Polytetrafluoroethylene nanofiber membrane using solution injection technology and preparation method thereof
Preparation of polytetrafluoroethylene nanofiber membranes through solution spraying technology solves the problems of high voltage and slow spinning speed in electrospinning method, and realizes high-efficiency and low-energy consumption nanofiber membrane preparation, which is suitable for industrial production and improves Fiber strength and durability.
Patent Information
- Application Number
- CN202411401949.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, the preparation of polytetrafluoroethylene nanofiber membranes by electrospinning method has problems such as high voltage, slow spinning speed, large energy consumption and low yield, making it difficult to achieve industrial production.
The polytetrafluoroethylene nanofiber membrane was prepared by solution spraying technology. The nanofibers were formed by stretching the polytetrafluoroethylene/polyethylene oxide spinning liquid at high speed airflow, and sintering it in a muffle furnace to remove polyethylene oxide. Alkane is obtained to obtain a polytetrafluoroethylene nanofiber membrane.
It has achieved significant improvement in spinning speed, reduced energy consumption, high production efficiency, tight fiber structure and high strength, and has good high temperature and chemical corrosion resistance, which is suitable for industrial production.
Smart Images

Figure CN118895607A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polytetrafluoroethylene nanofiber membrane utilizing a solution spraying technology and a preparation method thereof, belonging to the technical field of nanofiber preparation. Background Art
[0002] Polytetrafluoroethylene (PTFE) molecules are completely symmetrical, unbranched linear polymers. The appropriate atomic radius of the fluorine atom enables it to fill the gap between two carbon atoms and surround it around the CC main chain to form a low surface energy protective layer, giving the polytetrafluoroethylene material excellent chemical inertness.
[0003] Due to the high rigidity and chemical stability of polytetrafluoroethylene molecules, it is impossible to use traditional solution spinning and melt spinning methods to prepare polytetrafluoroethylene fiber materials. So far, the main methods for preparing polytetrafluoroethylene fibers include carrier spinning, paste extrusion spinning, electrospinning, membrane splitting spinning, etc. Electrospinning is the most common method for preparing nanofiber membranes. The polymer solution is stretched and refined into nanofibers under the action of a high electric field.
[0004] Most of the polytetrafluoroethylene nanofiber membranes currently published are prepared by the above-mentioned electrospinning method. The patent with publication number CN105862256A discloses a method for preparing polytetrafluoroethylene nanofiber porous membranes by polyethylene oxide (PEO) template sacrificial method, and the PEO / PTFE spinning solution is electrospun to form a PEO / PTFE primary composite nanofiber membrane, and then heat-treated to obtain a polytetrafluoroethylene nanofiber membrane. The patent with publication number CN116575184B discloses a method for preparing a polytetrafluoroethylene nanofiber membrane, using an electrospinning method and a modified spinning precursor to improve the tensile strength and weather resistance of the polytetrafluoroethylene nanofiber membrane. However, the above-mentioned electrospinning preparation of polytetrafluoroethylene nanofiber membranes has a voltage of up to 20KV and a spinning speed of only about 0.6mL / h, which has the defects of high energy consumption and low yield, making it difficult to industrialize production. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a polytetrafluoroethylene nanofiber membrane and a preparation method thereof using a solution blowing technology, which has a fast spinning speed, a simple and efficient preparation process, and is conducive to industrialization.
[0006] To achieve the above object, the present invention is implemented by adopting the following technical solutions: In one aspect, the present invention provides a method for preparing a polytetrafluoroethylene nanofiber membrane using a solution blowing technique, comprising: preparing polytetrafluoroethylene / polyethylene oxide spinning solution; The polytetrafluoroethylene / polyethylene oxide spinning solution is stretched by an air-jet spinning machine to obtain polytetrafluoroethylene / polyethylene oxide nanofibers; depositing polytetrafluoroethylene / polyethylene oxide nanofibers on a collecting roller to form a polytetrafluoroethylene / polyethylene oxide nanofiber membrane; The polytetrafluoroethylene / polyethylene oxide nanofiber membrane is sintered to remove the polyethylene oxide, thereby obtaining a polytetrafluoroethylene nanofiber membrane.
[0007] Furthermore, the preparation of polytetrafluoroethylene / polyethylene oxide spinning solution comprises: The polytetrafluoroethylene emulsion and the polyethylene oxide aqueous solution are mixed and stirred to obtain a polytetrafluoroethylene / polyethylene oxide mixed solution; The polytetrafluoroethylene / polyethylene oxide mixed solution is allowed to stand and bubbles are removed to obtain a polytetrafluoroethylene / polyethylene oxide spinning solution.
[0008] Furthermore, the mass ratio of the polyethylene oxide to the polytetrafluoroethylene is 1-2:10.
[0009] Furthermore, the conditions and parameters of the air-jet spinning machine for obtaining polytetrafluoroethylene / polyethylene oxide nanofibers by stretching the polytetrafluoroethylene / polyethylene oxide spinning solution include an air flow pressure range of 0.03~0.08MPa, an extrusion rate of 3~15mL / h, a temperature range of 40~45°C, and a humidity range of less than 30%.
[0010] Furthermore, the collecting roller used in the process of depositing the polytetrafluoroethylene / polyethylene oxide nanofibers on a collecting roller to form the polytetrafluoroethylene / polyethylene oxide nanofiber membrane is a constant speed rotating collecting roller, and the rotation speed range of the collecting roller is 60-120 rpm.
[0011] Furthermore, a hydrophobic anti-sticking non-woven fabric is laid on the collecting roller, and the hydrophobic anti-sticking non-woven fabric is used to prevent the polytetrafluoroethylene / polyethylene oxide nanofiber membrane from sticking to the collecting roller.
[0012] Furthermore, the sintering is achieved by a muffle furnace, which includes stepwise heating at 0.5-2°C / min to 360-400°C and maintaining for 8-12 minutes.
[0013] On the other hand, the present invention also provides a polytetrafluoroethylene nanofiber membrane, which is prepared by any of the above-mentioned methods for preparing the polytetrafluoroethylene nanofiber membrane.
[0014] Furthermore, the diameter of the nanofibers of the polytetrafluoroethylene nanofiber membrane is at a micro-nano scale, and the pore size is uniform.
[0015] Furthermore, under a low pressure drop of 100 Pa, the flow rate of gas passing through the polytetrafluoroethylene nanofiber membrane is in the range of 1.0-1.4 m / min.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention prepares polytetrafluoroethylene nanofiber membranes through solution blowing technology. The solution blowing technology uses high-speed airflow as a stretching driving force. The solvent overcomes the surface tension of the solution to volatilize, and the solute is stretched to obtain nanofibers. Compared with the electrostatic spinning process, the fiber stretching and thinning can be achieved without high voltage, which is safe and reliable, with low energy consumption. At the same time, multiple needles can be co-spinned with little mutual influence. The spinning speed can reach dozens of times the electrostatic spinning speed, with high practical application value. At the same time, the fibers can be flexibly deposited on the surfaces of various receivers, which is more convenient to use, with high production efficiency and industrialization. The polytetrafluoroethylene nanofiber membrane prepared by the solution blowing technology of the present invention uses polytetrafluoroethylene concentrated dispersion as raw material and polyethylene oxide as spinning carrier of polytetrafluoroethylene. No modification additives are required, and the preparation process is simple and efficient. The polytetrafluoroethylene nanofiber membrane after sintering has a compact fiber structure, few impurities, and high strength of the nanofiber membrane. At the same time, it has excellent high temperature resistance and chemical corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A schematic diagram of the process flow of the solution spraying technology in one embodiment of the present invention; Figure 2 A schematic diagram of a process for preparing a polytetrafluoroethylene nanofiber membrane in an embodiment of the present invention; Figure 3 This is a SEM schematic diagram of the polytetrafluoroethylene nanofiber membrane prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0019] Example 1
[0020] like Figure 1 and Figure 2 As shown, an embodiment of the present invention provides a method for preparing a polytetrafluoroethylene nanofiber membrane using a solution blowing technology, comprising the following steps: A 15% polyethylene oxide aqueous solution and a 60wt% polytetrafluoroethylene concentrated dispersion were mixed in a mass ratio of 1:2, wherein the mass ratio of polyethylene oxide to polytetrafluoroethylene was 1:8, stirred at 50°C for 10 hours in a water bath magnetic stirrer, and allowed to stand for 5 hours to remove internal bubbles, to obtain a uniform polytetrafluoroethylene / polyethylene oxide spinning solution.
[0021] The polytetrafluoroethylene / polyethylene oxide spinning solution is stretched by an air-jet spinning machine to obtain polytetrafluoroethylene / polyethylene oxide nanofibers. Specifically, the microwave heating and dehumidification device of the air-jet spinning machine is turned on, the spinning environment temperature is controlled to be 45°C and the humidity is controlled to be 26%, the polytetrafluoroethylene / polyethylene oxide spinning solution is loaded into a syringe, and the propulsion device extrude the spinning solution at a rate of 6 mL / h. Under the set ambient temperature and humidity conditions, the spinning solution is stretched with a high-speed airflow of 0.04 MPa, the solution in the spinning solution overcomes the surface tension of the solution to volatilize, and the solute is stretched to obtain polytetrafluoroethylene / polyethylene oxide nanofibers.
[0022] A layer of hydrophobic and anti-sticking non-woven fabric is laid on the collecting roller in advance, which is conducive to the collection and peeling of the nanofiber membrane. The polytetrafluoroethylene / polyethylene oxide nanofibers are deposited on the collecting roller covered with the non-woven fabric under the action of airflow to form a polytetrafluoroethylene / polyethylene oxide nanofiber membrane, wherein the rotation speed of the collecting roller is 100rpm.
[0023] The polytetrafluoroethylene / polyethylene oxide nanofiber membrane was peeled off from the collecting roller and placed in a muffle furnace for sintering. The temperature of the muffle furnace was increased stepwise at 1°C / min to 370°C for sintering for 10 minutes. After sintering to remove the polyethylene oxide, a polytetrafluoroethylene nanofiber membrane was obtained.
[0024] like Figure 3 As shown, the prepared polytetrafluoroethylene nanofiber membrane has uniform fiber morphology and an average diameter of about 960 nm. The fibers are interwoven to form a three-dimensional network structure, which makes it more advantageous in applications such as filtration and adsorption.
[0025] The air permeability test of the polytetrafluoroethylene nanofiber membrane showed that the gas flow rate of the polytetrafluoroethylene nanofiber membrane was 1.2m / min at a low pressure drop of 100MPa. The pressure drop refers to the pressure difference on both sides of the membrane.
[0026] Example 2
[0027] This embodiment provides a method for preparing a polytetrafluoroethylene nanofiber membrane using a solution blowing technique, comprising the following steps: A 15% polyethylene oxide aqueous solution and a 60wt% polytetrafluoroethylene concentrated dispersion were mixed in a mass ratio of 1:1.75, wherein the mass ratio of polyethylene oxide to polytetrafluoroethylene was 1:7, stirred at 50°C for 10 hours in a water bath magnetic stirrer, and allowed to stand for 5 hours to remove internal bubbles, to obtain a uniform polytetrafluoroethylene / polyethylene oxide spinning solution.
[0028] The polytetrafluoroethylene / polyethylene oxide spinning solution is stretched by an air-jet spinning machine to obtain polytetrafluoroethylene / polyethylene oxide nanofibers. Specifically, the microwave heating and dehumidification device of the air-jet spinning machine is turned on, the spinning environment temperature is controlled to be 45°C and the humidity is controlled to be 26%, the polytetrafluoroethylene / polyethylene oxide spinning solution is loaded into a syringe, and the propulsion device extrude the spinning solution at a rate of 6 mL / h. Under the set ambient temperature and humidity conditions, the spinning solution is stretched with a high-speed airflow of 0.04 MPa, the solution in the spinning solution overcomes the surface tension of the solution to volatilize, and the solute is stretched to obtain polytetrafluoroethylene / polyethylene oxide nanofibers.
[0029] A layer of hydrophobic and anti-sticking non-woven fabric is laid on the collecting roller in advance, which is conducive to the collection and peeling of the nanofiber membrane. The polytetrafluoroethylene / polyethylene oxide nanofibers are deposited on the collecting roller covered with the non-woven fabric under the action of airflow to form a polytetrafluoroethylene / polyethylene oxide nanofiber membrane, wherein the rotation speed of the collecting roller is 100rpm.
[0030] The polytetrafluoroethylene / polyethylene oxide nanofiber membrane was peeled off from the collecting roller and placed in a muffle furnace for sintering. The temperature of the muffle furnace was increased stepwise at 1°C / min to 370°C for sintering for 10 minutes. After sintering to remove the polyethylene oxide, a polytetrafluoroethylene nanofiber membrane was obtained.
[0031] The prepared polytetrafluoroethylene nanofiber membrane has uniform fiber morphology and an average diameter of about 986 nm, and the fibers are interwoven to form a three-dimensional network structure.
[0032] The air permeability test of the polytetrafluoroethylene nanofiber membrane showed that the gas flow rate of the polytetrafluoroethylene nanofiber membrane was 1.22 m / min at a low pressure drop of 100 MPa.
[0033] Example 3
[0034] This embodiment provides a method for preparing a polytetrafluoroethylene nanofiber membrane using a solution blowing technique, comprising the following steps: A 15% polyethylene oxide aqueous solution and a 60wt% polytetrafluoroethylene concentrated dispersion were mixed in a mass ratio of 1:2.25, wherein the mass ratio of polyethylene oxide to polytetrafluoroethylene was 1:9, stirred at 50°C for 10 hours in a water bath magnetic stirrer, and allowed to stand for 5 hours to remove internal bubbles, to obtain a uniform polytetrafluoroethylene / polyethylene oxide spinning solution.
[0035] The polytetrafluoroethylene / polyethylene oxide spinning solution is stretched by an air-jet spinning machine to obtain polytetrafluoroethylene / polyethylene oxide nanofibers. Specifically, the microwave heating and dehumidification device of the air-jet spinning machine is turned on, the spinning environment temperature is controlled to be 45°C and the humidity is controlled to be 26%, the polytetrafluoroethylene / polyethylene oxide spinning solution is loaded into a syringe, and the propulsion device extrude the spinning solution at a rate of 6 mL / h. Under the set ambient temperature and humidity conditions, the spinning solution is stretched with a high-speed airflow of 0.04 MPa, the solution in the spinning solution overcomes the surface tension of the solution to volatilize, and the solute is stretched to obtain polytetrafluoroethylene / polyethylene oxide nanofibers.
[0036] A layer of hydrophobic and anti-sticking non-woven fabric is laid on the collecting roller in advance, which is conducive to the collection and peeling of the nanofiber membrane. The polytetrafluoroethylene / polyethylene oxide nanofibers are deposited on the collecting roller covered with the non-woven fabric under the action of airflow to form a polytetrafluoroethylene / polyethylene oxide nanofiber membrane, wherein the rotation speed of the collecting roller is 100rpm.
[0037] The polytetrafluoroethylene / polyethylene oxide nanofiber membrane was peeled off from the collecting roller and placed in a muffle furnace for sintering. The temperature of the muffle furnace was increased stepwise at 1°C / min to 370°C for sintering for 10 minutes. After sintering to remove the polyethylene oxide, a polytetrafluoroethylene nanofiber membrane was obtained.
[0038] The prepared polytetrafluoroethylene nanofiber membrane has uniform fiber morphology and an average diameter of about 955 nm, and the fibers are interwoven to form a three-dimensional network structure.
[0039] The air permeability test of the polytetrafluoroethylene nanofiber membrane showed that the gas flow rate of the polytetrafluoroethylene nanofiber membrane was 1.12 m / min at a low pressure drop of 100 MPa.
[0040] The fiber diameters of the polytetrafluoroethylene nanofiber membranes prepared in Examples 1 to 3 and the air permeability flow rates after the air permeability test are shown in Table 1. The air permeability test refers to the standard GB / T 5453 for the determination of air permeability of fabrics, and the test area is 20 cm 2 : Test Parameters Example 1 Example 2 Example 3 Fiber diameter (nm) 960 986 955 Gas flow rate at 100MPa low pressure drop (m / min) 1.2 1.22 1.12 In principle, the fiber diameter and the air flow rate after the air permeability test are not linearly related. This is because when the fiber diameter increases, the pores between the fibers may become larger accordingly, which is conducive to the passage of gas to a certain extent, thereby improving the air permeability. However, the increase in fiber diameter may also cause the packing density of the fiber to change, or affect the structural uniformity of the fiber membrane, etc., and these factors may have an adverse effect on the air permeability. Combined with the data in Table 1, it can be seen from the comparison of Examples 1 to 3 that in order to obtain a suitable fiber diameter and air permeability, the mass ratio of polyethylene oxide to polytetrafluoroethylene is 1:8, which is the best, that is, Example 1 is the best. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the technical principles of the present invention, several improvements and deformations can be made, and these improvements and deformations should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a polytetrafluoroethylene nanofiber membrane using a solution blowing technique, characterized in that: include: preparing polytetrafluoroethylene / polyethylene oxide spinning solution; The polytetrafluoroethylene / polyethylene oxide spinning solution is stretched by an air-jet spinning machine to obtain polytetrafluoroethylene / polyethylene oxide nanofibers; depositing polytetrafluoroethylene / polyethylene oxide nanofibers on a collecting roller to form a polytetrafluoroethylene / polyethylene oxide nanofiber membrane; The polytetrafluoroethylene / polyethylene oxide nanofiber membrane is sintered to remove the polyethylene oxide, thereby obtaining a polytetrafluoroethylene nanofiber membrane.
2. The method for preparing a polytetrafluoroethylene nanofiber membrane using a solution spraying technique according to claim 1, characterized in that: The method for preparing polytetrafluoroethylene / polyethylene oxide spinning solution comprises: The polytetrafluoroethylene emulsion and the polyethylene oxide aqueous solution are mixed and stirred to obtain a polytetrafluoroethylene / polyethylene oxide mixed solution; The polytetrafluoroethylene / polyethylene oxide mixed solution is allowed to stand and bubbles are removed to obtain a polytetrafluoroethylene / polyethylene oxide spinning solution.
3. The method for preparing a polytetrafluoroethylene nanofiber membrane using a solution blowing technique according to claim 2, characterized in that: The mass ratio of the polyethylene oxide to the polytetrafluoroethylene is 1-2:
10.
4. The method for preparing a polytetrafluoroethylene nanofiber membrane using a solution spraying technique according to claim 1, characterized in that: The conditions and parameters of the air-jet spinning machine for obtaining polytetrafluoroethylene / polyethylene oxide nanofibers by stretching the polytetrafluoroethylene / polyethylene oxide spinning solution include an air flow pressure range of 0.03-0.08 MPa, an extrusion rate of 3-15 mL / h, a temperature range of 40-45° C., and a humidity range of less than 30%.
5. The method for preparing polytetrafluoroethylene nanofiber membrane using solution blowing technology according to claim 1, characterized in that: The collecting roller used in the process of depositing the polytetrafluoroethylene / polyethylene oxide nanofibers on a collecting roller to form the polytetrafluoroethylene / polyethylene oxide nanofiber membrane is a constant speed rotating collecting roller, and the rotation speed range of the collecting roller is 60-120 rpm.
6. The method for preparing a polytetrafluoroethylene nanofiber membrane using a solution spraying technique according to claim 5, characterized in that: The collecting roller is paved with a hydrophobic anti-sticking non-woven fabric, and the hydrophobic anti-sticking non-woven fabric is used to prevent the polytetrafluoroethylene / polyethylene oxide nanofiber membrane from adhering to the collecting roller.
7. The method for preparing polytetrafluoroethylene nanofiber membrane using solution spraying technology according to claim 1, characterized in that: The sintering is achieved by a muffle furnace, which includes stepwise heating at 0.5-2°C / min to 360-400°C and maintaining for 8-12 minutes.
8. A polytetrafluoroethylene nanofiber membrane, characterized in that: The nanofiber membrane is prepared by the method for preparing the polytetrafluoroethylene nanofiber membrane using solution blowing technology as described in any one of claims 1 to 7.
9. The polytetrafluoroethylene nanofiber membrane according to claim 8, characterized in that: The diameter of the nanofibers of the polytetrafluoroethylene nanofiber membrane is between 600 nm and 2.0 μm, and the pores formed between the nanofibers have uniform pore sizes.
10. The polytetrafluoroethylene nanofiber membrane according to claim 9, characterized in that: Under a low pressure drop of 100 Pa, the flow rate of gas passing through the polytetrafluoroethylene nanofiber membrane is in the range of 1.0-1.4 m / min.
Citation Information
Patent Citations
Method for preparing polytetrafluoroethylene (PTFE) nanofiber porous membrane by virtue of PEO template scarification method
CN105862256A
Method for preparing medical wound dressing by microfluidic gas jet spinning method
CN112921659A
Preparation method of flexible phenolic-based activated carbon fiber
CN113737317A
Preparation method of super-hydrophobic nanofiber membrane material
CN115946416A
Preparation method of polytetrafluoroethylene nanofiber membrane
CN116575184A
Cited By
Preparation method of polytetrafluoroethylene composite fiber membrane for sulfur removal based on solution injection
CN120662152A
Preparation method of polytetrafluoroethylene composite fiber membrane for desulfurization based on solution spraying
CN120662152B