Long-acting antibacterial coating stent as well as preparation method and application thereof

By alternately coating the surface of the ureteral stent with nano-silver gel and polyethyleneimine to form a multi-layer coating, the problems of urinary tract infection and crusting caused by the ureteral stent in the urine environment are solved, achieving long-lasting antibacterial and anti-adhesion effects. It is suitable for use after urinary tract stone surgery, ureteral stricture, and malignant tumors such as cervical cancer.

CN118892586AActive Publication Date: 2024-11-05TONGJI HOSPITAL ATTACHED TO TONGJI MEDICAL COLLEGE HUAZHONG SCI TECH

Patent Information

Application Number
CN202410895876.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-05
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Existing ureteral stents are prone to causing persistent urinary tract infections and crusting in the urine environment, and conventional antibacterial coatings are not stable or effective in this environment, making it difficult to effectively inhibit bacterial adhesion and crusting in the long term.

Method used

A multi-layer assembly technique is used to alternately coat the surface of the ureteral stent with nano-silver gel and polyethyleneimine. A uniform, stable, and long-lasting antibacterial coating is formed by a rotational coating method. The coating consists of three layers of nano-silver gel on the inner and outer sides and two layers of polyethyleneimine, which ensures stable sterilization and prevents crusting in the urine environment.

Benefits of technology

It achieves long-lasting antibacterial and anti-adhesion effects in the urine environment, reduces urinary tract infections and stent surface crusting, and has good cell compatibility and biocompatibility. It is suitable for use after urinary tract stone surgery, ureteral stricture, and malignant tumors such as cervical cancer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892586A_ABST
    Figure CN118892586A_ABST
Patent Text Reader

Abstract

The invention provides a long-acting antibacterial coating stent and a preparation method and application thereof.The long-acting antibacterial coating stent comprises a stent body and multiple antibacterial coatings, and the multiple antibacterial coatings are alternately applied to the surface of the stent, wherein the coatings on the inner wall and the outer wall of the stent body each comprise a coating formed by alternating three layers of nano-silver gel and two layers of polyethyleneimine, the nano-gel coating is formed by mixing the nano-silver gel and the polydopamine according to the solution volume ratio of 1: 1, and the uniformity of the coatings is ensured by adopting a spin coating method; the ureteral stent is suitable for being applied to ureteral stents, has good bactericidal performance and excellent anti-adhesion capacity, and can reduce the problems of urinary tract infection, stent surface crusting and the like caused by placement of the stents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ureteral stents, and in particular to a long-acting antibacterial coating stent and a preparation method and application thereof. Background Art

[0002] Urinary system stents such as ureteral stents and catheters are one of the indispensable tools in the diagnosis and treatment of many urinary tract diseases (urinary stones, ureteral stenosis, urinary system injuries, dysuria, urinary tract surgery, etc.). They can not only make the urine flow smoothly in the upper and lower urinary tracts through support and expansion, but also promote injury healing and stone removal.

[0003] As a foreign body in the urinary tract, urinary stents often cause proteins or bacteria in the urine to adhere to their surfaces after entering the human body. The bacteria after adhesion form bacterial biofilms by secreting polysaccharide matrix, fibrin, lipid protein, etc., thus causing refractory urinary tract infections. Such stent-related urinary tract infections usually cannot be suppressed by the use of antibiotics. In addition, the biofilm formed after bacterial adhesion and the presence of a special metabolic microenvironment in the urinary tract will cause calcium or non-calcium crystalline substances in the urine to adhere and aggregate on the surface of the stent, resulting in the formation of a crust on the surface of the stent. The above limitations are more significant in patients who need long-term placement of ureteral stents, increasing the treatment cost and pain of such patients who need to regularly replace new stents.

[0004] Antimicrobial coatings are designed to use surface modification and coating technology to apply antimicrobial agents to the surface of materials. Through the release of antimicrobial substances or contact sterilization, they inhibit the attachment and survival of bacteria on the stent and resist the formation and adhesion of urinary crystals, thereby inhibiting the formation of bacterial biofilms, and ultimately preventing infection and crusting. They are considered to be one of the most effective preventive measures. Currently, the antimicrobial agents commonly used in antimicrobial coatings include antibiotics, antimicrobial peptides, triclosan, nanosilver complexes, etc. Related research results also show that antimicrobial coatings can reduce the occurrence of infection and surface crusting to a certain extent.

[0005] However, the various calcium crystals, proteins, and changes in urine pH in the urine environment will affect the stability and functionality of the antibacterial coating material. For example, when the stent surface is covered with non-bacterial deposits, the antibacterial properties of the coating may be ineffective. Similarly, the difficulty in penetrating and drug resistance of the bacterial biofilm formed on the stent surface are also important reasons why many antibacterial coating solutions have been eliminated. Therefore, how to achieve long-term antibacterial and anti-adhesion effects and stably function in the special microenvironment of the urinary tract has become one of the urgent issues to be solved in the research of new urinary stents. Summary of the invention

[0006] One advantage of the present invention is that it provides a long-acting antibacterial coating stent and its preparation method and application. The long-acting antibacterial coating is coated on the surface of the ureteral stent through multi-layer assembly technology to obtain a long-acting antibacterial coating ureteral stent, which can achieve a stable bactericidal effect in the urine environment, thereby inhibiting infection.

[0007] One advantage of the present invention is that it provides a long-acting antibacterial coated stent and its preparation method and application, which can achieve long-term antibacterial and anti-adhesion, and play a stable role in the special microenvironment of the urinary tract. It is of great significance for solving problems such as urinary tract infection and stent surface crusting caused by stent placement in the urology field.

[0008] Another advantage of the present invention is that it provides a long-acting antibacterial coating stent and its preparation method and application. The inner and outer coatings of the ureteral stent are treated separately, and finally three layers of nanogel and two layers of polyethyleneimine are alternately coated respectively. The multi-layer material can effectively ensure the long-acting antibacterial effect.

[0009] Another advantage of the present invention is to provide a long-acting antibacterial coating stent and its preparation method and application. In the preparation process, a rotary coating method is adopted to make the coating more uniform and stable, and can maintain good sterilization and long-term stable anti-encrusting performance.

[0010] Another advantage of the present invention is to provide a long-acting antibacterial coating stent and its preparation method and application. The long-acting antibacterial coating not only has long-acting antibacterial properties, but also has good cell compatibility, is safe and non-cytotoxic, can reduce tissue inflammation, and is suitable for application in the field of ureteral stents.

[0011] Another advantage of the present invention is that it provides a long-acting antibacterial coated stent and its preparation method and application, which has antibacterial effect on many common bacteria, is degradable, and has good biocompatibility. The ureteral stent coated with a long-acting antibacterial coating is suitable for use after urinary stone surgery, ureteral stenosis, and malignant tumors such as cervical cancer.

[0012] According to one aspect of the present invention, the present invention provides a method for preparing a long-acting antibacterial coating stent, comprising the following steps:

[0013] (S10) preparing a long-lasting antibacterial coating solution;

[0014] (S20) treating the surface of the scaffold material;

[0015] (S30) coating the inner wall of the stent tube; and

[0016] (S40) Coating the outer wall of the stent tube.

[0017] The step (S10) comprises the following steps: (S101) preparation of nanogel; (S102) preparation of nanosilver gel; (S103) preparation of a first coating solution; and (S104) preparation of a second coating solution.

[0018] In the step (S101), a polyepoxide and a thiol compound are dissolved in a DMF solvent to a total concentration of 5%, wherein the molar ratio of the thiol group to the epoxy functional group is in the range of 1.2-1:1, and a nanogel is prepared by a proton transfer polymerization method using one of 1,8-diazacyclo[5.4.0]undec-7-ene (DBU) or triethylamine as a catalyst; and in the step (S102), silver nitrate is added to the nanogel, wherein the thiol functional group : silver nitrate molar ratio is 1:1-3, and sodium borohydride is used for reduction to prepare nano silver gel; wherein in the step (S103), 10mmol / L tris(hydroxymethylaminomethane) buffer solution is prepared, pH=8.5 is adjusted with hydrochloric acid, 2mg / mL dopamine solution is prepared with the buffer solution, and then mixed with the 2mg / mL nano silver gel prepared in the step (S102), so that the volume ratio of the dopamine solution to the nano silver gel solution is 1:1, and the first coating solution is obtained.

[0019] Wherein in the step (S104), the second coating solution is 3 mg / mL polyethyleneimine.

[0020] In the step (S20), the scaffold material is rinsed three times alternately with deionized water and 95% ethanol in an ultrasonic water bath, each rinse time is 5-10 minutes, and dried with nitrogen to complete the surface treatment of the scaffold material.

[0021] The step (S30) includes the following steps: (S301) first layer coating of the inner wall of the stent tube; (S302) second layer coating of the inner wall of the stent tube; and (S303) multi-layer coating of the inner wall of the stent tube.

[0022] In the step (S301), the first coating solution prepared in the step (S103) is sucked into the tube wall, the two ends of the tube are sealed, the stent tube is rotated at a 45° angle for 24 hours using a 3D rotator, the stent tube is taken out, the inner wall of the tube is cleaned with deionized water, and dried with nitrogen, thereby forming a stent tube with a single layer of nanosilver gel coated on the inner wall; in the step (S302), the second coating solution prepared in the step (S104) is sucked into the tube wall of the stent tube coated with the nanosilver gel, the two ends of the tube are sealed, and the stent tube is Use a 3D rotator to rotate at an angle of 45° for 30 minutes, take out, wash the inner wall of the tube with deionized water, and dry it with nitrogen. At this time, a stent tube with an inner wall coated with an inner layer of nanosilver gel and an outer layer of polyethyleneimine is formed; in the step (S303), the step (S301) and the step (S302) are repeated alternately, wherein the step (S301) is repeated twice and the step (S302) is repeated once. The final coating is composed of three layers of nanosilver gel and two layers of polyethyleneimine alternatingly, and the coating of the inner wall of the tube is completed.

[0023] The step (S40) includes the following steps: (S401) first layer coating of the outer wall of the stent tube; (S402) second layer coating of the outer wall of the stent tube; and (S403) multi-layer coating of the outer wall of the stent tube.

[0024] In the step (S401), both ends of the stent material with the inner wall coated are sealed and completely immersed in the first coating solution, and the amount of the first coating solution added is 1-2 mL / cm 2 The stent tube is rotated at an angle of 45° for 24 hours using a 3D rotator, the stent tube is taken out, the outer wall of the tube is cleaned with deionized water, and it is dried with nitrogen, thereby forming a stent tube with a single layer of nanosilver gel coated on the outer wall; in the step (S402), the stent tube in the step (S401) is completely immersed in the second coating solution, and the amount of the second coating solution input is 1-2 mL / cm 2 The stent tube is rotated at an angle of 45° for 30 minutes using a 3D rotator, taken out, the outer wall of the tube is cleaned with deionized water, and dried with nitrogen. At this time, a stent tube with an inner layer of nanosilver gel and an outer layer of polyethyleneimine is formed on the outer wall; in the step (S403), the step (S401) and the step (S402) are repeated alternately, wherein the step (S401) is repeated twice and the step (S402) is repeated once, and the final coating is composed of three layers of nanosilver gel and two layers of polyethyleneimine alternatingly, and the coating of the outer wall of the tube is completed.

[0025] According to another aspect of the present invention, the present invention also provides a long-acting antibacterial coating ureteral stent, comprising:

[0026] a bracket body; and

[0027] A multi-layer composite antibacterial coating comprises an inner coating and an outer coating, which are respectively and alternately coated on the inner surface and the outer surface of the stent body.

[0028] The multi-layer antibacterial coating comprises a nano silver gel coating and a polyethyleneimine coating, wherein the nano gel coating is formed by mixing the nano silver gel and the polydopamine in a solution volume ratio of 1:1.

[0029] The coatings on the inner wall and the outer wall of the stent body both include a coating formed by alternating three layers of nanosilver gel and two layers of polyethyleneimine.

[0030] According to another aspect of the present invention, the present invention further provides an application of a long-acting antibacterial coating stent, wherein the long-acting antibacterial coating is suitable for application to a ureteral stent.

[0031] The long-acting antibacterial coating stent comprises a stent body and a multi-layer antibacterial coating, wherein the coatings on the inner wall and the outer wall of the stent body both comprise a coating formed by alternating three layers of nanosilver gel and two layers of polyethyleneimine. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the existing ureteral stent tube after encrustation.

[0033] Figure 2 It is a schematic structural diagram of a ureteral stent with a long-acting antibacterial coating according to a preferred embodiment of the present invention.

[0034] Figure 3 This is a morphological diagram of a long-lasting antibacterial coating on a polyurethane substrate according to a preferred embodiment of the present invention.

[0035] Figure 4 It is an electron microscope scanning image and a hydrophilicity and hydrophobicity test image of the surface of the long-acting antibacterial coating according to the above preferred embodiment of the present invention.

[0036] Figure 5 It is a schematic diagram of the release of silver from the long-acting antibacterial coated ureteral stent sample according to the above preferred embodiment of the present invention.

[0037] Figure 6 It is a schematic diagram of the cytotoxicity release of the long-acting antibacterial coating stent sample according to the above preferred embodiment of the present invention.

[0038] Figure 7 and Figure 8 It is a schematic diagram of the antibacterial test results of the long-acting antibacterial coating stent sample and the modified ureteral stent according to the above preferred embodiment of the present invention.

[0039] Fig. 9It is a schematic diagram of testing the long-term antibacterial performance of the long-term antibacterial coated ureteral stent in a static artificial urine environment according to the above preferred embodiment of the present invention.

[0040] Fig.10 It is a schematic diagram of testing the long-term antibacterial performance of the long-term antibacterial coated ureteral stent in a flowing artificial urine environment according to the above preferred embodiment of the present invention.

[0041] Fig.11 It is a schematic diagram of the anti-encrustation performance test of the long-acting antibacterial coated ureteral stent in static and flowing artificial bacterial urine environments according to the above preferred embodiment of the present invention.

[0042] Fig.12 It is a schematic diagram of the anti-encrustation performance test of the long-acting antibacterial coated ureteral stent in different urine environments according to the above preferred embodiment of the present invention.

[0043] Fig.13 It is a schematic diagram of the antibacterial and anti-encrusting performance test of the long-acting antibacterial coated ureteral stent in animals according to the above preferred embodiment of the present invention.

[0044] Fig.14 It is a schematic diagram of the test of the surface calcium and magnesium deposition of the long-acting antibacterial coated ureteral stent in rats according to the above preferred embodiment of the present invention.

[0045] Fig.15 It is a schematic diagram of animal serum liver function indicators after the long-acting antibacterial coated ureteral stent according to the above preferred embodiment of the present invention is placed in an animal body.

[0046] Fig.16 It is a schematic diagram of the pathological results of liver and kidney tissues in an animal after the long-acting antibacterial coated ureteral stent according to the above preferred embodiment of the present invention is placed in the animal for a predetermined period of time.

[0047] Fig.17 It is a schematic diagram of evaluating bladder tissue inflammation in an animal body using the long-acting antibacterial coated ureteral stent according to the above preferred embodiment of the present invention. Fig.18 This is the test result of the long-acting antibacterial coated ureteral stent according to the above preferred embodiment of the present invention. DETAILED DESCRIPTION

[0048] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0049] Ureteral stents support, dilate and drain the ureters, and are mainly used to relieve obstruction or promote ureteral healing. However, in actual use, current ureteral stents, as foreign bodies in the urinary tract, often cause proteins or bacteria in the urine to adhere to their surfaces after entering the human body. The adhered bacteria form bacterial biofilms by secreting polysaccharide matrices, fibrin, lipid proteins, etc., thereby causing refractory urinary tract infections. Such stent-related urinary tract infections usually cannot be suppressed by the use of antibiotics. In addition, the biofilm formed after bacterial adhesion and the presence of the special metabolic microenvironment of the urinary tract will cause calcium or non-calcium crystalline substances in the urine to adhere and aggregate on the surface of the stent, resulting in the formation of a crust on the surface of the stent, such as attached Figure 1 The above limitations are more significant in patients who need long-term ureteral stent placement, increasing the cost and pain of regular replacement of new stents for such patients.

[0050] In order to solve the above technical problems, the present invention provides a long-acting antibacterial coated stent and its preparation method and application, which can achieve a stable bactericidal effect in the urine environment, thereby inhibiting stent-related urinary tract infection and the formation of stent surface crust.

[0051] Reference Figure 2 As shown, the long-acting antibacterial coating stent provided by the present invention includes a stent body 10, an inner coating 20, an outer coating 30 and a channel 40, wherein the channel 40 runs through the head end and the tail end of the stent body 10 to form a working channel for drainage.

[0052] The stent body 10 includes an inner wall 11 and an outer wall 12, the inner coating 20 is applied to the outer side of the inner wall 11, and the outer coating 30 is applied to the outer side of the outer wall 12, so that both the inner and outer sides of the stent body 10 of the ureteral stent are covered with the coating, so that the ureter has a long-lasting antibacterial effect.

[0053] The inner coating 20 and the outer coating 30 are both composite antibacterial coatings, and the inner coating 20 and the outer coating 30 both include two types of coatings, namely, a nanosilver gel coating and a polyethyleneimine coating, wherein the nanosilver gel coating is three layers, and the polyethyleneimine coating is two layers, and the nanosilver gel coating and the polyethyleneimine coating are alternately coated on the inner wall 11 and the outer wall 12. The multilayer coating formed by the alternate coating of multiple layers can achieve a good long-term antibacterial effect and effectively prevent bacteria and crusting.

[0054] Those skilled in the art will appreciate that the number of coatings of the inner coating 20 and the outer coating 30 is not limited to the examples in this embodiment, and may also be other numbers of coatings, such as alternating coatings of nanosilver gel and polyethyleneimine, or mixed coatings of nanosilver gel and polyethyleneimine.

[0055] The preparation method of the long-acting antibacterial coating stent provided by the present invention is as follows, wherein the preparation method of the long-acting antibacterial coating ureteral stent comprises the following steps:

[0056] (S10) preparing a long-lasting antibacterial coating solution;

[0057] (S20) treating the surface of the scaffold material;

[0058] (S30) coating the inner wall of the stent tube; and

[0059] (S40) Coating the outer wall of the stent tube.

[0060] Wherein said step (S10) comprises the following steps:

[0061] (S101) Preparation of nanogel;

[0062] (S102) Preparation of nanosilver gel;

[0063] (S103) preparing a first coating solution; and

[0064] (S104) Preparation of a second coating solution.

[0065] In the step (S101), polyepoxide and thiol compounds are used as reaction raw materials, and the molar ratio of thiol to epoxy functional group is 1.2-1:1, and they are dissolved in DMF solvent to make the total concentration 5%. Nanogel is prepared by proton transfer polymerization under alkaline catalyst.

[0066] The polyepoxide is an epoxy compound having at least two epoxy groups, and the thiol compound contains at least two thiol groups. The base catalyst is one of 1,8-diazacyclo[5.4.0]undec-7-ene (DBU) or triethylamine. The average particle size of the nanogel in water is 50-400 nm.

[0067] Example 1

[0068] The molar ratio of mercapto to epoxy is 1:1, and the catalyst is 1,8-diazacyclo[5.4.0]undec-7-ene (DBU).

[0069] Weigh 0.168 mmol of pentaerythritol-tetrakis-3-mercaptopropionate and 0.336 mmol of polyethylene glycol diglycidyl ether, with a thiol and epoxy molar ratio of 1:1, dissolve them in 5 mL of DMF solvent and stir magnetically for 30 min. Add 5 μL of DBU solution to the reaction solution and stir magnetically for 24 h under a nitrogen atmosphere to obtain nanogel.

[0070] Example 2

[0071] The molar ratio of mercapto to epoxy is 1:1, and the catalyst is triethylamine.

[0072] Weigh 0.168 mmol of pentaerythritol-tetrakis-3-mercaptopropionate and 0.336 mmol of polyethylene glycol diglycidyl ether, with a thiol and epoxy molar ratio of 1:1, dissolve them in 5 mL of DMF solvent and stir magnetically for 30 min. Add 140 μL of triethylamine solution to the reaction solution and stir magnetically for 24 h under a nitrogen atmosphere to obtain nanogel.

[0073] In the step (S102), silver nitrate is added to the nanogel at a molar ratio of thiol functional group to silver nitrate in the range of 1:1-3, and the nanosilver gel is prepared by reduction with sodium borohydride. The average particle size of the nanosilver in the prepared nanosilver gel is 5-50 nm.

[0074] Example 3

[0075] Take 1 mL of the nanogel prepared in any one of Example 1 and Example 2, slowly drop 9 mL of deionized water into the reaction solution at a ratio of 1:9 under magnetic stirring, and stir magnetically for 10 minutes.

[0076] 640 μL of 20 mg / mL silver nitrate solution was added to the reaction solution, and the mixture was magnetically stirred for 8-12 h at room temperature in the dark. 180 μL of 40 mg / mL sodium borohydride was added to the reaction solution, and the mixture was magnetically stirred for 4 h. The mixture was then purified by dialysis to obtain the prepared nanosilver gel solution.

[0077] Example 4

[0078] Take 1 mL of the nanogel prepared in any one of Example 1 and Example 2, slowly drop 9 mL of deionized water into the reaction solution at a ratio of 1:9 under magnetic stirring, and stir magnetically for 10 minutes.

[0079] 200 μL of 20 mg / mL silver nitrate solution was added to the reaction solution, and the mixture was magnetically stirred for 8-12 h at room temperature in the dark. 20 μL of 40 mg / mL sodium borohydride was added to the reaction solution, and the mixture was magnetically stirred for 4 h. The prepared nanosilver gel solution was then purified by dialysis.

[0080] In the step (S103), a first coating solution is prepared.

[0081] Example 5

[0082] Prepare 10mmol / L tris(hydroxymethylaminomethane) buffer solution, adjust pH to 8.5 with hydrochloric acid, use the buffer solution to prepare 2mg / mL dopamine solution, and quickly mix it with 2mg / mL nanosilver gel after dissolution. The volume ratio of dopamine solution to nanosilver gel solution is 1:1.

[0083] In the step (S104), a second coating solution is prepared.

[0084] Prepare 3 mg / mL polyethyleneimine.

[0085] In the step (S20), the ureteral stent is made of polyurethane (PU), including a thermoplastic polyurethane rubber (TPU) tube.

[0086] The scaffold material was rinsed alternately with deionized water and 95% ethanol for 3 times in an ultrasonic water bath, each rinse time was 5-10 minutes, and then dried with nitrogen.

[0087] The step (S30) comprises the following steps:

[0088] (S301) applying a first coating on the inner wall of the stent tube;

[0089] (S302) applying a second coating to the inner wall of the stent tube; and

[0090] (S303) Multi-layer coating of the inner wall of the stent tube.

[0091] In the step (S301), the first coating solution prepared in the step (S103) is sucked into the tube wall, and both ends of the tube are sealed. The stent tube is rotated at a 45° angle for 24 hours using a 3D rotator at room temperature; then the stent tube is taken out, the inner wall of the tube is gently cleaned with deionized water, the excess coating solution is removed, and the stent tube is dried with nitrogen, thereby forming a stent tube with a single layer of nanosilver gel coated on the inner wall.

[0092] In the step (302), the second coating solution prepared in the step (S104) is sucked into the wall of the stent tube coated with the nanosilver gel, and both ends of the tube are sealed. The stent tube is rotated at a 45° angle for 30 minutes using a 3D rotator at room temperature; then the stent tube is taken out, the inner wall of the tube is gently cleaned with deionized water, the excess coating solution is removed, and the stent tube is dried with nitrogen, thereby forming a stent tube with an inner wall coated with the nanosilver gel as an inner layer and the polyethyleneimine as an outer layer.

[0093] In the step (S303), the step (S301) and the step (S302) are repeated alternately, wherein the step (S301) is repeated twice and the step (S302) is repeated once. The final coating is composed of three layers of nanosilver gel and two layers of polyethyleneimine alternatingly, and the inner wall coating of the tube is completed.

[0094] The step (S40) comprises the following steps:

[0095] (S401) applying a first coating layer on the outer wall of the stent tube;

[0096] (S402) applying a second coating on the outer wall of the stent tube; and

[0097] (S403) Multi-layer coating of the outer wall of the stent tube.

[0098] In the step (S401), the two ends of the stent material with the inner wall coated are sealed and immersed in the prepared first coating solution, wherein the amount of the first coating solution added is 1-2 mL / cm 2 Stent tube, the preferred injection volume is 1mL / cm 2 , and the stent tube is completely immersed in the first coating solution. Under room temperature, the stent tube is rotated at a 45° angle for 24 hours using a 3D rotator; then the stent tube is taken out, the outer wall of the tube is gently cleaned with deionized water, the excess coating solution is removed, and the stent tube is dried with nitrogen gas, thereby forming a stent tube with a single layer of nanosilver gel coated on the outer wall.

[0099] Sealing both ends helps protect the inner wall of the stent tube that has been coated.

[0100] In the step (S402), the stent tube in the step (S401) is immersed in the prepared second coating solution, and the amount of the second coating solution added is 1-2 mL / cm 2 Stent tube, the preferred injection volume is 1mL / cm 2 , and the stent tube is completely immersed in the second coating solution. Under room temperature, the stent tube is rotated at a 45° angle for 30 minutes using a 3D rotator; then the stent tube is taken out, the outer wall of the tube is gently cleaned with deionized water, the excess coating solution is removed, and it is dried with nitrogen gas, at which time a stent tube with an inner layer of nanosilver gel and an outer layer of polyethyleneimine is formed.

[0101] In the step (S403), the step (S401) and the step (S402) are repeated alternately, wherein the step (S401) is repeated twice and the step (S402) is repeated once. The final coating is composed of three layers of nanosilver gel and two layers of polyethyleneimine alternatingly, and the outer wall coating of the tube is completed.

[0102] The biological tests for the ureteral stent prepared above are as follows:

[0103] Test 1: Topography test of long-lasting antibacterial coating on substrate

[0104] The morphology of the long-lasting antibacterial coating on the polyurethane substrate of the present invention is as follows: Figure 3 As shown (sPTE Ag :Single-layer nanosilver gel coating; mPTE Ag : Multilayer nano silver gel coating of the present invention), wherein Figure 3 A in the middle is the morphology of different coating methods on the surface of the polyurethane plate; Figure 3 B is the morphology of the coating of the present invention on the surface of the polyurethane tube. It can be seen that the spin coating method used in the present invention to prepare the coating is more uniform.

[0105] Test 2: Electron microscope scanning of the long-lasting antibacterial coating surface and surface hydrophilicity test

[0106] The electron microscope scanning image of the surface of the long-acting antibacterial coating of the present invention is as follows Figure 4 As shown in A, Figure 4 A is a single-layer nanogel (sPTE Ag ) and the multilayer nanosilver gel (mPTE) of the present invention Ag ) coating on the surface of polyurethane. The thickness of the multi-layer nano silver gel coating of the present invention is about 342-359nm.

[0107] The surface hydrophilicity test results are as follows Figure 4 As shown in B. The surface of the long-lasting antibacterial coating of the present invention was tested, and the results showed that the surface had stronger hydrophilicity, and the water contact angle was between 28-35°.

[0108] Test 3: Silver Release Test

[0109] in Figure 5 A is the silver content of each sampling point. Figure 5 B in the figure is the cumulative release curve of silver.

[0110] The common single-layer nanosilver coating (sPTE Ag ) polyurethane board and multi-layer long-lasting antibacterial coating (mPTE) prepared by the present invention Ag ) were cut into 50*10 mm size and immersed in 6 mL of PBS buffer with pH = 7.4. The Ag under physiological conditions was studied using an inductively coupled plasma tester. + The release behavior of nanosilver was calculated and the cumulative release of nanosilver in 60 days was as follows: Figure 5 As shown in the figure, it can be seen that compared with the ordinary single-layer nanosilver coating (sPTE Ag) polyurethane plate, the silver release of the long-acting antibacterial coating stent sample of the present invention is significantly improved, and the modified long-acting antibacterial coating stent provided by the present invention exhibits good cell compatibility.

[0111] Test 4: Cytotoxicity test

[0112] (1) The cultured 3T3 cells were inoculated into a 96-well plate at a density of 1×104 cells / well, 100 μL of DMEM complete medium was added to each well, and the cells were cultured in a cell culture incubator overnight; (2) The old medium was removed, a substrate (6 mm in diameter) was placed in the well plate, 100 μL of DMEM basal medium was added, and the cells were cultured for 24 h; (3) The old medium and substrate were removed, the cells were washed twice with PBS, 100 μL of DMEM basal medium containing 10% CCK-8 was added, and the cells were incubated for another 1 h. The optical density of each well at 450 nm was measured by an ELISA reader. Six replicate wells were set for each sample. The cell survival rate was calculated as follows: Figure 6 As shown: The results show that the coating is co-cultured with cells ( Figure 6 In A), the coated stent samples released in PBS for 24 hours and 48 hours have good cell compatibility.

[0113] Figure 6 Cytotoxicity test, where A is the cell viability of the stent coating sample after co-culture with cells for 24 hours, and B is the cell viability of the stent coating sample after co-culture with cells for 24 hours and 48 hours after release in PBS.

[0114] Test 5: In vitro antibacterial performance test

[0115] (1) Cut the substrate into small discs with a diameter of 6 mm, sterilize them with ultraviolet light for 15 to 30 minutes, place the substrate in a 96-well plate, add 10 -5 CFU / mL concentration of bacterial suspension; (2) inoculating substrates without antimicrobial nanogel coating as the control group; inoculating wells with bacterial solution without any substrate sample as the positive control, and wells without any bacteria and substrate sample as the negative control; (3) all samples and controls were incubated at 37°C for 24h; (4) taking 100μL of the solution in the above 96-well plate, evenly spread it on the agar plate and incubated for 24h, and the colonies were counted. Each group of experiments contained 3 parallel samples, and the antibacterial rate of each group of samples was calculated according to the following formula:

[0116] Killing%=(Control-Sample) / Control×100%

[0117] In the antibacterial test, two cultivation methods were used, the shaking method and the static method. In the shaking method, the antibacterial test solution was cultivated in a 37°C shaking incubator (120 rpm) for 24 h, and in the static method, the antibacterial test solution was cultivated in a 37°C hydroponic box for 24 h. The ordinary ureteral stent (before modification) and the long-acting antibacterial coating stent of the present invention (after modification) were used as controls, respectively. The results are shown in the attached Figure 7 As shown in the figure, it can be seen that the long-acting antibacterial coating stent in the present invention has an antibacterial effect on bacterial solutions in a static or moving state.

[0118] The antibacterial performance test was carried out in an artificial urine environment, and the common Gram-negative bacteria of the urinary system and methicillin-resistant Staphylococcus aureus were incubated for 24 hours. The results are shown in the attached Figure 8 and attached Fig.18 As shown in Table 1, from the attached Figure 8 and attached Fig.18 It can be seen from Table 1 that the long-acting antibacterial coating stent prepared by the present invention has antibacterial effects on several common bacteria such as Escherichia coli, Staphylococcus aureus, Proteus mirabilis, Enterococcus faecalis, etc. in the urine environment.

[0119] Test 6: Long-lasting antibacterial performance in urine environment

[0120] The prepared samples, single-layer samples and uncoated polyurethane ureteral stent samples were cut into 6*6mm sizes; artificial urine (calcium chloride 0.49g / L, magnesium chloride hexahydrate 0.65g / L, sodium chloride 4.6g / L, disodium sulfate 2.3g / L, trisodium citrate dihydrate 0.65g / L, disodium oxalate 0.02g / L, potassium dihydrogen phosphate 2.8g / L, potassium chloride 1.6g / L, ammonium chloride 1.0g / L, urea 25g / L, gelatin 5.0g / L) was prepared, the samples were immersed in a solution containing bacteria, incubated for 30 days, and bacteria were added at different time points for plating, such as Fig. 9 As shown, the antibacterial performance of the coated polyurethane material of the present invention in four bacteria and mixed bacteria environments over time is more outstanding than that of the single-layer material.

[0121] Fig. 9 : Long-term antibacterial test in a static artificial urine environment, A: Escherichia coli, B: Staphylococcus aureus, C: Enterococcus faecalis, D: Proteus mirabilis, E: Four mixed bacteria

[0122] The coating prepared by the present invention was coated on the inner wall of a silicone tube, and its long-term antibacterial performance was tested in an artificial urine circulation environment simulating urine flow (flow rate 1 mL / min, 37° C.). Fig.10 As shown, in the flowing urine environment infected with Escherichia coli and Proteus mirabilis, it has longer-lasting bactericidal performance than a single layer.

[0123] Test 7: Anti-crusting test

[0124] The coating prepared by the present invention was applied to a polyurethane plate, cut into 10*3mm size, immersed in 10mL artificial urine containing Proteus mirabilis for 24h, and the urine pH was measured at different time points. After 24h, the sample was taken out and scanned by electron microscope. The results are as follows: Fig.11 As shown in Figure A, the coating group prepared by the present invention can kill bacteria faster, thereby inhibiting the increase in pH caused by urease produced by bacteria, and ultimately inhibiting the formation of magnesium ammonium phosphate precipitation, keeping urine clear, and almost no crystals on its surface. After 30 days of testing in a flowing urine environment under the same conditions, the results are as follows Fig.11 As shown in B, it can maintain good sterilization and anti-crusting properties.

[0125] Fig.11 : A: Anti-crusting performance test under static artificial bacterial urine conditions; B: Long-term anti-crusting performance test under flowing artificial bacterial urine conditions.

[0126] In addition, the long-term antibacterial coating stent of the present invention was tested for its long-term anti-encrusting performance in different artificial urine environments and compared with a common ureteral stent as a reference. The comparative test results in normal artificial urine, hypercalcemia and hyperoxaluria are shown in the attached Fig.12 As shown in the figure, it can be seen that the long-acting antibacterial coating stent of the present invention has a highly effective anti-encrusting performance in various urine environments.

[0127] Test 8: Antibacterial and anti-encrusting test in animals

[0128] The prepared samples and uncoated polyurethane materials were cut into 4*2mm sizes. SD rats aged 6-8 weeks were selected. The rats were fasted 12 hours before surgery and anesthetized by intraperitoneal injection. After anesthesia, the rats were weighed, fixed, and disinfected. The midline incision was made in the abdomen to find and expose the bladder. Urine was extracted with a syringe and flushed with saline. An incision of about 5mm was made at the top of the bladder, and the stent sample was placed. The bladder, subcutaneous muscle tissue, and skin were sutured layer by layer. The rats were killed on the 15th and 30th days after implantation, and the stents were removed and SEM surface morphology tests were performed on the stents. The test results are as follows: Fig.13 and Fig.14 As shown, it can be seen from the results that compared with the control group (uncoated polyurethane material, i.e. PU before modification), the long-lasting antibacterial composite coating of the present invention also exhibits good antibacterial and long-lasting stable anti-encrusting effects in the urine environment of animals.

[0129] Fig.13 :A: Surface electron microscopy and urine smear results after implantation in animals; B: Calcium and magnesium deposition on the material surface 15 and 30 days after implantation in animals.

[0130] Test 9: Animal safety test

[0131] Thirty days after implantation in rat bladders, the silver levels in blood and urine were below the detection limit. Fig.18 Table 2 and Appendix Fig.15 As shown in Figure 2, the liver and kidney function indicators of the animals were all within the normal range, and the liver and kidney pathological tissue results at 30 days were as follows: Fig.16 As shown in the figure, no obvious abnormality was found in the liver and kidney tissues, indicating that the coating of the present invention has good safety and biocompatibility. Fig.17 As shown, the long-acting antibacterial coating stent (ie, modified PU) provided by the present invention causes less inflammation in surrounding tissues.

[0132] Fig.15 The serum liver and kidney function indexes of animals after 15 and 30 days of implantation. Fig.16 The results of liver and kidney tissue pathology 30 days after implantation in animals, A: liver, B: kidney.

[0133] From the above test results, it can be seen that the long-acting antibacterial coating stent prepared by the above preparation method has multiple coatings alternately forming a composite coating, and the surface is evenly coated. In biological detection, the long-acting antibacterial coating stent provided by the present invention has no cytotoxicity, good biocompatibility, and antibacterial and anti-encrusting properties, and is suitable for clinical use as a ureteral stent.

[0134] It should be understood by those skilled in the art that the embodiments of the present invention described above and shown in the accompanying drawings are only examples and do not limit the present invention. The purpose of the present invention has been fully and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.

Claims

1. A method for preparing a long-acting antibacterial coating stent, characterized in that: The following steps are involved: (S10) preparing a long-lasting antibacterial coating solution; (S20) treating the surface of the scaffold material; (S30) coating the inner wall of the stent tube; and (S40) Coating the outer wall of the stent tube.

2. The method for preparing a long-acting antibacterial coating stent according to claim 1, wherein the step (S10) comprises the following steps: (S101) Preparation of nanogel; (S102) preparing nano silver gel; (S103) preparing a first coating solution; And (S104) preparing a second coating solution.

3. The method for preparing a long-acting antibacterial coating stent according to claim 2, wherein in the step (S101), a polyepoxide and a thiol compound are dissolved in a DMF solvent to a total concentration of 5%, wherein the molar ratio of the thiol group to the epoxy functional group is in the range of 1.2-1:1, and a nanogel is prepared by a proton transfer polymerization method using one of 1,8-diazacyclo[5.4.0]undec-7-ene (DBU) or triethylamine as a catalyst; wherein in the step (S102), a polyepoxide and a thiol compound are added to the nanogel. Silver nitrate is added, wherein the molar ratio of thiol functional group to silver nitrate is 1:1-3, and sodium borohydride is used for reduction to prepare nano silver gel; wherein in the step (S103), 10mmol / L tris(hydroxymethylaminomethane) buffer solution is prepared, pH=8.5 is adjusted with hydrochloric acid, 2mg / mL dopamine solution is prepared with the buffer solution, and then mixed with the 2mg / mL nano silver gel prepared in the step (S102), so that the volume ratio of the dopamine solution to the nano silver gel solution is 1:1, so as to obtain the first coating solution.

4. The method for preparing a long-acting antibacterial coating stent according to claim 3, wherein in the step (S104), the second coating solution is 3 mg / mL polyethyleneimine.

5. The method for preparing a long-acting antibacterial coated stent according to any one of claims 2 to 4, wherein in the step (S20), the stent material is rinsed three times alternately with deionized water and 95% ethanol in an ultrasonic water bath, each rinse time is 5-10 minutes, and dried with nitrogen to complete the surface treatment of the stent material.

6. The method for preparing a long-acting antibacterial coating stent according to claim 5, wherein the step (S30) comprises the following steps: (S301) first layer coating of the inner wall of the stent tube; (S302) second layer coating of the inner wall of the stent tube; and (S303) multi-layer coating of the inner wall of the stent tube.

7. The method for preparing a long-acting antibacterial coating stent according to claim 6, wherein in the step (S301), the first coating solution prepared in the step (S103) is sucked into the tube wall, the two ends of the tube are closed, the stent tube is rotated at a 45° angle for 24 hours using a 3D rotator, the inner wall of the tube is washed with deionized water, and dried with nitrogen, thereby forming a stent tube with an inner wall coated with a single layer of nanosilver gel; in the step (S302), the second coating solution prepared in the step (S104) is sucked into the tube wall of the stent tube coated with the nanosilver gel. The two ends of the tube are sealed, and the stent tube is rotated at an angle of 45° for 30 minutes using a 3D rotator, taken out, and the inner wall of the tube is cleaned with deionized water and dried with nitrogen. At this time, a stent tube with an inner wall coated with an inner layer of nanosilver gel and an outer layer of polyethyleneimine is formed; in the step (S303), the step (S301) and the step (S302) are repeated alternately, wherein the step (S301) is repeated twice and the step (S302) is repeated once, and the final coating is composed of three layers of nanosilver gel and two layers of polyethyleneimine alternatingly, and the inner wall coating of the tube is completed.

8. The method for preparing a long-acting antibacterial coating stent according to claim 7, wherein the step (S40) comprises the following steps: (S401) applying a first coating layer on the outer wall of the stent tube; (S402) applying a second coating on the outer wall of the stent tube; and (S403) multi-layer coating of the outer wall of the stent tube.

9. The method for preparing a long-acting antibacterial coating stent according to claim 8, wherein in the step (S401), the two ends of the stent material with the inner wall coated are sealed and completely immersed in the first coating solution, and the amount of the first coating solution added is 1-2 mL / cm 2 The stent tube is rotated at an angle of 45° for 24 hours using a 3D rotator, the stent tube is taken out, the outer wall of the tube is cleaned with deionized water, and it is dried with nitrogen, thereby forming a stent tube with a single layer of nanosilver gel coated on the outer wall; in the step (S402), the stent tube in the step (S401) is completely immersed in the second coating solution, and the amount of the second coating solution input is 1-2 mL / cm 2 The stent tube is rotated at an angle of 45° for 30 minutes using a 3D rotator, taken out, the outer wall of the tube is cleaned with deionized water, and dried with nitrogen. At this time, a stent tube with an inner layer of nanosilver gel and an outer layer of polyethyleneimine is formed on the outer wall; in the step (S403), the step (S401) and the step (S402) are repeated alternately, wherein the step (S401) is repeated twice and the step (S402) is repeated once, and the final coating is composed of three layers of nanosilver gel and two layers of polyethyleneimine alternatingly, and the coating of the outer wall of the tube is completed.

10. A long-acting antibacterial coated ureteral stent, characterized in that: include: a bracket body; and A multi-layer composite antibacterial coating comprises an inner coating and an outer coating, which are respectively and alternately coated on the inner surface and the outer surface of the stent body.

11. The long-acting antibacterial coating stent according to claim 10, wherein each of the composite antibacterial coatings comprises a nanosilver gel coating and a polyethyleneimine coating, wherein the nanogel coating is formed by mixing the nanosilver gel and the polydopamine in a solution volume ratio of 1:

1.

12. The long-acting antibacterial coating stent according to claim 11, wherein the coatings on the inner wall and the outer wall of the stent body each comprise a coating formed by alternating three layers of nanosilver gel and two layers of polyethyleneimine.

13. The long-acting antibacterial coating stent according to any one of claims 10 to 12, wherein the long-acting antibacterial coating stent is prepared by the preparation method according to any one of claims 1 to 9.

14. An application of a long-acting antibacterial coating stent, characterized in that: The long-acting antibacterial coating is suitable for application in ureteral stents.

15. The use of the long-acting antibacterial coating according to claim 14, wherein the long-acting antibacterial coating stent comprises a stent body and a multi-layer composite antibacterial coating, wherein the coatings on the inner wall and the outer wall of the stent body both comprise a coating formed by alternating three layers of nanosilver gel and two layers of polyethyleneimine.

Citation Information

Patent Citations

  • Polymeric antifouling coating with antimicrobial peptides

    CA3219883A1

  • Method for preparing bionic coating through crosslinking of epoxy group and mercapto group

    CN105288731A

  • Method for preparing multi-layer membrane long-acting antibacterial coating based on bionic dopamine in-situ reduction nano silver

    CN106620900A

  • Implant with drug coating and preparation method thereof

    CN108744041A

  • Urethral stent with long-acting antibacterial and anti-stenosis functions and preparation method thereof

    CN113577401A

Cited By

  • Temperature-sensitive response type sodium polyacrylate catheter leakproof coating, preparation method and application thereof