate emulsion, and its preparation method comprises the following steps:

[0086] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.8g alkaline ionic liquid [1-methyl-3-ethylimidazole] [CAB] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 60%, 1.0g diethyl sulfate was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by reduced pressure distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 940 and the NCO mass percentage was 19.8%;

[0087] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 11.9 g of MPEG-350 (average molecular weight of 350 g / mol) was first added to partially block the NCO in the polyisocyanate. When the blocking rate reached 18.02%, 48.71 g of cardanol NX-2026 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0088] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 4.0 g of external emulsifier O-20, and 2.0 g of glacial acetic acid were mixed evenly, and then 54.0 g of water at the same temperature was slowly added thereto for emulsification by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0089] Comparative Example 3

[0090] This comparative example provides a cardanol-blocked polyisocyanate emulsion, and its preparation method comprises the following steps:

[0091] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.8g alkaline ionic liquid [1-methyl-3-ethylimidazole] [CAB] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 40%, 1.0g diethyl sulfate was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by reduced pressure distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 620 and the NCO mass percentage was 23.4%;

[0092] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 22.0 g of MPEG-350 (average molecular weight of 350 g / mol) was first added to partially block the NCO in the polyisocyanate. When the blocking rate reached 28.2%, 50.5 g of cardanol NX-2026 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0093] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 4.0 g of external emulsifier O-20, and 2.0 g of glacial acetic acid were mixed evenly, and then 54.0 g of water at the same temperature was slowly added thereto for emulsification by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0094] Comparative Example 4

[0095] This comparative example provides a cardanol-blocked polyisocyanate emulsion, and its preparation method comprises the following steps:

[0096] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.8g alkaline ionic liquid [1-methyl-3-ethylimidazole] [CAB] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 40%, 1.0g diethyl sulfate was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by reduced pressure distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 620 and the NCO mass percentage was 23.4%;

[0097] (2) 40.0 g of the product polyisocyanate of (1) was placed in a three-mouth reaction kettle. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst, and 70.7 g of cardanol NX-2026 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0098] (3) At room temperature, 40 g of the product of cardanol-blocked polyisocyanate in (2), 4.0 g of external emulsifier O-20, and 2.0 g of glacial acetic acid were mixed evenly, and then 54.0 g of water at the same temperature was slowly added thereto for emulsification by phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion with a mass percentage concentration of 40%.

[0099] Comparative Example 5

[0100] This embodiment provides a cardanol-blocked polyisocyanate emulsion, and the preparation method thereof comprises the following steps:

[0101] (1) Under nitrogen protection, at 60°C and mechanical stirring, 200.0g HDI was subjected to addition condensation under the action of 1.8g alkaline ionic liquid [1-methyl-3-ethylimidazole] [CAB] catalyst. After 3 hours, the NCO mass percentage of the system was measured. When the conversion rate reached 40%, 1.0g diethyl sulfate was immediately added to terminate the condensation reaction, the temperature was lowered, solid impurities were filtered out, and unreacted monomers were removed by reduced pressure distillation to obtain polyisocyanate. The test showed that the average molecular weight of the polyisocyanate was 620 and the NCO mass percentage was 23.4%;

[0102] (2) 40.0 g of the product polyisocyanate of (1) was added to a three-mouth reaction kettle. Under nitrogen protection, temperature of 80°C and mechanical stirring, 2 drops of bismuth neodecanoate were used as a catalyst. 14.0 g of MPEG-350 (average molecular weight of 350 g / mol) was first added to partially block the NCO in the polyisocyanate. When the blocking rate reached 17.9%, 57.9 g of cardanol NX-2026 was added to completely block the remaining NCO in the polyisocyanate. The temperature was lowered and the material was discharged to obtain a light yellow transparent viscous liquid, i.e., cardanol-blocked polyisocyanate;

[0103] (3) At room temperature, 40 g of the cardanol-blocked polyisocyanate product of (2) and 2.0 g of glacial acetic acid were mixed evenly, and then 58.0 g of water at the same temperature was slowly added thereto for emulsification by a phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion having a mass percentage concentration of 40%.

[0104] Comparative Example 6

[0105] Cross-linking agent: RUCO-GUARDXCR (blocked polyisocyanate emulsion) (provided by Rudolf Chemical Co., Ltd., Germany).

[0106] Comparative Example 7

[0107] Crosslinking agent: PHOBOLXAN (blocked oxime isocyanate dispersion) (provided by Huntsman Group Textile Chemicals Division).

[0108] Performance Testing

[0109] 1. The following properties of the cardanol-blocked polyisocyanate emulsions prepared in Examples 1 to 6 and the products of Comparative Examples 1 to 7 were measured, and the results are shown in Table 1. (1) Emulsion particle size d50: tested according to the national standard "GB / T19077-2016 Particle size distribution laser diffraction method"; (2) Centrifugal stability: tested according to the industry standard "HG / T4737-2014 Determination of centrifugal stability of liquid products of textile dyeing and finishing auxiliaries"; (3) Normal temperature stability: the same mass of waterproofing agents were placed at room temperature (25°C) for 3 months, and the appearance of the waterproofing agents was observed. (4) Film strength: first coated on a polypropylene plate, and after it did not flow, cured at 150°C*30min to form a film, and the tensile strength of the cured film was tested using a universal strength tester (WDW-20KW). Test conditions: tensile speed: 20mm / min, sample size: 20mm (length)*10mm (width)*20-40μm, temperature 25°C, humidity: 50%.

[0110] 2. The cardanol-blocked polyisocyanate emulsions prepared in Examples 1 to 6 and the products of Comparative Examples 1 to 7 were applied to 32 s Cotton double jersey (150g / m 2) was waterproofed, and the results are shown in Table 2. (1) The waterproof performance was evaluated according to "GB / T4745-2012 Testing and Evaluation of Waterproof Performance of Textiles - Water-Impact Method"; the washing method was carried out according to "GB / T8629-2017 "Household Washing and Drying Procedure for Textile Testing"; (2) White mark test: the fabric was visually inspected after mechanical simulated hand grabbing. (3) Color difference: the unfinished fabric was used as the standard sample and the finished fabric was used as the sample. The color was measured by spectrophotometry and the color difference (dECMC(2:1)) was calculated.

[0111] Process flow: prepare working liquid → dip fabric into working liquid → dry fabric → bake fabric → finished product. Details are as follows:

[0112] 1) Prepare working fluid: waterproofing agent RUCO-DRYECOplus 50 g / L (based on hyperbranched dendritic macromolecular compounds and hydrocarbon polymers, provided by Rudolf Chemical Co., Ltd., Germany), cross-linking agent (cardanol-blocked polyisocyanate emulsions of Examples 1 to 6 and products of Comparative Examples 1 to 7): 5 g / L;

[0113] 2) Padding working fluid: rolling rate 75%;

[0114] 3) Drying: The impregnated fabric is dried at 80°C;

[0115] 4) Baking: The dried fabric is heat treated at 150°C for 3 minutes.

[0116]

[0117] As can be seen from Table 1, the cardanol-blocked polyisocyanate emulsions prepared in Examples 1-6 have a particle size d50 of 80-100 nm, and have excellent comprehensive properties such as stability and film strength.

[0118] However, the comparative examples are obviously inferior to the embodiments in the corresponding performance tests because they do not adopt the necessary technical solutions. Comparative Example 1 uses conventional catalysts to condense trimers, and Comparative Example 2 has a high degree of isocyanate condensation, which will make the amount of polymers too high, the particle size of the emulsion larger, the stability worse, and the strength of the film slightly reduced. In Comparative Example 3, there is an excess of MPEG, the product is too water-based, the adhesion is poor, the sealing is insufficient, and the cross-linking synergistic effect of the waterproofing agent is poor. In the present invention, too little MPEG will make the product poor in dispersibility. During heat treatment, the polyisocyanate emulsion blocked by cardanol and the waterproofing agent molecules will undergo microphase separation, resulting in poor curing synergistic ability of waterproofing. Comparative Example 4 only uses cardanol for blocking, and Comparative Example 5 does not add an emulsifier. The above two methods result in products with either too small particle size (but poor coating strength) or too large particle size (poor stability and poor coating strength). The external emulsifier of the present invention plays a dispersing role. At the same time, the HLB value of the external emulsifier is within a certain range, which is conducive to increasing the hydration layer outside the latex particles and improving the stability of nano-dispersion. If the HLB value is too low, the dispersibility is too poor. If the HLB value is too high, the binding force with the colloid particles is too poor, and the hydrophilicity is too strong, which will affect the waterproof effect of the fabric. Comparative Examples 6 and 7 are two external samples, respectively. The structure of the closed product is unknown, the coating strength is high (the cross-linking density is large), the emulsion particle size is large, the storage stability is not high, and they contain a large amount of solvent, which is closely related to the fact that the trimer raw material used has more polymers, the internal emulsifier is not used in the closed process, the space of the sealing agent is small, and the HLB of the external emulsifier is too small or too large. The use of a large amount of solvent can improve stability, but it will cause environmental damage. As the solvent evaporates, the emulsion will produce a large amount of precipitation.

[0119] As can be seen from Table 2, after finishing, the white marks (hand scratches) of the fabrics are compared. Examples 1-6 have no white marks, while Comparative Examples 1-7 have slight white marks, which shows that the nano-scale cardanol-blocked polyisocyanate emulsion is conducive to eliminating white marks. White marks will appear if the cross-linking density is too large or insufficient. The color change effect of the finishing of Examples 1-6 on the fabric is less than that of Comparative Examples 1-7. The comparison of the waterproof performance of the fabrics is as follows: the waterproof performance of Examples 1-6 before washing is higher than that of Comparative Examples 1-5, reaching the level of Comparative Examples 6 and 7 (two external samples); after the fabrics have been washed 10 times at home, the durability of Examples 1-6 is equivalent to that of Comparative Examples 6 and 7, while Comparative Examples 1-5 drops from about 4-5 before washing to below 3, indicating that the polyisocyanate structure, the type and amount of the blocking agent, and the emulsification process of the blocking agent are crucial to the waterproof performance and durability of the fabric.

[0120] In the preparation method of the present invention, the structure of polyisocyanate and the structural selection and proportion of the blocking agent, internal emulsifier and external emulsifier are very critical. Aliphatic diisocyanate is condensed into trimer under the catalysis of alkaline imidazolium ionic liquid, and the conversion rate of the product is high and the side reaction is less. The use of alkaline imidazolium ionic liquid is one of the innovations of the present invention. The synthesized polyisocyanate is blocked by cardanol and a small amount of internal emulsifier polyethylene glycol monomethyl ether. The product has low viscosity, liquid state, and certain hydrophilicity, which is conducive to subsequent nano-scale emulsification and dispersion. This is the second innovation of the present invention.

[0121] Cardanol-blocked polyisocyanate emulsion has a low melting point and viscosity, but high cohesive energy and strong adhesion, which can improve the adhesion and film-forming flexibility of waterproof polymer particles on fibers, and effectively solve the problems of hard hand feeling and white marks (hand scratches) on the cloth surface in the prior art. Thermal baking unblocks the cardanol polyisocyanate blocker, allowing the waterproof agent to cross-link and fix on the fabric, and the waterproof performance is permanently enhanced. The cross-linking agent component ratio is based on the emulsion particle size, centrifugal stability, hand feel and white mark degree, and the waterproof performance of the fabric as evaluation means, and is obtained through many experiments, repeated verification and optimization. Among them, the average molecular functionality of the polyisocyanate cannot be too small, at least more than 3.3, and cannot be too large, and should be less than 4.5, otherwise the viscosity is too large, resulting in insufficient sealing and emulsification. The blocking rate of cardanol to polyisocyanate cannot be too small. If the blocking rate is too small, on the one hand, the cross-linking degree will decrease, and on the other hand, the hydrophilicity will be too strong and the adhesion will be too low, so that the waterproofing synergistic and curing effects are not obvious, and the problem of white marks cannot be solved; the blocking rate cannot be too large. If it is too large, the hydrophilicity will be too poor, and it will be difficult to obtain a nano-scale water dispersion, resulting in poor adhesion, sticking to the roller, defects on the cloth surface, and the limitations of waterproofing synergistic and curing and white marks cannot be solved. The emulsification process of cardanol-blocked polyisocyanate is also very important. The emulsification method (phase inversion method), external emulsifier HLB and dosage, emulsification temperature, and pH value play a decisive role in the formation of a stable nano-scale water dispersion. If the emulsifier HLB is unreasonable, the particle size is too large, the waterproof grade is reduced, and if the emulsifier is used too much, there are too many film defects on the fiber, and the waterproof grade deteriorates.

[0122] In addition, the temperature and reaction time in the preparation method are also very critical; if the temperature is too low, it is not conducive to the diffusion and activity of isocyanate; if the temperature is too high, the activity of isocyanate is too high, resulting in more side reactions and even explosion; if the reaction time is too long, the product will degrade and the crosslinking will be reduced; if the reaction time is too short, the conversion rate is not high, which will also reduce the crosslinking.

[0123] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the specification of the present invention under the concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a cardanol-blocked polyisocyanate emulsion, characterized in that: The preparation method comprises the following steps: (1) Under nitrogen protection, at 35-65° C. and with mechanical stirring, 200.0 g of diisocyanate is subjected to addition condensation under the action of 0.5-2.0 g of alkaline ionic liquid catalyst. After 3 hours, the NCO mass percentage of the system is measured. When the conversion rate reaches 30-50%, an acid terminator in an amount equal to the molar number of the alkaline ionic liquid catalyst is added to terminate the condensation reaction, the temperature is lowered, solid impurities are removed by filtration, and unreacted monomers are removed by molecular distillation to obtain polyisocyanate; (2) 40.0 g of the polyisocyanate obtained in step (1) is added to a reaction kettle, and under nitrogen protection, a temperature of 50-90° C. and mechanical stirring, an internal emulsifier and 2-3 drops of catalyst bismuth neodecanoate are first added to partially block the NCO in the polyisocyanate, and the blocking rate is controlled to 8%-18% by adjusting the amount of the internal emulsifier added, and then cardanol is added to completely block the remaining NCO in the polyisocyanate, and the temperature is lowered and the material is discharged to obtain a light yellow transparent viscous liquid, i.e., a cardanol-blocked polyisocyanate; the internal emulsifier in step (2) is polyethylene glycol monomethyl ether; (3) At room temperature, 40.0 g of the cardanol-blocked polyisocyanate prepared in step (2), 2.0-6.0 g of an external emulsifier, and 2.0 g of glacial acetic acid were uniformly mixed, and water at the same temperature was slowly added thereto. The mixture was emulsified by a phase inversion method to obtain a cardanol-blocked polyisocyanate emulsion having a mass percentage concentration of 35%-45%; The alkaline ionic liquid catalyst in step (1) is an imidazolyl ionic liquid, the chemical structure of which is shown in formula (I); (I); In formula (I), for the two substituents on the imidazolium cation group, R1 = C n H 2n-1 , n = 1, 2; R2 = C m H 2m-1 , 1 < m < 10; the anion A - is selected from 2-(carbamoyl)-benzoate or phthalimide-N-oxyanion; The structural formula of 2-(carbamoyl)-benzoate is: ; The structural formula of phthalimide-N-oxide anion is: .

2. The method for preparing a cardanol-blocked polyisocyanate emulsion according to claim 1, wherein: In the step (1), the diisocyanate is selected from aliphatic diisocyanates.

3. The method for preparing the cardanol-blocked polyisocyanate emulsion according to claim 2, wherein: The diisocyanate is selected from one or more of isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.

4. The method for preparing the cardanol-blocked polyisocyanate emulsion according to claim 1, characterized in that: The structure of cardanol in step (2) is shown in formula (II), where n=0, 1, 2 or 3; (Ⅱ)。 5. The method for preparing the cardanol-blocked polyisocyanate emulsion according to claim 1, characterized in that: In the step (3), the external emulsifier is a nonionic surfactant.

6. The method for preparing the cardanol-blocked polyisocyanate emulsion according to claim 5, characterized in that: The HLB value of the external emulsifier in step (3) is 14-16.

7. A cardanol-blocked polyisocyanate emulsion prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the cardanol-blocked polyisocyanate emulsion according to claim 7 in waterproof finishing of textiles.