Manufacturing method of low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors
By employing steps such as acid leaching and high-temperature purification sintering, a silicon carbide boat support with low iron content is prepared, solving the problem of difficult control of iron content in silicon carbide boat supports. This results in a pollution-free and long-life silicon carbide boat support suitable for the photovoltaic and semiconductor industries.
Patent Information
- Application Number
- CN202410931330.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing silicon carbide wafer mounts have problems in the photovoltaic and semiconductor industries, such as difficulty in controlling iron content, leading to silicon wafer contamination and short lifespan.
The process involves acid rinsing and purification, water washing and drying, raw material mixing, blank forming, splicing and sintering, and ultrasonic-assisted stirring and high-temperature purification sintering to control the iron content and prepare a low-iron-content, pollution-free silicon carbide boat support.
This achievement significantly reduces the iron content in silicon carbide boat supports, meeting the demands of the photovoltaic and semiconductor industries for pollution-free and long-life applications, and improving the flexural strength and thermal stability of the boat supports.
Smart Images

Figure BDA0004939755420000251
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of boat support production and processing, and in particular to a method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors. Background Art
[0002] The boat support is a key bearing component of the diffusion process equipment in the photovoltaic and semiconductor industries. Its application in the photovoltaic and semiconductor industries is mainly in the production process of photovoltaic cells, as a carrier for photovoltaic cells. In the photovoltaic and semiconductor industries, the traditional boat support material is mainly quartz, but because the quartz boat support is easy to deform in high temperature environment and has a short service life of about 3-6 months, silicon carbide boat support, as a new type of boat support material, has gradually become the preferred boat support material in the photovoltaic and semiconductor industries due to its good thermal stability and long service life.
[0003] Silicon carbide has excellent high temperature resistance and corrosion resistance, and its strength is high. Due to the chemical properties of silicon carbide ceramics, it is difficult to form, so it is usually prepared by reaction sintering. The reaction sintering method includes the steps of powder preparation, block pressing, drying and sintering. These steps involve many parameters. For example, the powder preparation stage requires a reasonable ratio of raw materials and the preparation of powder with a compliant particle size. The block pressing stage requires reasonable pressure conditions and block size design, and the temperature setting and processing time setting of the drying and sintering stages. If these steps are not designed reasonably, it will affect the hardness and other indicators of the finished product.
[0004] Silicon carbide boat supports can replace quartz boat supports and have a longer service life of more than 5 years. The use of silicon carbide boat supports can significantly reduce the cost of use, reduce downtime caused by maintenance and repairs, and reduce production capacity losses. Silicon carbide, as the main raw material for making silicon carbide boat supports, has properties such as high strength, high elastic modulus, high thermal expansion coefficient, good thermal shock resistance and acid and alkali corrosion resistance. Due to these excellent properties, silicon carbide materials are often used in industrial fields such as microelectronics, mechanical seals, aerospace, and heat exchange. Silicon carbide micropowder, which is the raw material used to prepare silicon carbide ceramics, has a significant effect on the various properties of silicon carbide ceramics after sintering. In order to obtain silicon carbide ceramics with excellent performance, manufacturers have put forward strict requirements on the particle size, particle shape, purity and fluidity of silicon carbide powder.
[0005] The photovoltaic and semiconductor industries usually use quartz as boat supports to support the wafer boat, on which silicon wafers are loaded for diffusion, coating and annealing processes. As the industry's requirements for the performance and efficiency of silicon wafers become increasingly stringent, rapid heat treatment technology has been widely adopted, and increasingly stringent requirements have been placed on the kiln support. Quartz boat supports are rarely used, have a short lifespan and are easily damaged, so they are gradually being replaced by silicon carbide boat supports with better performance. However, although the bearing strength and lifespan of traditional reaction-sintered silicon carbide boat supports can meet industry requirements, their impurity content, especially the iron content, is difficult to control. A large number of applications have shown that the iron content in the reaction-sintered silicon carbide boat supports will contaminate the silicon wafers, causing the color of the silicon wafers to darken and become scrapped. Therefore, it is particularly important to seek a method for manufacturing a low-iron content, pollution-free, high-purity silicon carbide boat support. Summary of the invention
[0006] In order to solve the problems mentioned in the above background technology, the present invention provides a method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0009] S1. Pickling and purification
[0010] Pour the SiC powder into a pickling agent solution, perform ultrasonic-assisted stirring pickling, and obtain a pickling slurry; wherein the concentration of the pickling agent solution is 0.05-0.2 mol / L, and the ultrasonic power is 180W-270W;
[0011] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into the pickling agent solution at a liquid-to-solid ratio of (4-6):1, the pickling temperature is 60-70°C, the ultrasonic frequency is 50-145kHz, the stirring speed is 150-350rpm, and the pickling time is 50-150min; the pickling agent is one or a combination of hydrochloric acid, sulfuric acid, and nitric acid;
[0012] S2, washing and drying
[0013] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content;
[0014] S3, Raw material mixing
[0015] The silicon carbide powder with low iron content and the high temperature resistant binder are uniformly mixed in a ratio of 5-8:1.5-2, and a proper amount of sintering aid is added to the mixture, and the mixture is mixed and ground to prepare a slurry; wherein the amount of the sintering aid added is 10-25% of the total amount of the silicon carbide powder and the high temperature resistant binder.
[0016] S4, blank forming
[0017] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying to remove moisture. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2000-2300°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0018] S5, splicing and sintering
[0019] The split components of the silicon carbide boat support are spliced together, and after being spliced into a complete boat support, they are sent into a vacuum furnace for high-temperature siliconization and sintering treatment at 1650-1700°C. After leaving the kiln, they are subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0020] The green silicon carbide powder with three particle size distributions of 90-100 μm, 8-10 μm and 1.5-2.5 μm average particle size used in the present invention must be subjected to acid washing and purification treatment, and the chemical composition is as follows: SiC%≥99.9%, Fe2O3%≤0.005%;
[0021] The working environment of semi-finished product production processes such as raw material weighing, mud preparation, grouting molding, and natural drying must be controlled at room temperature of 25℃~35℃, relative humidity of 40~50%, and closed and dust-free.
[0022] The present invention adopts a grouting molding method. Strictly controlling the increase of impurity content, especially iron content, during the production process is the key to the present invention. Therefore, the equipment and tools such as mixers, ball mills, pressure grouting machines used in the semi-finished product production processes such as batching, mud preparation, grouting molding, and natural drying, and the parts in contact with the mud adopt non-metallic linings, which can be stainless steel and polyurethane linings, preferably polyurethane linings. The batching barrel, grouting tank, stirring paddle, and plastic cup must be cleaned every time without water droplets or debris.
[0023] The steps for mud preparation are as follows:
[0024] A total of 100 kg of silicon carbide powder with three particle sizes of 90-100 μm, 8-10 μm and 1.5-2.5 μm are weighed respectively according to a weight ratio of 30-35:15-20:47-50, and fine powder and coarse powder are added to a ball mill in sequence; a high temperature resistant binder and an appropriate amount of sintering aid are added, and the mixture is ground and mixed to prepare a slurry.
[0025] Determine the slurry properties after ball milling: fluidity and specific gravity. If the slurry fluidity after ball milling is ≤35 seconds, the specific gravity is ≥2.4g / cm3, and there is no lumps of undispersed material in the slurry, the discharge requirements are met;
[0026] Put the ball-milled slurry into a barrel and stir it with a stirring paddle. The slurry needs to be stirred for more than 40 hours and can only be used after the slurry performance reaches the use standard.
[0027] The present invention adopts grouting molding. All utensils for holding mud must be cleaned to avoid contamination with mud of other materials. When the gypsum mold is closed, the gypsum mold must be cleaned with a brush. After the mold is closed and clamped, the model is laid flat and blown clean again with compressed air to ensure that no impurities are mixed into the grouting process. Vacuum degassing must be performed before grouting, and the vacuum degree is controlled at -0.5 to -1 bar. During grouting, the surface of the gypsum mold is gently tapped with a rubber hammer to facilitate the removal of bubbles. After the product is solidified, it is demoulded and naturally dried for 24 hours after demoulding. The temperature is controlled at ≥25°C and the humidity is controlled at ≥40%. The side panels, short panels, connecting panels and small parts required for the splicing of silicon carbide boat brackets are obtained by grouting molding.
[0028] The present invention adopts a two-step drying method of natural drying and hot air drying. The naturally dried wool body is sent to a drying furnace for drying. The drying temperature is up to 80°C and the drying time is 46 hours. In this way, the natural drying and hot air drying processes prevent the rapid dissipation of surface moisture of the product in the early stage of drying, and the cracking problem of the product is well solved. The heat source of the drying furnace used is an electric heating pipe, and a heat circulation fan and pipeline are installed. A purification adsorber is installed at the inlet of the pipeline to purify dust, oil gas, water and other impurities in the circulating hot air.
[0029] Carving
[0030] The blanks of side panels, short panels, connecting panels and small parts required for the splicing of silicon carbide boat supports are processed by engraving machines into semi-finished blanks such as side panels, short panels, connecting panels, etc. that meet the requirements of the drawings.
[0031] Purification calcination
[0032] The semi-finished product is purified and sintered in a medium-frequency graphite induction furnace. Before heating, it is first evacuated to a vacuum degree below 5Pa, and heating is started. The temperature is from room temperature to 200℃ for 3 to 4 hours, and vacuum is evacuated; the temperature is from 201 to 900℃ for 4 to 6 hours, and the vacuum is stopped. High-purity nitrogen with a purity of 99.996% is filled to restore normal pressure. At the same time, the wax exhaust fan is started to remove organic matter, and high-purity nitrogen is continuously filled at a rate of 30 to 50 ml / min; heating at 900 to 1100℃ for 1 to 2 hours, and vacuum is evacuated; high-purity argon with a purity of 99.996% is filled at 1100 to 2000℃, and sintering is carried out at normal pressure for 8 to 9 hours; heating at 2000 to 2300℃ for 8 to 9 hours; and keeping warm at 2300℃ for 5 hours.
[0033] Splicing
[0034] The silicon carbide boat support split parts are spliced into blanks, and after being spliced into a complete boat support, they are sent into a vacuum furnace for high-temperature siliconization and sintering at 1650-1700℃
[0035] Siliconizing sintering
[0036] A vacuum graphite electrode furnace is used. Before heating, vacuum is first evacuated to a vacuum degree of less than 5Pa, and heating is started. The temperature is from room temperature to 200℃ for 1 to 2 hours, and vacuum is evacuated; from 201 to 900℃ for 5 to 6 hours, vacuum is stopped, and high-purity nitrogen is filled to restore normal pressure. At the same time, the wax exhaust fan is started to remove organic matter, and high-purity nitrogen is continuously filled at a rate of 80 to 100 ml / min; heating at 900 to 1100℃ for 1 to 2 hours, vacuum is evacuated; heating at 1100 to 1300℃ for 2 to 3 hours; heating at 1300 to 1500℃ for 3 to 4 hours; heating at 1500 to 1650℃ for 3 to 4 hours; and keeping at 1650℃ for 2 hours. High-purity nitrogen is filled when cooling down, and the temperature is naturally cooled down.
[0037] The silicon used for siliconizing sintering is semiconductor silicon with a purity of 99.999%. The particle size is 3-5mm. After surface coating treatment, the semiconductor silicon is roasted together with the boat support that needs siliconizing treatment, with a weight ratio of 15-30:100. The surface coating treatment is to add a slurry of ultra-pure carbon black, hexagonal boron nitride, PVP K90 and water during the heating and stirring of the semiconductor silicon, so that a layer of coating is applied to the surface of the silicon particles, a certain amount of water is quickly removed, and then slowly dried. Before being put into the kiln, it is forced to be dried at 80°C again to ensure that there is no water and the surface coating is intact.
[0038] Finished product processing and impurity removal
[0039] After leaving the kiln, it is processed by grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning, drying and other processes. The finished product impurity removal process uses dilute hydrochloric acid, with a concentration controlled at 8-15%, a temperature controlled at 20-40℃, and a soaking time controlled at 20-60min; the product soaked in hydrochloric acid is repeatedly ultrasonically cleaned and dried, the purpose of which is to remove impurity oxides such as Fe, Al, Ca, Mg, and Ti on the surface of the product.
[0040] result
[0041] The product obtained after the above process is experimentally determined to have SiC% ≥ 95%, free silicon ≤ 5%, flexural strength ≥ 250Mpa, apparent porosity ≤ 0.01%, bulk density ≥ 3.02g / cm3, Fe content ≤ 5ppm, Ti content ≤ 5ppm, Mg content ≤ 3ppm, Zn content ≤ 2ppm, Al content ≤ 1ppm, Ca content ≤ 1ppm, and low impurity content, which can meet the requirements of silicon wafer diffusion process in photovoltaic and semiconductor industries for service life and pollution-free.
[0042] Preferably, the method for preparing the high temperature resistant adhesive comprises the following steps:
[0043] The graphite powder is dried, ground and sieved to ensure that its particle size is uniform and the particle size is controlled between 6-10μm;
[0044] The screened graphite powder is mixed with an organic cross-linking agent in a mixer to ensure that the graphite powder is evenly coated with the resin, a Lewis acid catalyst is added, and the temperature is controlled at 95-120°C. After the reaction is completed, a high temperature resistant adhesive is obtained.
[0045] Preferably, the organic crosslinking agent is an aqueous polyurethane dispersion with a solid content of 35-50%, an average particle size of 1-5 um, and an average molecular weight of 500-2000.
[0046] Graphite is a layered material composed of carbon atoms, with layers bonded by weak van der Waals forces. This structure gives it some unique properties, such as good lubricity and conductivity. When graphite is mixed with an aqueous polyurethane dispersion and used as a binder, it can form a tight bonding layer between the surfaces of silicon carbide. The layered structure of graphite and the interaction between layers can be used to achieve the purpose of making the two surfaces tightly bonded.
[0047] Preferably, the sintering aid is ultrapure carbon black, porous silicon, and metal oxides compounded in a ratio of 1.3:1.5-2:0.7-1. The metal oxide is one or a combination of Al2O3, MgO, ZrO2, and CuO.
[0048] Silicon carbide is a strong covalent bond compound with a relatively low grain boundary diffusion coefficient, which means that the migration rate of atoms or ions at the grain boundary is slow. In addition, its sintering driving force is limited, which means that the ability to push atoms or ions to rearrange during the sintering process is insufficient, and pure silicon carbide is difficult to sinter densely. Therefore, in order to assist the sintering process of silicon carbide ceramics, appropriate sintering aids must be added. The sintering aid will react with SiO2 on the surface of silicon carbide at a low melting point to form a low-temperature eutectic liquid phase, thereby completing the liquid phase sintering process.
[0049] The ultra-pure carbon black used has undergone high-temperature impurity removal treatment. The high-temperature impurity removal process is to send commercially available carbon black with a purity of ≥99% into a vacuum furnace, and undergo a high-temperature impurity removal treatment at 1600°C under a vacuum state to obtain ultra-pure carbon black with a purity of ≥99.9%.
[0050] The ultrapure carbon black added in the present invention has the property of porous adsorption, and can be more fully and evenly mixed with silicon carbide, and carbon has a strong reducing ability, and can eliminate oxygen impurities.
[0051] Porous silicon and ultrapure carbon black form silicon carbide at high temperature. Silicon carbide is an excellent deoxidizer that can reduce the oxygen content during the silicon carbide formation process. At the same time, the presence of silicon will inhibit the decomposition of silicon carbide crystals and enhance the strength of silicon carbide ceramic materials.
[0052] As an additive, alumina can promote the grain growth and grain boundary movement of the material, thereby improving the density and mechanical strength of alumina ceramics. This can not only enhance the thermal stability of the material, but also help improve its cavitation resistance; in the later stage of sintering, the growth of grains plays an important role in sintering densification. As a sintering aid, alumina can inhibit the abnormal growth of grains, thereby facilitating the densification process.
[0053] Magnesium oxide can form solid solutions with other oxides, thus changing the sintering characteristics of the material. Zirconium oxide and copper oxide can stabilize the lattice structure of the material during sintering, prevent crystal transformation, and help inhibit abnormal grain growth.
[0054] Preferably, the mixed grinding method is: the silicon carbide, high temperature resistant binder and sintering aid are placed in a ball mill lined with tetrafluoroethylene for wet mixing, and the ball mill is used for 12-15 hours at a speed of 280-300r / min, and the ball mill is reversed every 25 minutes, and the ball milling medium is silicon oxide ball milling beads. The ball milling time is long, and the sintering aid and silicon carbide powder can be effectively mixed. The use of silicon oxide ball milling beads can reduce the introduction of impurities that affect the thermal conductivity of the silicon carbide ceramic material.
[0055] Preferably, the mold filling method is: evenly coating the boron nitride ethanol solution on the inner wall of the graphite mold and both ends of the gasket, and after the ethanol evaporates, loading the completely dried powder and compacting it.
[0056] Adding boron nitride ethanol isolates the powder from the inner wall of the mold, prevents reaction and adhesion during sintering, and reduces the penetration of impurities in the mold into the silicon melt. After solidification, it can be demoulded smoothly to prevent the ceramic material and the mold from cracking due to stress of reaction adhesion during the condensation process. Usually, the mold can be reused after using the release agent, which reduces the production cost.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] 1. Silicon carbide in the present invention is a strong covalent bond compound, and its grain boundary diffusion coefficient is relatively low, which means that the migration rate of atoms or ions at the grain boundary is slow. In addition, its sintering driving force is limited, which means that the ability to promote the rearrangement of atoms or ions during the sintering process is insufficient, and pure silicon carbide is difficult to sinter densely. Therefore, in order to assist the sintering process of silicon carbide ceramics, appropriate sintering aids must be added. The sintering aid will react with SiO2 on the surface of silicon carbide at a low melting point to form a low-temperature eutectic liquid phase, thereby completing the liquid phase sintering process.
[0059] 2. The ultrapure carbon black in the present invention has the property of porous adsorption, and can be mixed more fully and evenly with silicon carbide, and carbon has a strong reducing ability, which can eliminate oxygen impurities. Silicon and carbon form silicon carbide at high temperature. Silicon carbide is an excellent deoxidizer, which can reduce the oxygen content in the process of silicon carbide formation. At the same time, due to the presence of silicon, the decomposition of silicon carbide crystals will be inhibited and the strength of silicon carbide ceramic materials will be enhanced.
[0060] 3. In the present invention, graphite is a layered material composed of carbon atoms, and the layers are bonded by weak van der Waals forces. This structure gives it some unique properties, such as good lubricity and conductivity. When graphite is mixed with an aqueous polyurethane dispersion and used as a binder, a tight bonding layer can be formed between the surfaces of silicon carbide. The layered structure of graphite and the interaction between the layers can be used to achieve the purpose of making the two surfaces tightly bonded.
[0061] In summary, the present invention uses low-iron-content and pollution-free silicon carbide powder as raw material to prepare the boat support, which can be widely used in photovoltaic and semiconductor industries and has high social use value and application prospects. DETAILED DESCRIPTION
[0062] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] Unless otherwise specified, the raw materials used in the present invention are all conventional products purchased from the market. Among them, SiC powder was purchased from Shandong Jialin Energy Technology Co., Ltd.;
[0064] Porous silicon was purchased from Lianyungang Wohua New Material Technology Co., Ltd., with a particle size of 400 mesh;
[0065] Hydrochloric acid, sulfuric acid, nitric acid, aqueous polyurethane dispersion, graphite, carbon black, Al2O3, MgO, ZrO2 and CuO were all purchased from Aladdin.
[0066] The mixed grinding method is as follows: the silicon carbide, the high temperature resistant binder and the sintering aid are wet mixed in a ball mill jar lined with tetrafluoroethylene, and the ball mill is used for 13 hours at a rotation speed of 300 r / min, and the ball mill is reversed once every 25 minutes, and the ball milling medium is silicon oxide ball milling beads. The ball milling time is long, and the sintering aid and the silicon carbide powder can be effectively mixed. The use of silicon oxide ball milling beads can reduce the introduction of impurities and thus affect the thermal conductivity of the silicon carbide ceramic material.
[0067] The mold filling method comprises the following steps: applying the boron nitride ethanol solution evenly to the inner wall of the graphite mold and both ends of the gasket, and after the ethanol evaporates, filling in completely dried powder and compacting.
[0068] Preparation Example
[0069] The preparation method of the high temperature resistant adhesive comprises the following steps:
[0070] The graphite powder is dried, ground and sieved to ensure that its particle size is uniform and the particle size is controlled between 6 μm;
[0071] 100g of sieved graphite powder and 65g of aqueous polyurethane dispersion (solid content of 40%, average particle size of 2.5um, average molecular weight of 1000) were mixed in a mixer to ensure that the graphite powder was evenly coated with the resin, 5g of Lewis acid catalyst was added, the temperature was controlled at 100°C, and a high temperature resistant adhesive was obtained after the reaction was completed.
[0072] Example 1
[0073] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0074] S1. Pickling and purification
[0075] 30 g of SiC powder with an average particle size of 90 μm, 20 g of SiC powder with an average particle size of 8 μm, and 50 g of SiC powder with an average particle size of 2.5 μm are poured into a pickling agent hydrochloric acid solution, and ultrasonic-assisted stirring pickling is performed to obtain a pickling slurry; wherein the concentration of the pickling agent hydrochloric acid solution is 0.05 mol / L, and the ultrasonic power is 180 W;
[0076] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into the pickling agent solution at a liquid-to-solid ratio of 4:1, the pickling temperature is 60° C., the ultrasonic frequency is 50 kHz, the stirring speed is 150 rpm, and the pickling time is 100 min;
[0077] S2, washing and drying
[0078] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.5%, and the impurity content is reduced to Fe < 0.006%;
[0079] S3, Raw material mixing
[0080] 50g of silicon carbide powder with low iron content was evenly mixed with 15g of the high temperature resistant binder in the preparation example, 10g of sintering aid was added to the mixture, and the mixture was mixed and ground to prepare a slurry; the sintering aid was a compound of 13g of ultrapure carbon black, 15g of porous silicon, and 10g of Al2O3.
[0081] S4, blank forming
[0082] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a temperature of 2000°C under nitrogen protection to obtain a silicon carbide boat support split component blank.
[0083] S5, splicing and sintering
[0084] The split components of the silicon carbide boat support are spliced together, and after being spliced into a complete boat support, they are sent into a vacuum furnace for 1700℃ high-temperature siliconization and sintering treatment. After leaving the kiln, they are subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0085] Example 2
[0086] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0087] S1. Pickling and purification
[0088] 35 g of SiC powder with an average particle size of 90 μm, 20 g of SiC powder with an average particle size of 8 μm, and 47 g of SiC powder with an average particle size of 2.5 μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.1 mol / L, and the ultrasonic power was 200 W;
[0089] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a hydrochloric acid solution at a liquid-to-solid ratio of 4:1, the pickling temperature is 65° C., the ultrasonic frequency is 100 kHz, the stirring speed is 200 rpm, and the pickling time is 100 min;
[0090] S2, washing and drying
[0091] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.6%, and the impurity content is reduced to Fe < 0.005%;
[0092] S3, Raw material mixing
[0093] 50 g of silicon carbide powder with low iron content was uniformly mixed with 20 g of the high temperature resistant binder in the preparation example, and 15 g of a sintering aid was added to the mixture. After mixing and grinding, the mixture was sieved using an ultrasonic vibration sieve (mesh size 400 meshes).
[0094] The sintering aid is a compound of 13g ultrapure carbon black, 20g porous silicon and 10g Al2O3.
[0095] S4, blank forming
[0096] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2100°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0097] S5, splicing and sintering
[0098] The split components of the silicon carbide boat support are spliced together into a complete boat support, which is then sent into a vacuum furnace for high-temperature siliconization and sintering at 1650°C. After leaving the kiln, it is subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning, and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0099] Example 3
[0100] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0101] S1. Pickling and purification
[0102] 30 g of SiC powder with an average particle size of 90 μm, 15 g of SiC powder with an average particle size of 8 μm, and 48 g of SiC powder with an average particle size of 2.5 μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.15 mol / L, and the ultrasonic power was 220 W;
[0103] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a pickling agent hydrochloric acid solution at a liquid-to-solid ratio of 4:1, the pickling temperature is 65°C, the ultrasonic frequency is 100kHz, the stirring speed is 150rpm, and the pickling time is 100min;
[0104] S2, washing and drying
[0105] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.4%, and the impurity content is reduced to Fe < 0.005%;
[0106] S3, Raw material mixing
[0107] 50 g of silicon carbide powder with low iron content was mixed evenly with 18 g of the high temperature resistant binder in the preparation example, 12 g of a sintering aid was added to the mixture, mixed and ground, and then sieved using an ultrasonic vibration sieve (mesh size 400 mesh);
[0108] The sintering aid is a compound of 13g ultrapure carbon black, 18g porous silicon and 8g Al2O3.
[0109] S4, blank forming
[0110] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2150°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0111] S5, splicing and sintering
[0112] The split components of the silicon carbide boat support are spliced together into a complete boat support, which is then sent into a vacuum furnace for high-temperature siliconization and sintering at 1680°C. After leaving the kiln, it is subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning, and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0113] Example 4
[0114] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0115] S1. Pickling and purification
[0116] 30 g of SiC powder with an average particle size of 95 μm, 20 g of SiC powder with an average particle size of 8 μm, and 50 g of SiC powder with an average particle size of 1.5 μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.2 mol / L, and the ultrasonic power was 270 W;
[0117] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a pickling agent hydrochloric acid solution at a liquid-to-solid ratio of 5:1, the pickling temperature is 70°C, the ultrasonic frequency is 145kHz, the stirring speed is 350rpm, and the pickling time is 150min;
[0118] S2, washing and drying
[0119] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.8%, and the impurity content is reduced to Fe < 0.004%;
[0120] S3, Raw material mixing
[0121] 100 g of silicon carbide powder with low iron content was uniformly mixed with 30 g of the high temperature resistant binder in the preparation example, 20 g of a sintering aid was added to the mixture, mixed and ground, and then sieved using an ultrasonic vibration sieve (mesh size 500 mesh);
[0122] The sintering aid is a compound of 26g ultrapure carbon black, 30g porous silicon and 14g ZrO2.
[0123] S4, blank forming
[0124] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2150°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0125] S5, splicing and sintering
[0126] The split components of the silicon carbide boat support are spliced together, and after being spliced into a complete boat support, they are sent into a vacuum furnace for 1700℃ high-temperature siliconization and sintering treatment. After leaving the kiln, they are subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0127] Example 5
[0128] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0129] S1. Pickling and purification
[0130] 30 g of SiC powder with an average particle size of 100 μm, 20 g of SiC powder with an average particle size of 8 μm, and 47 g of SiC powder with an average particle size of 2.5 μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.15 mol / L, and the ultrasonic power was 250 W;
[0131] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a pickling agent nitric acid solution at a liquid-to-solid ratio of 5:1, the pickling temperature is 65°C, the ultrasonic frequency is 145kHz, the stirring speed is 300rpm, and the pickling time is 120min;
[0132] S2, washing and drying
[0133] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.4%, and the impurity content is reduced to Fe < 0.006%;
[0134] S3, Raw material mixing
[0135] 100 g of silicon carbide powder with low iron content was uniformly mixed with 35 g of the high temperature resistant binder in the preparation example, 25 g of a sintering aid was added to the mixture, mixed and ground, and then sieved using an ultrasonic vibration sieve (mesh size 400 mesh);
[0136] The sintering aid is a compound of 26g ultrapure carbon black, 34g porous silicon and 16g ZrO2.
[0137] S4, blank forming
[0138] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a temperature of 2200°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0139] S5, splicing and sintering
[0140] The split components of the silicon carbide boat support are spliced together into a complete boat support, which is then sent into a vacuum furnace for high-temperature siliconization and sintering at 1660°C. After leaving the kiln, it is subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning, and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0141] Example 6
[0142] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0143] S1. Pickling and purification
[0144] 35 g of SiC powder with an average particle size of 90 μm, 20 g of SiC powder with an average particle size of 10 μm, and 50 g of SiC powder with an average particle size of 2.5 μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.2 mol / L, and the ultrasonic power was 270 W;
[0145] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a pickling agent nitric acid solution at a liquid-to-solid ratio of 5:1, the pickling temperature is 70°C, the ultrasonic frequency is 145kHz, the stirring speed is 350rpm, and the pickling time is 150min;
[0146] S2, washing and drying
[0147] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.7%, and the impurity content is reduced to Fe < 0.005%;
[0148] S3, Raw material mixing
[0149] 100 g of silicon carbide powder with low iron content was mixed evenly with 40 g of the high temperature resistant binder in the preparation example, 30 g of a sintering aid was added to the mixture, mixed and ground, and then sieved using an ultrasonic vibration sieve (mesh size 500 mesh);
[0150] The sintering aid is a compound of 65g ultrapure carbon black, 75g porous silicon and 50g ZrO2.
[0151] S4, blank forming
[0152] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2100°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0153] S5, splicing and sintering
[0154] The split components of the silicon carbide boat support are spliced together, and after being spliced into a complete boat support, they are sent into a vacuum furnace for 1700℃ high-temperature siliconization and sintering treatment. After leaving the kiln, they are subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0155] Example 7
[0156] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0157] S1. Pickling and purification
[0158] 35 g of SiC powder with an average particle size of 100 μm, 15 g of SiC powder with an average particle size of 10 μm, and 50 g of SiC powder with an average particle size of 2.5 μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.1 mol / L, and the ultrasonic power was 220 W;
[0159] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a pickling agent hydrochloric acid solution at a liquid-to-solid ratio of 6:1, the pickling temperature is 60°C, the ultrasonic frequency is 100kHz, the stirring speed is 200rpm, and the pickling time is 100min;
[0160] S2, washing and drying
[0161] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.8%, and the impurity content is reduced to Fe < 0.004%;
[0162] S3, Raw material mixing
[0163] 500 g of silicon carbide powder with low iron content was uniformly mixed with 150 g of the high temperature resistant binder in the preparation example, 100 g of a sintering aid was added to the mixture, mixed and ground, and then sieved using an ultrasonic vibration sieve (mesh size 500 mesh).
[0164] The sintering aid is a compound of 130 g ultrapure carbon black, 150 g porous silicon and 70 g CuO.
[0165] S4, blank forming
[0166] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2150°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0167] S5, splicing and sintering
[0168] The split components of the silicon carbide boat support are spliced together, and after being spliced into a complete boat support, they are sent into a vacuum furnace for 1700℃ high-temperature siliconization and sintering treatment. After leaving the kiln, they are subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0169] Example 8
[0170] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0171] S1. Pickling and purification
[0172] 30 g of SiC powder with an average particle size of 90 μm, 20 g of SiC powder with an average particle size of 10 μm, and 50 g of SiC powder with an average particle size of 1.5 μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.1 mol / L, and the ultrasonic power was 250 W;
[0173] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a pickling agent hydrochloric acid solution at a liquid-to-solid ratio of 6:1, the pickling temperature is 70°C, the ultrasonic frequency is 145kHz, the stirring speed is 350rpm, and the pickling time is 120min;
[0174] S2, washing and drying
[0175] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.5%, and the impurity content is reduced to Fe < 0.005%;
[0176] S3, Raw material mixing
[0177] 500 g of silicon carbide powder with low iron content was uniformly mixed with 180 g of the high temperature resistant binder in the preparation example, and 150 g of a sintering aid was added to the mixture. After mixing and grinding, the mixture was sieved using an ultrasonic vibration sieve (mesh size 400 meshes).
[0178] The sintering aid is a compound of 130 g ultrapure carbon black, 180 g porous silicon and 80 g CuO.
[0179] S4, blank forming
[0180] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2300°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0181] S5, splicing and sintering
[0182] The split components of the silicon carbide boat support are spliced together into a complete boat support, which is then sent into a vacuum furnace for high-temperature siliconization and sintering at 1650°C. After leaving the kiln, it is subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning, and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0183] Example 9
[0184] A method for manufacturing a low-iron-content pollution-free silicon carbide boat support for photovoltaics and semiconductors, comprising the following steps:
[0185] S1. Pickling and purification
[0186] 35g of SiC powder with an average particle size of 90μm, 20g of SiC powder with an average particle size of 8μm, and 50g of SiC powder with an average particle size of 1.5μm were poured into a pickling agent solution, and ultrasonic-assisted stirring pickling was performed to obtain a pickling slurry; wherein the concentration of the pickling agent solution was 0.2mol / L, and the ultrasonic power was 270W;
[0187] In S1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into a pickling agent hydrochloric acid solution at a liquid-to-solid ratio of 6:1, the pickling temperature is 68°C, the ultrasonic frequency is 140kHz, the stirring speed is 300rpm, and the pickling time is 120min; the pickling agent is one or a combination of sulfuric acid and nitric acid;
[0188] S2, washing and drying
[0189] The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content. The Fe element content is analyzed by ICP-OES. After testing, the Fe impurity removal rate of the silicon carbide powder can reach 93.5%, and the impurity content is reduced to Fe < 0.006%;
[0190] S3, Raw material mixing
[0191] 800 g of silicon carbide powder with low iron content was uniformly mixed with 200 g of the high temperature resistant binder in the preparation example, and 250 g of a sintering aid was added to the mixture. After mixing and grinding, the mixture was sieved using an ultrasonic vibration sieve (mesh size 500 mesh).
[0192] The sintering aid is a compound of 130 g ultrapure carbon black, 200 g porous silicon and 100 g CuO.
[0193] S4, blank forming
[0194] The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2300°C under the protection of inert gas to obtain a silicon carbide boat support split component blank.
[0195] S5, splicing and sintering
[0196] The split components of the silicon carbide boat support are spliced together, and after being spliced into a complete boat support, they are sent into a vacuum furnace for 1700℃ high-temperature siliconization and sintering treatment. After leaving the kiln, they are subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
[0197] Comparative Example 1
[0198] The difference between this comparative example and Example 1 is that the high temperature resistant binder in the preparation example is replaced by a commercially available aluminum dihydrogen phosphate binder purchased from Zibo Yueyang Chemical Technology Co., Ltd. with a CAS number of 151-692-82836.
[0199] Comparative Example 2
[0200] The difference between this comparative example and Example 1 is that the high temperature resistant binder in the preparation example is replaced with 100 g of commercially available graphite powder and 65 g of epoxy resin. The graphite powder is purchased from Hebei Hezhen Industrial Co., Ltd. with a product number of 01 and a crystal particle size of 2000 mm.
[0201] The epoxy resin was purchased from Guangzhou Yixin Chemical Technology Co., Ltd. with a CAS number of 61788-97-4.
[0202] Comparative Example 3
[0203] The difference between this comparative example and Example 1 is that the high temperature resistant binder in the preparation example is replaced by a commercially available aqueous polyurethane dispersion, Guangzhou Hangeng New Materials Co., Ltd., model 893, with a solid content of 32%.
[0204] Comparative Example 4
[0205] The difference between this comparative example and Example 1 is that no sintering aid is added in step S3, mixing the raw materials.
[0206] The bending strength adopts the GB / T 1965-1996 porous ceramic bending strength test method;
[0207] Thermal conductivity adopts GB / T22588-2008 flash method to measure thermal diffusivity or thermal conductivity;
[0208] The porosity adopts the test method of apparent porosity and capacity of porous ceramics in GB / T 1966-1996;
[0209] Wear resistance test: The samples prepared in the examples and comparative examples were tested with reference to GB / T 9867-2008; the specific experimental data are shown in Table 1:
[0210] Table 1
[0211]
[0212] In summary, the silicon carbide boat support prepared in the embodiment of the present invention has greatly improved bending strength, thermal conductivity and wear resistance compared to the control example, and the silicon carbide boat support prepared in the present application has a lower porosity, so it has a higher thermal conductivity, and plays an important role in the process equipment of the photovoltaic and semiconductor industries.
[0213] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaics and semiconductors, It is characterized in that The following steps are involved: S1. Pickling and purification Pour the SiC powder into a pickling agent solution, perform ultrasonic-assisted stirring pickling, and obtain a pickling slurry; wherein the concentration of the pickling agent solution is 0.05-0.2 mol / L, and the ultrasonic power is 180W-270W; S2, washing and drying The pickled slurry is repeatedly rinsed with deionized water and the pH value is adjusted to 6-7 to obtain washed SiC powder, which is then dried to obtain silicon carbide powder with low iron content; S3, Raw material mixing The silicon carbide powder with low iron content and the high temperature resistant binder are uniformly mixed in a certain proportion, an appropriate amount of sintering aid is added to the mixture, and the mixture is mixed and ground to prepare a slurry; S4, blank forming The blank of the boat support split component is obtained by the grouting molding process. The blank is trimmed and carved into a semi-finished boat support split component that meets the size requirements after natural drying and hot air drying to remove moisture. The semi-finished product enters the induction furnace and is purified and sintered at a high temperature of 2000-2300°C under the protection of inert gas to obtain a silicon carbide boat support split component blank. S5, splicing and sintering The split components of the silicon carbide boat support are spliced together, and after being spliced into a complete boat support, they are sent into a vacuum furnace for high-temperature siliconization and sintering treatment at 1650-1700°C. After leaving the kiln, they are subjected to grinding, sandblasting, fine washing, impurity removal, ultrasonic cleaning and drying processes to obtain a low-iron content and pollution-free silicon carbide boat support.
2. A method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 1, It is characterized in that In the step 1, the conditions for ultrasonic-assisted stirring pickling are: pouring the SiC powder to be pickled into the pickling agent solution at a liquid-to-solid ratio of (4-6):1, the pickling temperature is 60-70°C, the ultrasonic frequency is 50-145kHz, the stirring speed is 150-350rpm, and the pickling time is 50-150min; The pickling agent is one or a combination of hydrochloric acid, sulfuric acid and nitric acid.
3. The method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 1, It is characterized in that The preparation method of the high temperature resistant adhesive comprises the following steps: The graphite powder is dried, ground and sieved to ensure that its particle size is uniform and the particle size is controlled between 6-10μm; The screened graphite powder is mixed with an organic cross-linking agent in a mixer to ensure that the graphite powder is evenly coated with the resin, a Lewis acid catalyst is added, and the temperature is controlled at 95-120°C. After the reaction is completed, a high temperature resistant adhesive is obtained.
4. The method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 3, It is characterized in that The organic cross-linking agent is an aqueous polyurethane dispersion with a solid content of 35-50%, an average particle size of 1-5um, and an average molecular weight of 500-2000.
5. The method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 1, It is characterized in that The sintering aid is ultrapure carbon black, porous silicon and metal oxide, which are compounded in the ratio of 1.3:1.5-2:0.7-1.
6. A method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 5, It is characterized in that The metal oxide is Al 2 O 3 、MgO、ZrO 2 and CuO or a combination of them.
7. The method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 1, It is characterized in that The mixed grinding method is: placing the silicon carbide, high temperature resistant binder and sintering aid in a ball mill liner with tetrafluoroethylene for wet mixing, using a ball mill for ball milling for 12-15 hours, with a rotation speed of 280-300r / min, reversing once every 25 minutes, and the ball milling medium is silicon oxide ball milling beads.
8. The method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 1, It is characterized in that When the blank is formed in step S4, the boron nitride ethanol solution is evenly coated on the inner wall of the graphite mold and both ends of the gasket. After the ethanol evaporates, the completely dried powder is loaded and compacted.
9. The method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 1, It is characterized in that The silicon carbide powder uses 3N green silicon carbide powder with three particle size distributions of average particle diameters of 90-100 μm, 8-10 μm and 1.5-2.5 μm as raw material, and the proportion of the three is controlled at a weight ratio of 30-35:15-20:47-50.
10. The method for manufacturing a low iron content pollution-free silicon carbide boat support for photovoltaic and semiconductor use according to claim 1, It is characterized in that The added amount of the sintering aid is 10-25% of the total amount of the silicon carbide powder and the high temperature resistant binder; the silicon carbide powder with low iron content and the high temperature resistant binder are mixed in a ratio of 5-8:1.5-2.
Citation Information
Patent Citations
Porous silicon carbide ceramic and preparation method thereof
CN105294107A
C / C-ZrC composite material as well as preparation method and application thereof
CN106588044A
Method for preparing multiphase composite ceramic sealing ring
CN110028322A
Method for preparing siliconizing silicon carbide hot-press casting oven fire-bearing beryllium
CN110218094A
Low-carbon ultra-low-carbon aluminum silicon carbide carbon refractory material and preparation method thereof
CN110330320A
Cited By
Boat support and manufacturing method thereof
CN119751095A
Boat support and manufacturing method thereof
CN119751095B
Preparation method of high-purity polycrystalline silicon carbide substrate
CN121472998A