Method for improving cycle performance of high-surface-load all-solid-state battery cell
By using composite electrolyte and solvent mixing ball milling technology of halide electrolyte and sulfide electrolyte in solid-state batteries, the problem of poor dispersion of electrolyte particles in solid-state batteries is solved, and the cycle performance and conductivity of the battery core are improved, making it suitable for large-capacity battery applications. .
Patent Information
- Application Number
- CN202410767524.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-29
AI Technical Summary
Existing solid-state batteries have large battery internal resistance and poor electrolyte particle dispersion, which affects the cell cycle performance. Especially in large-area capacity cathodes, the ion conductivity and particle size are insufficiently matched, resulting in poor cell cycle performance.
Using a composite electrolyte of halide electrolyte and sulfide electrolyte, through the mixing of non-polar and polar solvents and ball milling technology, the dispersion of electrolyte particles and the ionic conductivity of the composite cathode are improved to prepare a product with excellent voltage polarization and cycle performance All-solid-state batteries.
It significantly increases the ionic conductivity of the positive electrode sheet, improves the cycle performance of the battery core, and reduces the internal resistance of the battery core. It is suitable for mass production and maintains the environmental protection and safety of the method.
Smart Images

Figure BDA0004892995550000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a method for improving the cycle performance of a high-area-load all-solid-state battery cell. Background Art
[0002] At present, solid-state batteries use non-flammable solid electrolytes to replace flammable organic liquid electrolytes, which greatly improves the safety of the battery system and achieves a simultaneous increase in energy density. In addition, solid electrolytes have low toxicity, a wide temperature adaptability range, and are non-flammable, which also greatly improves the electrochemical performance of batteries. Its application areas are constantly expanding, and the development of solid electrolytes and all-solid-state batteries has become a current research hotspot.
[0003] However, in the prior art, solid-state batteries still have large internal resistance and poor dispersion of electrolyte particles, which in turn affects the cycle performance of the battery cell. For example, the Chinese invention patent application with publication number CN117542960A discloses a composite positive electrode plate and its preparation method and application. This method uses halide additives to increase the compaction density of the positive electrode plate and improve the lithium ion conductivity of the composite positive electrode plate. However, this method simply uses halide as a composite positive electrode ion conductive additive to meet the needs of large-capacity positive electrodes (>5mAh / cm 2 The requirement for ionic conductivity and particle size matching (pole thickness > 150μm) leads to an increase in the internal pores of the composite positive electrode, which in turn increases the internal resistance of the battery cell, thereby affecting the cycle performance of the battery cell.
[0004] In addition, a Chinese invention patent with publication number CN115602914A discloses a method for preparing a sulfide solid electrolyte film. The method is to disperse the sulfide electrolyte in a non-polar solvent, n-heptane, and add a binder to form a suspension of the sulfide electrolyte. However, if the electrolyte is a mixture of a sulfide electrolyte and a halide electrolyte, the particle size of the electrolyte is usually widely distributed. The method uses a non-polar solvent alone, which will lead to poor dispersion of the electrolyte particles, affecting the ion-conducting effect of the final ion-conducting additive, and further affecting the cycle performance of the battery cell. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for improving the cycle performance of high-area-load all-solid-state battery cells, which can make the internal resistance of the battery cell lower and the dispersion of the electrolyte better, thereby improving the cycle performance of the battery cell.
[0006] In order to achieve the purpose of the above invention, the technical solution adopted by the present invention is as follows:
[0007] The present invention provides a method for improving the cycle performance of a high-area-load all-solid-state battery cell, comprising the following steps:
[0008] S1, preliminarily mixing the halide electrolyte and the sulfide electrolyte to obtain a first mixture;
[0009] S2, preliminarily mixing the non-polar solvent and the polar solvent to obtain a mixed solvent;
[0010] S3, putting the first mixture obtained in S1 into the mixed solvent obtained in S2 for ball milling;
[0011] S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture;
[0012] S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
[0013] A method for improving the cycle performance of a high-area-loaded all-solid-state battery cell of the present invention uses a halide electrolyte and a sulfide electrolyte as a composite electrolyte, so that the ionic conductivity of the positive electrode sheet is significantly improved. In addition, a non-polar solvent and a polar solvent are mixed as a mixed solvent, and the halide electrolyte and the sulfide electrolyte are mixed by wet method and ball milling, so that the dispersion of the electrolyte particles can be better. Therefore, the voltage polarization of the all-solid-state battery cell assembled by the composite positive electrode prepared by the present invention is reduced, and the cycle performance is improved.
[0014] Furthermore, the mass ratio of the halide electrolyte to the sulfide electrolyte is (0.1-3):(7-9.5). Preferably, the mass ratio of the halide electrolyte to the sulfide electrolyte is (0.5-2):(8-9.5).
[0015] Furthermore, the chemical formula of the halide electrolyte is Li a M b X c , wherein M is a metal element, including one or more of Sc, Y, La, Ho, Er, Tm, Yb, Lu, Al, Ga, In, Tl, and Fe; X is one or more of the non-metal elements F, Cl, Br, I, At, O, S, Se, and Te; wherein 0<a≤5, 0<b≤3, and 0<c≤10;
[0016] and / or
[0017] The particle size distribution of the halide electrolyte is 500nm-50μm, and the particle size of the halide electrolyte D50 is 800nm-3μm. Further preferably, the particle size of the halide electrolyte D50 is 1μm-2μm. Under the preferred particle size, the particle size matching of the halide and other materials of the positive electrode is optimal.
[0018] Furthermore, the halide electrolyte is Li3ScCl6, Li2Sc 2 / 3 Cl4、Li2In 1 / 3 Sc 1 / 3 Cl4、Li 2.25 Zr 0.75 Fe 0.25 Cl6、Li 2.7 Zr 0.3 In 0.7 One or a combination of two or more of Cl6, Li2ZrCl6, Li2ZrBr6, Li3InCl6, Li3InBr6. Further preferably, the halide electrolyte is Li3InCl6 or Li2ZrCl6.
[0019] Furthermore, the sulfide electrolyte is Li 6-i PS 5-i Q 1+i , Li 10 PcqI 12 , (100-x)Li2S-xP2S5 or a combination of two or more thereof;
[0020] Wherein, Q is one or more of the non-metallic elements F, Cl, Br, I, 1≤i≤2; Cg is one or more of the carbon group elements Si, Ge, Sn; 10≤x≤50;
[0021] and / or
[0022] The particle size distribution of the sulfide electrolyte is 500nm-50μm, and the particle size of the sulfide electrolyte D50 is 1μm-10μm. Preferably, the particle size of the sulfide electrolyte D50 is 3μm-7μm. Under the preferred particle size, the particle size matching of the sulfide and the rest of the positive electrode material is optimal.
[0023] Furthermore, the sulfide electrolyte is Li6PS5Cl.
[0024] Further, the volume ratio of the non-polar solvent to the polar solvent is 100:(1-5); preferably, the volume ratio of the non-polar solvent to the polar solvent is 100:2; and / or
[0025] The solid content of the second mixture is 50% to 70%. Preferably, the solid content of the second mixture is 55% to 58%.
[0026] Among them, within the range of the volume ratio of the non-polar solvent to the polar solvent and the solid content of the second mixture, the optimal dispersion performance of the electrolyte particles can be achieved without excessively damaging the excellent conductive properties of the solid electrolyte itself.
[0027] Further, the non-polar solvent is one or a combination of two or more of n-pentane, isopentane, cyclopentane, hexane, cyclohexane, n-heptane, isooctane, toluene, p-xylene, carbon tetrachloride or petroleum ether; and / or
[0028] The polar solvent is one or a combination of two or more of isobutanol, dichloromethane, methyl 2-bromobutyrate, butyl acetate, benzyl acetate, ethyl acetate, isopropanol, chloroform, isobutyl isobutyrate, butyl isobutyrate, pyridine, acetic acid, acetonitrile, butyl butyrate, N,N-dimethylformamide, ethylene glycol, hexyl butyrate or octyl acetate.
[0029] Furthermore, in the step S3, the first mixture obtained in S1 is put into the mixed solvent obtained in S2 and ball milling beads are added for ball milling.
[0030] Furthermore, the ball-to-material ratio of the ball mill is (1-40):1; the diameter of the ball mill beads is 1mm-20mm; the rotation speed of the ball mill is 100rpm-600rpm; and the time of the ball mill is 0.5h-6h.
[0031] Preferably, the ball-to-material ratio is (10-20):1, the ball diameter is 2 mm-5 mm, the ball speed is 300 rpm-500 rpm, and the ball milling time is 1 h-2 h. Under this ball milling parameter, sufficient mixing between electrolyte particles can be achieved, and the electrolyte particles will not be destroyed due to excessive ball milling energy.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) A method of improving the cycle performance of a high-area-loaded all-solid-state battery cell of the present invention uses a halide electrolyte and a sulfide electrolyte as a composite electrolyte, so that the ionic conductivity of the positive electrode sheet is significantly improved, and the ionic conductivity of the composite electrolyte σ≥3mS / cm. In addition, a non-polar solvent is mixed with a polar solvent as a mixed solvent, and the halide electrolyte and the sulfide electrolyte are wet mixed and ball milled to mix, which can make the electrolyte particles more dispersed and achieve full mixing of the halide electrolyte and the sulfide electrolyte. Therefore, the voltage polarization of the all-solid-state battery cell assembled with the composite positive electrode prepared by the present invention is reduced, and the cycle performance is improved.
[0034] (2) The method of the present invention for improving the cycle performance of high-area-load all-solid-state batteries has the characteristics of mild conditions, environmental protection and safety, simple method, and suitability for large-scale production. DETAILED DESCRIPTION
[0035] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0036] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said", "the", "first", "second" and "third" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0037] In an embodiment of the present invention, a method for improving the cycle performance of a high-area-load all-solid-state battery cell comprises the following steps:
[0038] S1, preliminarily mixing the halide electrolyte and the sulfide electrolyte to obtain a first mixture;
[0039] S2, preliminarily mixing the non-polar solvent and the polar solvent to obtain a mixed solvent;
[0040] S3, putting the first mixture obtained in S1 into the mixed solvent obtained in S2 for ball milling;
[0041] S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture;
[0042] S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
[0043] A method for improving the cycle performance of a high-area-loaded all-solid-state battery cell in the embodiment adopts a halide electrolyte and a sulfide electrolyte as a composite electrolyte, so that the ionic conductivity of the positive electrode sheet is significantly improved. In addition, a non-polar solvent and a polar solvent are mixed as a mixed solvent, and the halide electrolyte and the sulfide electrolyte are mixed by wet method and ball milling, so that the dispersion of the electrolyte particles can be better. Therefore, the voltage polarization of the all-solid-state battery cell assembled by the composite positive electrode prepared by the present invention is reduced, and the cycle performance is improved.
[0044] In some embodiments, the mass ratio of the halide electrolyte to the sulfide electrolyte is (0.1-3): (7-9.5). Preferably, the mass ratio of the halide electrolyte to the sulfide electrolyte is (0.5-2): (8-9.5).
[0045] In some embodiments, the chemical formula of the halide electrolyte is Li a M b Xc , wherein M is a metal element, including one or more of Sc, Y, La, Ho, Er, Tm, Yb, Lu, Al, Ga, In, Tl, and Fe; X is one or more of the non-metal elements F, Cl, Br, I, At, O, S, Se, and Te; wherein 0<a≤5, 0<b≤3, and 0<c≤10;
[0046] and / or
[0047] The particle size distribution of the halide electrolyte is 500nm-50μm, and the particle size of the halide electrolyte D50 is 800nm-3μm. Further preferably, the particle size of the halide electrolyte D50 is 1μm-2μm. Under the preferred particle size, the particle size matching of the halide and other materials of the positive electrode is optimal.
[0048] In some embodiments, the halide electrolyte is Li3ScCl6, Li2Sc 2 / 3 Cl4、Li2In 1 / 3 Sc 1 / 3 Cl4、Li 2.25 Zr 0.75 Fe 0.25 Cl6、Li 2.7 Zr 0.3 In 0.7 One or a combination of two or more of Cl6, Li2ZrCl6, Li2ZrBr6, Li3InCl6, Li3InBr6. Further preferably, the halide electrolyte is Li3InCl6 or Li2ZrCl6.
[0049] In some embodiments, the sulfide electrolyte is Li 6-i PS 5-i Q 1+i , Li 10 PcqI 12 , (100-x)Li2S-xP2S5 or a combination of two or more thereof;
[0050] Wherein, Q is one or more of the non-metallic elements F, Cl, Br, I, 1≤i≤2; Cg is one or more of the carbon group elements Si, Ge, Sn; 10≤x≤50;
[0051] and / or
[0052] The particle size distribution of the sulfide electrolyte is 500nm-50μm, and the particle size of the sulfide electrolyte D50 is 1μm-10μm. Preferably, the particle size of the sulfide electrolyte D50 is 3μm-7μm. Under the preferred particle size, the particle size matching of the sulfide and the rest of the positive electrode material is optimal.
[0053] In some embodiments, the sulfide electrolyte is Li6PS5Cl.
[0054] In some embodiments, the volume ratio of the non-polar solvent to the polar solvent is 100:(1-5); preferably, the volume ratio of the non-polar solvent to the polar solvent is 100:2; and / or
[0055] The solid content of the second mixture is 50% to 70%. Preferably, the solid content of the second mixture is 55% to 58%.
[0056] Among them, within the range of the volume ratio of the non-polar solvent to the polar solvent and the solid content of the second mixture, the optimal dispersion performance of the electrolyte particles can be achieved without excessively damaging the excellent conductive properties of the solid electrolyte itself.
[0057] In some embodiments, the non-polar solvent is one or a combination of two or more of n-pentane, isopentane, cyclopentane, hexane, cyclohexane, n-heptane, isooctane, toluene, p-xylene, carbon tetrachloride or petroleum ether; and / or
[0058] The polar solvent is one or a combination of two or more of isobutanol, dichloromethane, methyl 2-bromobutyrate, butyl acetate, benzyl acetate, ethyl acetate, isopropanol, chloroform, isobutyl isobutyrate, butyl isobutyrate, pyridine, acetic acid, acetonitrile, butyl butyrate, N,N-dimethylformamide, ethylene glycol, hexyl butyrate or octyl acetate.
[0059] In some embodiments, in step S3, the first mixture obtained in S1 is added to the mixed solvent obtained in S2 and ball milling beads are added for ball milling.
[0060] In some embodiments, the ball-to-material ratio of the ball mill is (1-40):1; the diameter of the ball mill beads is 1 mm-20 mm; the rotation speed of the ball mill is 100 rpm-600 rpm; and the ball milling time is 0.5 h-6 h.
[0061] Preferably, the ball-to-material ratio is (10-20):1, the ball diameter is 2 mm-5 mm, the ball speed is 300 rpm-500 rpm, and the ball milling time is 1 h-2 h. Under this ball milling parameter, sufficient mixing between electrolyte particles can be achieved, and the electrolyte particles will not be destroyed due to excessive ball milling energy.
[0062] The following describes the invention in conjunction with specific embodiments.
[0063] Example 1
[0064] A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to this embodiment includes the following steps:
[0065] S1. Preliminarily mix the halide electrolyte and the sulfide electrolyte to obtain a first mixture; in this embodiment, the mass ratio of the halide electrolyte to the sulfide electrolyte is 1:9; in this embodiment, the halide electrolyte is Li3InCl6; in this embodiment, the halide electrolyte particle size distribution is 500nm~50μm, and the halide electrolyte D50 particle size is 1μm~2μm; in this embodiment, the sulfide electrolyte is Li6PS5Cl; in this embodiment, the sulfide electrolyte particle size distribution is 500nm~50μm, and the sulfide electrolyte D50 particle size is 3μm~7μm;
[0066] S2, preliminarily mixing the non-polar solvent and the polar solvent to obtain a mixed solvent; in this embodiment, the volume ratio of the non-polar solvent to the polar solvent is 100:2; in this embodiment, the non-polar solvent is n-pentane; in this embodiment, the polar solvent is isobutanol;
[0067] S3, putting the first mixture obtained in S1 into the mixed solvent obtained in S2 and adding ball milling beads for ball milling; in this embodiment, the ball-to-material ratio of the ball milling is 10:1; the diameter of the ball milling beads is 10 mm; the speed of the ball milling is 480 rpm; and the ball milling time is 1 hour;
[0068] S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture; in this embodiment, the solid content of the second mixture is 56%;
[0069] S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
[0070] Example 2
[0071] The difference between Example 2 and Example 1 is that the mass ratio of the halide electrolyte to the sulfide electrolyte in step S1 is 0.5:9.5; the remaining steps and condition parameters are the same as those in Example 1.
[0072] Example 3
[0073] The difference between Example 3 and Example 1 is that the mass ratio of the halide electrolyte to the sulfide electrolyte in step S1 is 3:7; the remaining steps and condition parameters are the same as those in Example 1.
[0074] Example 4
[0075] The difference between Example 4 and Example 1 is that the volume ratio of the non-polar solvent to the polar solvent in step S2 is 100:5; the remaining steps and condition parameters are the same as those in Example 1.
[0076] Example 5
[0077] A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to this embodiment includes the following steps:
[0078] S1. Preliminarily mix the halide electrolyte and the sulfide electrolyte to obtain a first mixture. In this embodiment, the mass ratio of the halide electrolyte to the sulfide electrolyte is 0.1:8. In this embodiment, the halide electrolyte is Li3ScCl6 and Li2Sc 2 / 3 Cl4 combination; In this embodiment, the particle size distribution of the halide electrolyte is 500nm~50μm, and the particle size of the halide electrolyte D50 is 800nm~3μm; In this embodiment, the sulfide electrolyte is Li 10 SiP2S 12 ; In this embodiment, the particle size distribution of the sulfide electrolyte is 500nm~50μm, and the particle size of the sulfide electrolyte D50 is 1μm~3μm.
[0079] S2. Preliminarily mixing the non-polar solvent and the polar solvent to obtain a mixed solvent; in this embodiment, the volume ratio of the non-polar solvent to the polar solvent is 100:1; in this embodiment, the non-polar solvent is a combination of isopentane and cyclopentane; in this embodiment, the polar solvent is a combination of dichloromethane and methyl 2-bromobutyrate.
[0080] S3, putting the first mixture obtained in S1 into the mixed solvent obtained in S2 and adding ball milling beads for ball milling; in this embodiment, the ball-to-material ratio of the ball milling is 1:1; the diameter of the ball milling beads is 1 mm; the speed of the ball milling is 600 rpm; and the ball milling time is 6 hours;
[0081] S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture; in this embodiment, the solid content of the second mixture is 50%;
[0082] S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
[0083] Example 6
[0084] A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to this embodiment includes the following steps:
[0085] S1. Preliminarily mix the halide electrolyte and the sulfide electrolyte to obtain a first mixture; in this embodiment, the mass ratio of the halide electrolyte to the sulfide electrolyte is 2:7.5; in this embodiment, the halide electrolyte is a combination of Li2ZrCl6 and Li3InBr6; in this embodiment, the particle size distribution of the halide electrolyte is 500nm~50μm, and the particle size of the halide electrolyte D50 is 2μm~3μm; in this embodiment, the sulfide electrolyte is Li 10 SnP2S 12 ; In this embodiment, the particle size distribution of the sulfide electrolyte is 500nm~50μm, and the particle size of the sulfide electrolyte D50 is 5μm~6μm.
[0086] S2. Preliminarily mixing the non-polar solvent and the polar solvent to obtain a mixed solvent; in this embodiment, the volume ratio of the non-polar solvent to the polar solvent is 100:3; in this embodiment, the non-polar solvent is a combination of n-heptane and isooctane; in this embodiment, the polar solvent is a combination of methyl 2-bromobutyrate, butyl acetate and ethyl acetate.
[0087] S3, putting the first mixture obtained in S1 into the mixed solvent obtained in S2 and adding ball milling beads for ball milling; in this embodiment, the ball-to-material ratio of the ball milling is 40:1; the diameter of the ball milling beads is 20 mm; the speed of the ball milling is 100 rpm; and the ball milling time is 0.5 h;
[0088] S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture; in this embodiment, the solid content of the second mixture is 70%;
[0089] S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
[0090] Example 7
[0091] A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to this embodiment includes the following steps:
[0092] S1. Preliminarily mix the halide electrolyte and the sulfide electrolyte to obtain a first mixture. In this embodiment, the mass ratio of the halide electrolyte to the sulfide electrolyte is 1:8.5. In this embodiment, the halide electrolyte is Li 2.7 Zr 0.3 In 0.7Cl6; in this embodiment, the particle size distribution of the halide electrolyte is 500nm~50μm, and the particle size of the halide electrolyte D50 is 800nm~3μm; in this embodiment, the sulfide electrolyte is 70Li2S-30P2S5; in this embodiment, the particle size distribution of the sulfide electrolyte is 20~30μm, and the particle size of the sulfide electrolyte D50 is 1μm~3μm.
[0093] S2. Preliminarily mix the non-polar solvent and the polar solvent to obtain a mixed solvent; in this embodiment, the volume ratio of the non-polar solvent to the polar solvent is 100:4; in this embodiment, the non-polar solvent is a combination of hexane, cyclohexane, n-heptane and isooctane; in this embodiment, the polar solvent is N,N-dimethylformamide.
[0094] S3, putting the first mixture obtained in S1 into the mixed solvent obtained in S2 and adding ball milling beads for ball milling; in this embodiment, the ball-to-material ratio of the ball milling is 20:1; the diameter of the ball milling beads is 5 mm; the speed of the ball milling is 200 rpm; and the ball milling time is 5 hours;
[0095] S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture; in this embodiment, the solid content of the second mixture is 60%;
[0096] S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
[0097] Example 8
[0098] A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to this embodiment includes the following steps:
[0099] S1. Preliminarily mix the halide electrolyte and the sulfide electrolyte to obtain a first mixture; in this embodiment, the mass ratio of the halide electrolyte to the sulfide electrolyte is 1.5:8; in this embodiment, the halide electrolyte is a combination of Li3InCl6 and Li3InBr6; in this embodiment, the halide electrolyte particle size distribution is 500nm~50μm, and the halide electrolyte D50 particle size is 1μm~3μm; in this embodiment, the sulfide electrolyte is Li6PS5Cl; in this embodiment, the sulfide electrolyte particle size distribution is 30μm~40μm, and the sulfide electrolyte D50 particle size is 7μm~8μm.
[0100] S2. Preliminarily mix the non-polar solvent and the polar solvent to obtain a mixed solvent; in this embodiment, the volume ratio of the non-polar solvent to the polar solvent is 100:2; in this embodiment, the non-polar solvent is a combination of toluene and p-xylene; in this embodiment, the polar solvent is a combination of acetonitrile and butyl butyrate.
[0101] S3, adding the first mixture obtained in S1 into the mixed solvent obtained in S2 and adding ball milling beads for ball milling; in this embodiment, the ball-to-material ratio of the ball milling is 30:1; the diameter of the ball milling beads is 15 mm; the speed of the ball milling is 350 rpm; and the ball milling time is 4 hours;
[0102] S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture; in this embodiment, the solid content of the second mixture is 55%;
[0103] S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
[0104] Comparative Example 1
[0105] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not use a polar solvent, but only uses a non-polar solvent to mix with the electrolyte, and then directly performs ball milling after mixing, and the ball milling parameters are the same as those of Example 1. The remaining steps are the same as those of Example 1.
[0106] Comparative Example 2
[0107] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 does not use a sulfide electrolyte, but only uses a halide electrolyte as the positive electrode ion-conducting material. The remaining steps and condition parameters are the same as those of Example 1.
[0108] Experimental test:
[0109] (1) Electrochemical performance test of all-solid-state battery cells
[0110] The sulfide electrolyte Li6PS5Cl and PTFE were subjected to dry film formation to obtain an electrolyte membrane. Then, the positive electrode sheets obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were respectively assembled with the electrolyte membrane and the Li-In negative electrode into a single-layer soft-pack battery. Then, the electrochemical performance of the soft-pack battery cells was tested respectively. The test results are shown in Table 1.
[0111] Table 1 Electrochemical performance test results of soft-pack batteries of embodiments and comparative examples
[0112]
[0113] It can be seen from Table 1 that the first-cycle constant current charging ratio of the battery cell prepared by the positive electrode sheet in Example 1 is higher than that of the battery cell prepared by the positive electrode sheet in Comparative Example 2, indicating that the voltage polarization of the battery cell assembled in Example 1 is small and the internal resistance of the battery cell is low. This is because sulfide electrolyte and halide electrolyte are used simultaneously in the positive electrode ion-conducting material, which optimizes the particle size matching while ensuring the ionic conductivity of the composite positive electrode, thereby achieving the effect of reducing the internal resistance.
[0114] In addition, from the comparison between Example 1 and Comparative Example 1, it can be seen that the voltage polarization phenomenon in Comparative Example 1 is more serious than that in Example 1 (the constant current charging ratio is lower), and the cycle performance is worse than that in Example 1. Comparative Example 1 shows that an appropriate amount of polar solvent should be added when mixing sulfide and halide electrolytes to ensure the dispersion of the corresponding electrolyte particles and obtain a uniformly mixed mixed powder as an ion conductor for the composite positive electrode.
[0115] In addition, from the comparison between Examples 2 to 3 and Example 1, it can be seen that the composite electrolyte powder mixed by the method proposed in the present invention has a wider selectivity, and there is an optimal value for the mixing ratio of halide electrolyte to sulfide electrolyte, and the battery cell cycle performance is best under the optimal value.
[0116] Therefore, the present invention provides a method for improving the cycle performance of high-area-load all-solid-state battery cells, by simultaneously using sulfide electrolyte and halide electrolyte as composite positive electrode ion-conducting materials, and using non-polar and polar solvents in combination, and dispersing and fully mixing the above-mentioned mixed electrolyte by mechanical ball milling, thereby achieving full mixing of the sulfide electrolyte and the halide electrolyte. A large-area capacity battery cell with a composite powder of sulfide electrolyte and halide electrolyte as the positive electrode ion-conducting material can greatly improve the cycle polarization phenomenon and greatly improve the cycle stability of the battery cell.
[0117] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for improving the cycle performance of a high-area-load all-solid-state battery cell, characterized in that: The following steps are involved: S1, preliminarily mixing the halide electrolyte and the sulfide electrolyte to obtain a first mixture; S2, preliminarily mixing the non-polar solvent and the polar solvent to obtain a mixed solvent; S3, putting the first mixture obtained in S1 into the mixed solvent obtained in S2 for ball milling; S4, after the ball milling is completed, the ball milled material is vacuum dried and separated from the ball material to obtain a second mixture; S5. Mix the second mixture with the positive electrode active material, the conductive agent and the binder to obtain a third mixture, and make the third mixture into a positive electrode sheet, and assemble the positive electrode sheet into an all-solid-state battery cell.
2. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 1, characterized in that: The mass ratio of the halide electrolyte to the sulfide electrolyte is (0.1-3):(7-9.5).
3. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 1, characterized in that: The chemical formula of the halide electrolyte is Li a M b X c , wherein M is a metal element, including one or more of Sc, Y, La, Ho, Er, Tm, Yb, Lu, Al, Ga, In, Tl, and Fe; X is one or more of the non-metal elements F, Cl, Br, I, At, O, S, Se, and Te; wherein 0<a≤5, 0<b≤3, and 0<c≤10; and / or The particle size distribution of the halide electrolyte is 500nm-50μm, and the particle size D50 of the halide electrolyte is 800nm-3μm.
4. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 3, characterized in that: The halide electrolyte is Li3ScCl6, Li2Sc 2 / 3 Cl4、Li2In 1 / 3 Sc 1 / 3 Cl4、Li 2.25 Zr 0.75 Fe 0.25 Cl6、Li 2.7 Zr 0.3 In 0.7 One or a combination of two or more of Cl6, Li2ZrCl6, Li2ZrBr6, Li3InCl6, Li3InBr6.
5. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 1, characterized in that: The sulfide electrolyte is Li 6-i PS 5-i Q 1+i , Li 10 PcqI 12 , (100-x)Li2S-xP2S5 or a combination of two or more thereof; Wherein, Q is one or more of the non-metallic elements F, Cl, Br, I, 1≤i≤2; Cg is one or more of the carbon group elements Si, Ge, Sn; 10≤x≤50; and / or The particle size distribution of the sulfide electrolyte is 500 nm to 50 μm, and the D50 particle size of the sulfide electrolyte is 1 μm to 10 μm.
6. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 5, characterized in that: The sulfide electrolyte is Li6PS5Cl.
7. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 1, characterized in that: The volume ratio of the non-polar solvent to the polar solvent is 100:(1-5); and / or The solid content of the second mixture is 50% to 70%.
8. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 1, characterized in that: The non-polar solvent is one or a combination of two or more of n-pentane, isopentane, cyclopentane, hexane, cyclohexane, n-heptane, isooctane, toluene, p-xylene, carbon tetrachloride or petroleum ether; and / or The polar solvent is one or a combination of two or more of isobutanol, dichloromethane, methyl 2-bromobutyrate, butyl acetate, benzyl acetate, ethyl acetate, isopropanol, chloroform, isobutyl isobutyrate, butyl isobutyrate, pyridine, acetic acid, acetonitrile, butyl butyrate, N,N-dimethylformamide, ethylene glycol, hexyl butyrate or octyl acetate.
9. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 1, characterized in that: In the step S3, the first mixture obtained in S1 is put into the mixed solvent obtained in S2 and ball milling beads are added for ball milling.
10. A method for improving the cycle performance of a high-area-load all-solid-state battery cell according to claim 9, characterized in that: The ball-to-material ratio of the ball mill is (1-40):1; The diameter of the ball milling beads is 1 mm to 20 mm; The rotation speed of the ball mill is 100 rpm to 600 rpm; The ball milling time is 0.5h to 6h.
Citation Information
Patent Citations
Sulfide solid electrolyte film and preparation method thereof
CN115602914A
Composite positive pole piece as well as preparation method and application thereof
CN117542960A
Cited By
Selenium-doped sulfide solid electrolyte and preparation method thereof
CN120497427A
A selenium-doped sulfide solid-state electrolyte and a preparation method thereof
CN120497427B
Double-layer solid electrolyte and solid-state battery