Efficient lossless dry film removing liquid and preparation method thereof

By adding polyethyleneimine, PAMAM and alkylamide to the film removal liquid, using hydrogen bond and interface modification technology, the dry film on the copper-plated alloy ITO conductive film is effectively removed without loss, and the traditional film removal is solved The problem of low corrosion and removal efficiency of the conductive film on liquid significantly improves the yield and film removal efficiency.

CN118895183APending Publication Date: 2024-11-05SHENZHEN FISHER NEW MATERIALS CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410922154.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The traditional inorganic alkali film removal liquid has corrosion damage to the copper-plated alloy ITO conductive film, and the film removal efficiency is low, so it cannot efficiently remove fine dry films, resulting in low yield.

Method used

Using a high-efficiency non-destructive dry film removal liquid, including water, defoaming agent, organic solvent, surfactant, polyethyleneimine, PAMAM, alkylamide and organic base, the hydrolysis of ester bonds by catalyzing hydroxide ion, amine The radical functional groups form hydrogen bonds and react with the dry film, rapid penetration of polyethyleneimine and interface modification, combining the effects of PAMAM and surfactant to achieve efficient dissolution and removal of the dry film.

Benefits of technology

The dry film removal efficiency and yield rate are significantly improved, and corrosion damage to the ITO conductive film and copper substrate are avoided. The concentration of the film removal liquid can be reduced and the efficiency is high, the removal time is shortened, and the quality of sensor manufacturing is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004937022410000081
    Figure BDA0004937022410000081
Patent Text Reader

Abstract

The invention relates to the field of electronic materials, and particularly discloses an efficient lossless dry film removing liquid and a preparation method thereof.The dry film removing liquid is prepared from, by weight, 50-70 parts of water, 0.5-1.5 parts of a defoaming agent, 10-20 parts of an organic solvent, 5-13 parts of a surfactant, 5-10 parts of polyethyleneimine, 3-5 parts of PAMAM, 1-3 parts of a corrosion inhibitor, 3-5 parts of alkyl amide and 15-20 parts of organic alkali; the preparation method comprises the following steps: mixing the surfactant and the water according to the ratio, then adding the organic solvent, the organic alkali, the polyethyleneimine, the PAMAM and the alkylamide for mixing, and finally adding the corrosion inhibitor and the defoaming agent for mixing to prepare the dry film removing liquid. The prepared dry film removing liquid is an organic film removing liquid capable of efficiently removing a dry film, and has no corrosion damage to an indium tin oxide conductive film and a copper base material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electronic materials, and more specifically, to a highly efficient and non-destructive dry film remover and a preparation method thereof. Background Art

[0002] Copper alloy indium selenide oxide (ITO) conductive film is a transparent conductive material, mainly composed of indium oxide (In2O3) and a small amount of tin oxide (SnO2). This material has the characteristics of high transparency, low resistivity, good thermal stability and chemical stability. Among them, the high transparency (up to 85% to 90%) makes ITO conductive film perform well in optical devices, while the low resistivity (usually 10 -4 Up to 10 -3 Ω·cm range) ensures its good electrical conductivity.

[0003] By plating copper alloy on the ITO conductive film, its conductive performance and stability can be further improved. As an excellent conductive material, copper combined with ITO can form a more stable and efficient conductive channel. In addition, copper alloy plating can also enhance the corrosion resistance and wear resistance of the ITO conductive film, so that it can maintain stable performance in various environments.

[0004] In the process of preparing sensors using copper alloy indium selenide oxide (ITO) conductive film, an ITO conductive film coating is sputtered on a substrate by magnetron sputtering and subjected to high temperature annealing to obtain an indium tin oxide conductive film, and then a layer of copper alloy is plated on the TTO conductive film to form a copper alloy indium tin oxide conductive film. The obtained copper alloy ITO conductive film has a wide range of applications in touch sensors, photoelectric sensors, chemical sensors, and biosensors.

[0005] In the manufacturing process of the sensor, in order to form the required circuit pattern and structure, a layer of dry film is usually first attached to the ITO conductive film. This layer of dry film will act as a template in the subsequent development, etching and other process steps. When the circuit pattern is transferred to the ITO conductive film through the etching process, this layer of dry film is no longer needed and needs to be removed so that the subsequent process can continue. In the process of removing the dry film, a specific film stripping solution is required to dissolve and remove the dry film. For the copper alloy-plated ITO conductive film, the effect of the film stripping solution on ITO and copper alloy needs to be specially considered to ensure that the performance of the ITO conductive film will not be damaged while removing the dry film.

[0006] At present, traditional film stripping solutions are mainly alkaline substances such as sodium hydroxide or potassium hydroxide. However, traditional inorganic alkaline film stripping solutions are corrosive to the conductive film substrate, causing the resistance of the conductive film to increase. In addition, the amount of foaming is large, and it is impossible to peel off the dry film with a high degree of photosensitive fineness. It is not easy to clean and may cause white spots and low yield. Therefore, there is an urgent need to develop an organic film stripping solution that can efficiently remove the dry film and has no corrosion damage to the indium tin oxide conductive film and the copper substrate, so as to improve the yield. Summary of the invention

[0007] In order to prepare an organic film stripping solution that can efficiently remove dry film without causing corrosion damage to the indium tin oxide conductive film and the copper substrate, the present application provides a highly efficient and non-destructive dry film stripping solution and a preparation method thereof.

[0008] In the first aspect, the present application provides an efficient and non-destructive dry film remover, which adopts the following technical solution: A highly efficient and non-destructive dry film stripping liquid comprises the following raw materials in parts by weight: 50-70 parts of water, 0.5-1.5 parts of defoaming agent, 10-20 parts of organic solvent, 5-13 parts of surfactant, 5-10 parts of polyethyleneimine, 3-5 parts of PAMAM, 1-3 parts of corrosion inhibitor, 3-5 parts of alkylamide and 15-20 parts of organic base.

[0009] By adopting the above technical scheme, the present application further adds polyethyleneimine and PAMAM on the basis of organic base. The hydroxide ions in the organic base can catalyze the hydrolysis of ester bonds to generate alcohols and carboxylic acids, and polyethyleneimine has multiple primary amine, secondary amine and tertiary amine groups. These amine functional groups can form hydrogen bonds with polar groups in the dry film, which helps to weaken the intermolecular forces inside the dry film, making it easier to be dissolved by the film removal liquid. In addition, the amine groups react with the dry film polymer to make its structure loose, accelerating the dissolution process. In addition, polyethyleneimine can quickly penetrate into the micropores and cracks of the dry film, increasing the contact area between the film removal liquid and the dry film, thereby improving the film removal efficiency. In addition, polyethyleneimine acts as an interfacial modifier and interacts with the surface of the film material through the amine groups to reduce the adhesion between the dry film and the substrate, thereby facilitating the removal of the dry film. In addition, polyethyleneimine can also form a stable complex with metal, thereby preventing the stripping solution from corroding copper. It was found that when polyethyleneimine was added to the stripping solution, the organic stripping solution of the dry film could be efficiently removed, with better removal effect, and no corrosion damage to the indium tin oxide conductive film and the copper substrate, and the yield rate was significantly improved; In addition, the addition of PAMAM in the present application not only interacts with the surface energy of the dry film through the amine group, affects the stability of the dry film, causes the destruction of the dry film structure, and thus achieves the removal of the dry film, but PAMAM also acts as a surfactant, which helps PAMAM to form a thin covering layer on the surface of the dry film, thereby changing the surface properties of the dry film, making it easier to be wetted and hydrolyzed, and improving its film removal efficiency and effect. Finally, the composite addition of polyethyleneimine and PAMAM significantly improves the film removal effect while not causing corrosion damage to the indium tin oxide conductive film and the copper substrate, thereby improving the yield rate.

[0010] The addition of alkylamide in this application can form hydrogen bonds with the polymer in the dry film, destroy the intermolecular forces of the dry film, make it easier to dissolve, and improve the efficiency and rate of dry film removal; the addition of surfactant can reduce the surface tension of the film stripping solution, improve its wettability to the film, and thus accelerate the dissolution process of the dry film; the addition of chelating agent ensures that the copper plating layer on the ITP conductive film layer will not be oxidized and corroded. Finally, the dry film stripping solution prepared in this application can efficiently remove the organic film stripping solution of the dry film, and has no corrosion damage to the indium tin oxide conductive film and the copper substrate.

[0011] Optionally, the alkyl amide is selected from one or both of acetamide and acrylamide.

[0012] By adopting the above technical solution, acetamide and acrylamide may assist in removing the dry film by affecting the adhesion and friction coefficient between the dry film and the substrate. It was found that when the above substances were added to the dry film remover, the dry film removal effect was further improved.

[0013] Optionally, the raw materials of the dry film stripping solution further include 1-3 parts by weight of diphenyl phosphate.

[0014] By adopting the above technical scheme, diphenyl phosphate has an acid-base dual functional group. On the one hand, the acidic part reacts with the ester bond in the polyester molecular chain to reduce the stability of the ester bond. On the other hand, the alkaline part participates in the hydrolysis reaction, promotes the attack of water molecules, and accelerates direct breakage, thereby promoting the hydrolysis of polyester. The addition of diphenyl phosphate in the dry film remover further improves the dry film removal effect.

[0015] Optionally, the surfactant is selected from one or more of polyoxyethylene octylphenol ether, sodium alkylbenzene sulfonate, sodium dodecyl sulfate and fatty alcohol polyoxyethylene ether phosphate.

[0016] Optionally, the surfactant is sodium alkylbenzene sulfonate and fatty alcohol polyoxyethylene ether phosphate in a mass ratio of 1: (0.6-0.8).

[0017] By adopting the above technical scheme, sodium alkylbenzene sulfonate (LAS) and fatty alcohol polyoxyethylene ether phosphate (AEO phosphate) are mixed as surfactants in the dry film removal liquid on the copper indium tin oxide conductive film. The sulfonic acid group in the sodium alkylbenzene sulfonate has strong hydrophilicity and excellent emulsifying properties, which helps to remove the dry film, and the polyoxyethylene chain segment in the fatty alcohol polyoxyethylene ether phosphate can reduce the surface tension of the film removal liquid, which is beneficial to enhance the wettability and permeability of the film removal liquid, making it easier for the dry film removal liquid to penetrate into the dry film, weakening the adhesion between the dry film and the substrate, and improving the removal ability. In addition, the phosphate group in the fatty alcohol polyoxyethylene ether phosphate can better combine with the ester group and impurities in the dry film, which helps to disperse the oil and impurities in the dry film into the water phase, forming a stable dispersion system, making it easier to be cleaned, thereby enhancing the removal effect of the dry film.

[0018] Optionally, the organic base is selected from one or more of tetramethylammonium hydroxide, ethanolamine, ammonia water, ethylenediamine, polyethylene polyamine.

[0019] Optionally, the organic solvent is one or more of isopropanol, ethanol, propylene glycol, and glycerol.

[0020] By adopting the above technical solution, the above organic solvent can be selected to dissolve and disperse the organic matter in the dry film, thereby achieving the removal of the dry film.

[0021] Optionally, the defoaming agent is a polyether defoaming agent; the corrosion inhibitor is benzotriazole and its derivatives.

[0022] Optionally, the water is tap water and micro-nano bubble water in a mass ratio of 1:(1-1.2). The micro-nano bubble water is prepared by using tap water as a water source and nitrogen as an aeration source, and is aerated for 5-10 minutes with an air intake of 5-8 L / min by a micro-nano bubble aerator and then left to stand.

[0023] By adopting the above technical solution, since the interfacial potential of micro-nano bubble water affects the adsorption performance of the bubble surface, it is found that when micro-nano degassing water is added to the defilming liquid, the removal effect and efficiency of the dry film are better, and the substrate will not be damaged.

[0024] In a second aspect, the present application provides a method for preparing an efficient and non-destructive dry film remover, which adopts the following technical solution: A method for preparing an efficient and non-destructive dry film remover comprises the following steps: The surfactant is mixed with water according to a ratio, and then an organic solvent, an organic base, polyethyleneimine, PAMAM and an alkylamide are added and mixed, and finally a corrosion inhibitor and a defoaming agent are added and mixed to prepare a dry film removing liquid.

[0025] By adopting the above technical solution, the method provided by the present application is simple, convenient and easy to operate.

[0026] Optionally, 1-3 parts by weight of diphenyl phosphate is added together with the alkyl amide.

[0027] In summary, this application has the following beneficial effects: 1. In addition to the organic base, the present application further adds polyethyleneimine. The hydroxide ions in the organic base can catalyze the hydrolysis of the ester bond to generate alcohol and carboxylic acid, and polyethyleneimine has multiple primary amine, secondary amine and tertiary amine groups. These amine functional groups can form hydrogen bonds with the polar groups in the dry film, which helps to weaken the intermolecular forces inside the dry film, making it easier to be dissolved by the film stripping solution. In addition, the amine groups react with the dry film polymer to loosen its structure and accelerate the dissolution process. In addition, polyethyleneimine can quickly penetrate into the micropores and cracks of the dry film, increase the contact area between the film stripping solution and the dry film, thereby improving the film stripping efficiency. In addition, polyethyleneimine, as an interfacial modifier, interacts with the surface of the film material through the amine groups, reduces the adhesion between the dry film and the substrate, thereby facilitating the removal of the dry film. In addition, polyethyleneimine can also form a stable complex with metal, thereby preventing the stripping solution from corroding copper. It was found that when polyethyleneimine was added to the stripping solution, the organic stripping solution of the dry film could be efficiently removed, with better removal effect, and no corrosion damage to the indium tin oxide conductive film and the copper substrate, and the yield rate was significantly improved; 2. The addition of PAMAM in this application not only affects the stability of the dry film through the interaction between the amine group and the surface energy of the dry film, causing the destruction of the dry film structure, thereby achieving the removal of the dry film, but also acts as a surfactant, which helps PAMAM to form a thin covering layer on the surface of the dry film, thereby changing the surface properties of the dry film, making it easier to be wetted and hydrolyzed, and improving its film removal efficiency and effect. Finally, the composite addition of polyethyleneimine and PAMAM significantly improves the film removal effect while not causing corrosion damage to the indium tin oxide conductive film and the copper substrate, thereby improving the yield rate; 3. The addition of alkylamide in this application, the amide group can form hydrogen bonds with the polymer in the dry film, destroy the intermolecular forces of the dry film, make it easier to dissolve, and improve the efficiency and rate of dry film removal; the addition of surfactant can reduce the surface tension of the stripping solution, improve its wettability to the film, and thus accelerate the dissolution process of the dry film; the addition of chelating agent ensures that the copper plating layer on the ITP conductive film layer will not be oxidized and corroded. Finally, the dry film stripping solution prepared in this application can efficiently remove the organic stripping solution of the dry film, and has no corrosion damage to the indium tin oxide conductive film and the copper substrate; 4. The diphenyl phosphate added in the present application has an acid-base dual functional group. On the one hand, the acidic part reacts with the ester bond in the polyester molecular chain to reduce the stability of the ester bond. On the other hand, the alkaline part participates in the hydrolysis reaction, promotes the attack of water molecules, and accelerates direct breakage, thereby promoting the hydrolysis of polyester. The addition of diphenyl phosphate in the dry film remover further improves the dry film removal effect. DETAILED DESCRIPTION

[0028] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0029] At present, inorganic bases such as potassium hydroxide are mainly used for dry film removal, but it is found that inorganic bases are corrosive to the conductive film substrate, causing the resistance of the conductive film to increase, and it is necessary to study new dry film removers. Although some documents also record the use of inorganic bases such as tetramethylammonium hydroxide, ethanolamine, ammonia water, ethylenediamine, and polyethylene polyamine for dry film removal, it is found that when the above inorganic bases are used for removal, on the one hand, the removal efficiency is low, and the time to completely remove the dry film is difficult to exceed 30 seconds, and when the dry film is removed, the concentration of the dry film remover is relatively high. After a lot of research and experiments by the applicant, it was found that when polyethyleneimine, PAMAM and alkylamide are added to the dry film remover, the dry film removal efficiency is significantly improved, and the time for complete removal of the dry film is greatly shortened. Moreover, when the dry film is removed, a lower concentration of the dry film remover can achieve a higher removal efficiency, and the dry film on the copper-plated ITO conductive film can be completely removed in a shorter time.

[0030] The polyether defoamer in the following examples is polyether L61.

[0031] Example 1 A method for preparing an efficient and non-destructive dry film remover comprises the following steps: 9 g of surfactant was mixed with 60 g of tap water, and then 15 g of organic solvent, 18 g of organic base, 8 g of polyethyleneimine, 4 g of PAMAM, and 4 g of alkylamide were added and mixed, and finally 2 g of corrosion inhibitor and 1.0 g of polyether defoamer were added and mixed to prepare a dry film removal liquid.

[0032] Among them, the surfactant is sodium dodecylbenzene sulfonate and sodium isooctyl polyoxyethylene ether phosphate in a mass ratio of 1:0.7, the organic base is diethanolamine, the organic solvent is propylene glycol, the corrosion inhibitor is benzotriazole (BTA), and the alkyl amide is acetamide.

[0033] Example 2 A method for preparing an efficient and non-destructive dry film remover comprises the following steps: 5g of surfactant was mixed with 50g of tap water, and then 10g of organic solvent, 15g of organic base, 5g of polyethyleneimine, 3g of PAMAM, and 3g of alkylamide were added and mixed, and finally 1g of corrosion inhibitor and 0.5g of polyether defoamer were added and mixed to prepare a dry film removal liquid.

[0034] Among them, the surfactant is sodium dodecylbenzene sulfonate and sodium isooctyl polyoxyethylene ether phosphate in a mass ratio of 1:0.6, the organic base is tetramethylammonium hydroxide, the organic solvent is glycerol, the corrosion inhibitor is benzotriazole (BTA), and the alkyl amide is acrylamide.

[0035] Example 3 A method for preparing an efficient and non-destructive dry film remover comprises the following steps: 13g of surfactant was mixed with 70g of tap water, and then 20g of organic solvent, 20g of organic base, 10g of polyethyleneimine, 5g of PAMAM, and 5g of alkylamide were added and mixed, and finally 3g of corrosion inhibitor and 1.5g of polyether defoamer were added and mixed to prepare a dry film removal liquid.

[0036] Among them, the surfactant is sodium dodecylbenzene sulfonate and sodium isooctyl polyoxyethylene ether phosphate in a mass ratio of 1:0.8, the organic base is ethylenediamine, the organic solvent is ethanol, the corrosion inhibitor is benzotriazole (BTA), and the alkyl amide is acetamide and acrylamide in a mass ratio of 1:1.

[0037] Example 4 A method for preparing an efficient and non-destructive dry film removing liquid is carried out according to the method in Example 1, except that sodium dodecylbenzene sulfonate is used as the surfactant.

[0038] Example 5 A method for preparing an efficient and non-destructive dry film remover is carried out according to the method in Example 1, except that sodium isooctyl polyoxyethylene ether phosphate is used as the surfactant.

[0039] Example 6 A method for preparing an efficient and non-destructive dry film remover is carried out according to the method in Example 1, except that an equal amount of sodium isooctyl polyoxyethylene ether phosphate in the surfactant is replaced by fatty alcohol polyoxyethylene ether AEO-9.

[0040] Example 7 A method for preparing an efficient and non-destructive dry film remover is carried out according to the method in Example 1, except that an equal amount of polyoxyethylene octylphenol ether sodium isooctyl alcohol ether phosphate in the surfactant is replaced by polyoxyethylene octylphenol ether.

[0041] Example 8 A method for preparing an efficient and non-destructive dry film remover is carried out according to the method in Example 1, except that an equal amount of sodium isooctyl polyoxyethylene ether phosphate in the surfactant is replaced by sodium dodecyl sulfate.

[0042] Example 9 A method for preparing an efficient and non-destructive dry film stripping solution is carried out according to the method in Example 1, except that 2 g of diphenyl phosphate is added at the same time as the alkyl amide.

[0043] Example 10 A method for preparing an efficient and non-destructive dry film stripping solution is carried out according to the method in Example 1, except that 1 g of diphenyl phosphate is added at the same time as the alkyl amide.

[0044] Embodiment 11 A method for preparing an efficient and non-destructive dry film stripping solution is carried out according to the method in Example 1, except that 3 g of diphenyl phosphate is added at the same time as the alkyl amide.

[0045] Example 12 A method for preparing an efficient and non-destructive dry film removal liquid is carried out according to the method in Example 1, except that tap water and micro-nano bubble water are selected in a mass ratio of 1:1. The micro-nano bubble water uses tap water as a water source, and then uses nitrogen as an aeration source. The micro-nano bubble water is prepared by a micro-nano bubble aerator, aerated for 10 minutes with an air intake of 5 L / min, and then allowed to stand for 1 hour to obtain the micro-nano bubble water.

[0046] Embodiment 13 A method for preparing an efficient and non-destructive dry film removal liquid is carried out according to the method in Example 1, except that tap water and micro-nano bubble water are selected in a mass ratio of 1:1.2. The micro-nano bubble water uses tap water as a water source, and then uses nitrogen as an aeration source. The micro-nano bubble water is prepared by a micro-nano bubble aerator with an air intake of 8 L / min, aerated for 5 minutes, and then allowed to stand for 1 hour to obtain the micro-nano bubble water.

[0047] Comparative Example 1 A method for preparing a dry film stripping solution is carried out according to the method in Example 1, except that polyethyleneimine, PAMAM and alkylamide are not added to the raw materials.

[0048] Comparative Example 2 A method for preparing a dry film stripping solution is carried out according to the method in Example 1, except that an equal amount of polyethyleneimine is replaced by diethanolamine.

[0049] Comparative Example 3 A method for preparing a dry film stripping solution is carried out according to the method in Example 1, except that PAMAM is replaced by diethanolamine in equal amounts.

[0050] Comparative Example 4 A method for preparing a dry film stripping solution is carried out according to the method in Example 1, except that acetamide is not added to the raw materials.

[0051] Comparative Example 5 A method for preparing a dry film stripping solution is carried out according to the method in Example 1, except that an equal amount of acetamide is replaced by diethanolamine.

[0052] Comparative Example 6 A method for preparing a dry film stripping solution is carried out according to the method in Example 1, except that the amount of alkyl amide added is 2 g.

[0053] Comparative Example 7 A method for preparing a dry film stripping solution is carried out according to the method in Example 1, except that the added amount of polyethyleneimine is 4 g and the added amount of PAMAM is 2 g.

[0054] Performance Testing The dry film stripping solution prepared in the above embodiments and comparative examples was diluted with water to a weight percentage of 6wt%, and the removal time of the dry film on the copper-plated alloy ITO conductive film (no residual glue on the surface after stripping, the time for complete removal of the dry film) and the effect on the copper-plated alloy ITO conductive film were statistically analyzed. The stripping temperature was 55°C, and the statistical results are shown in Table 1 below.

[0055] Table 1: In addition, in the above-mentioned film removal process, it can be observed that the dry film is peeled off in small pieces. Combined with the test results in Table 1 above, it can be seen that the film removal solution in this application has a higher removal efficiency for the dry film on the copper alloy ITO conductive film, and it will not damage TTO or corrode the copper alloy. Combined with the test results of Example 1 in Table 1 and Examples 4 and 5, it can be seen that when only one of sodium dodecyl sulfonate or sodium isooctyl alcohol polyoxyethylene ether phosphate is selected as the surfactant, the removal efficiency is reduced, especially when sodium dodecyl sulfonate is selected, the effect is more significantly reduced. Combined with the test results of Example 6, when the sodium isooctyl alcohol polyoxyethylene ether phosphate in Example 6 is replaced by fatty alcohol polyoxyethylene ether AEO-9 in equal amounts, its removal efficiency is improved compared with Example 5, but it is still weaker than Example 1. Combined with the test results of Examples 7 and 8, when the surfactant is selected from sodium dodecylbenzene sulfonate and compounded with other types of surfactants, its effect is reduced compared with Example 1.

[0056] Referring to the test results of Examples 9-11, it can be seen that when diphenyl phosphate is added to the dry film remover, the removal efficiency and removal time of the dry film can be further improved, and no loss or corrosion will be caused. Combined with the test results of Examples 12 and 13, it can be seen that when part of the water is replaced by micro-nano bubble water, the dry film removal efficiency and removal time are further improved, especially the removal time is shortened to within 30 seconds, which makes a prominent breakthrough in the dry film removal time, and does not damage ITO and does not cause corrosion to copper alloy.

[0057] Referring to the test results of Example 1 and Comparative Example 1, it can be seen that when polyethyleneimine, PAMAM and alkylamide are not added to the raw material, the dry film removal time is long, up to 55s, and the removal rate is also reduced. Referring to the test results of Comparative Examples 2 and 3, it can be seen that when polyethyleneimine or PAMAM is replaced with diethanolamine, a common organic base, the dry film removal time is long. Combined with the test results of Comparative Examples 4 and 5, when alkylamide is not added to the raw material, the removal efficiency is significantly reduced, and the addition of alkylamide further improves the dry film removal efficiency. Referring to the test results of Example 1 and Comparative Examples 6 and 7, it can be seen that when the amount of alkylamide, polyethyleneimine or PAMAM added is too small, although it has a certain effect on dry film removal, the effect is far weaker than the result in Example 1.

[0058] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A highly efficient and non-destructive dry film remover, characterized in that: It includes the following raw materials in parts by weight: 50-70 parts of water, 0.5-1.5 parts of defoaming agent, 10-20 parts of organic solvent, 5-13 parts of surfactant, 5-10 parts of polyethyleneimine, 3-5 parts of PAMAM, 1-3 parts of corrosion inhibitor, 3-5 parts of alkylamide and 15-20 parts of organic base.

2. The high-efficiency non-destructive dry film remover according to claim 1, characterized in that: The alkyl amide is selected from one or both of acetamide and acrylamide.

3. The high-efficiency non-destructive dry film remover according to claim 1, characterized in that: The raw materials of the dry film stripping solution also include 1-3 parts by weight of diphenyl phosphate.

4. The high-efficiency non-destructive dry film remover according to claim 1, characterized in that: The surfactant is selected from one or more of polyoxyethylene octylphenol ether, sodium alkylbenzene sulfonate, sodium dodecyl sulfate and fatty alcohol polyoxyethylene ether phosphate.

5. The high-efficiency non-destructive dry film remover according to claim 1, characterized in that: The surfactant is selected from sodium alkylbenzene sulfonate and fatty alcohol polyoxyethylene ether phosphate in a mass ratio of 1: (0.6-0.8).

6. The high-efficiency non-destructive dry film remover according to claim 1, characterized in that: The organic base is selected from one or more of tetramethylammonium hydroxide, ethanolamine, ammonia water, ethylenediamine, polyethylene polyamine.

7. The high-efficiency non-destructive dry film remover according to claim 1, characterized in that: The organic solvent is selected from one or more of isopropanol, ethanol, propylene glycol and glycerol.

8. The high-efficiency non-destructive dry film remover according to claim 1, characterized in that: The defoamer is a polyether defoamer; the corrosion inhibitor is benzotriazole and its derivatives.

9. The method for preparing the high-efficiency non-destructive dry film remover as claimed in claim 1, characterized in that: The following steps are involved: The surfactant is mixed with water according to a ratio, and then an organic solvent, an organic base, polyethyleneimine, PAMAM and an alkylamide are added and mixed, and finally a corrosion inhibitor and a defoaming agent are added and mixed to prepare a dry film removing liquid.

10. The method for preparing a highly efficient and non-destructive dry film remover according to claim 9, characterized in that: 1-3 parts by weight of diphenyl phosphate are added together with the alkyl amide.

Citation Information

Cited By

  • Environment-friendly film removing liquid and preparation method thereof

    CN119506018A

  • An environmentally friendly film-removing liquid and its preparation method

    CN119506018B

  • Film stripping liquid suitable for dry film after plasma treatment and use method of film stripping liquid