Laser-assisted thick copper microwave plate processing method

Through the laser-assisted thick copper microwave plate processing method, the combination of laser thinning and chemical etching is used to solve the problems of side etching and tip over-etching in traditional chemical etching processes, achieving high-precision transmission line preparation, ensuring that Stable transmission of high-frequency signals.

CN118900506APending Publication Date: 2024-11-05BEIJING LANMU LASER TECH CO LTD

Patent Information

Application Number
CN202411072460.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional chemical etching processes are prone to side corrosion and tip over-etching problems when etching thick copper microwave plates, resulting in insufficient accuracy of transmission line edges and insufficient characteristic impedance, which affects the transmission of high-frequency signals.

Method used

Using laser-assisted thick copper microwave plate processing method, by coating protective film on the surface of the copper layer and laser thinning treatment with a laser, the light spot is formed along the signal transmission line for external division and internal filling, and the copper layer is thinned, and then according to Substrate thickness is selected by laser or chemical etching to remove residual thin copper and protective film.

Benefits of technology

It significantly improves the accuracy and impedance characteristics of the transmission line, controls the thickness of the copper layer in the range of 0-36um, reduces the side etching and tip over-etching problems caused by chemical etching, and ensures the stability and consistency of signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900506A_ABST
    Figure CN118900506A_ABST
Patent Text Reader

Abstract

The invention provides a laser-assisted thick copper microwave plate processing method, and relates to the technical field of microwave plate manufacturing, and the method comprises the following steps: coating the surface of a copper layer of a thick copper microwave plate with a protective film; performing laser thinning treatment on the surface of the copper layer of the thick copper microwave plate coated with the protective film through a laser; and according to the thickness of the substrate of the thick copper microwave plate, removing the thin copper and the protective film remained on the thick copper microwave plate after laser thinning treatment. According to the method, the problem that the transmission line characteristic impedance does not reach the standard due to the fact that the boundary dimension is difficult to control after large depth etching of chemical etching is solved in a laser specific area thinning mode, especially for a thick copper microwave plate, the effect is more obvious, the precision of a transmission line can be guaranteed through the high-precision characteristic of laser, and the transmission efficiency is improved. Ideal appearance effects can be obtained in a straight line area, an inner right-angle area, an outer right-angle area and a side wall, and the problems of lateral corrosion and tip over-corrosion caused by chemical etching are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of microwave board manufacturing, and in particular to a laser-assisted thick copper microwave board processing method. Background Art

[0002] Traditional microwave board circuits are prepared through a series of chemical methods such as film lamination, exposure, development, etching, and cleaning. This set of processes is suitable for mass production. However, during the etching process, there will be inevitable problems of side etching and over-etching at the tip. Specifically, the inner and outer right angles are too large; the side walls are not vertical; the straight area is slightly bent, and other abnormalities. These abnormalities are more obvious the thicker the copper layer. This problem leads to insufficient edge accuracy of the transmission line and substandard characteristic impedance, which directly affects the high-frequency signal.

[0003] The first is the problem of side etching. Chemical etching is omnidirectional. During the etching process, there is both vertical etching and horizontal etching. The final etching profile effect is a U-shaped structure with tilted edges. On the one hand, the side walls are not vertical, and on the other hand, a portion of the etching solution will bypass the mask and etch the circuits that should be retained. This phenomenon is inevitable for chemical etching, but for thin copper circuit boards below 36um, the over-etching effect caused by side etching can generally be controlled within 15um, which is basically within an acceptable range. However, for thick copper microwave boards with high copper thickness and high requirements for circuit accuracy, this problem is a very difficult problem to deal with. For example, for 100um thick copper, the side etching problem will cause a precision difference of more than 40um, and this deviation is very difficult to accept for high-frequency microwave boards. The formation mechanism of this side etching problem is as follows Figure 2 shown.

[0004] The second problem is the over-etching of the tip. The chemical etching process is usually accompanied by the movement of positive and negative ions. Due to the existence of the tip discharge phenomenon, the electrochemical reaction at the tip is faster than other parts, and the etching efficiency is higher. This eventually leads to over-etching of the tip, which is similar to the rounded effect, such as Figure 3 shown.

[0005] The above phenomenon is also difficult to avoid for chemical etching. For conventional circuit boards, the influence of these aspects can be avoided as much as possible through circuit design. Circuits are generally designed to avoid right angles in various ways. The optimization methods are as follows: Figure 4 shown.

[0006] But for microwave boards, the inner right angles and outer right angles are often part of the signal transmission line, and there is no way to avoid them through design. We can only find other ways to ensure that the right angle or sharp angle area is not distorted. In summary, high-frequency microwave boards have very strict requirements on the production accuracy of transmission lines. Conventional chemical processes inevitably have problems such as side corrosion and tip corrosion, which affect the production accuracy, and then affect the impedance characteristics, resulting in signal distortion.

[0007] Currently, no effective solution has been proposed for the problems in the related technologies. Summary of the invention

[0008] In view of this, the present invention provides a laser-assisted thick copper microwave plate processing method to solve the above-mentioned problems.

[0009] In order to solve the above problems, the specific technical solutions adopted by the present invention are as follows:

[0010] A laser-assisted thick copper microwave plate processing method, the method comprising the following steps:

[0011] S1. Coating a protective film on the surface of the copper layer of the thick copper microwave board;

[0012] S2, performing laser thinning processing on the copper layer surface of the thick copper microwave board coated with the protective film by a laser;

[0013] S3. According to the substrate thickness of the thick copper microwave board, the thin copper and protective film remaining on the thick copper microwave board after the laser thinning process are removed.

[0014] Furthermore, the protective film is a dry film after exposure or a wet film after exposure;

[0015] The dry film after exposure is a semi-solid photosensitive etching dry film, and the wet film after exposure is a liquid photoresist.

[0016] Furthermore, the semi-solid photosensitive etching dry film is composed of a PE film, an ultraviolet light-curable intermediate film layer and a PET film.

[0017] Furthermore, the liquid photoresist is composed of liquid resin, solvent, monomer, initiator and filler.

[0018] Further, performing laser thinning on the copper layer surface of the thick copper microwave board coated with the protective film by a laser includes:

[0019] S21, using a laser to focus the laser on the copper layer surface of the thick copper microwave board coated with a protective film to form a light spot;

[0020] S22. The laser within the spot range vaporizes the copper layer surface into copper vapor, and the copper vapor is sucked away by the dust collection system.

[0021] S23, the laser performs laser thinning processing on the copper layer surface of the thick copper microwave board coated with the protective film along the laser processing path.

[0022] Furthermore, the diameter of the light spot is 10um-100um, the movement mode of the light spot is reciprocating along the laser processing path, and the overlap rate between two adjacent groups of light spots is 20%-50%.

[0023] Furthermore, the laser processing path includes outer segmentation and internal filling. Outer segmentation is the route along which the laser travels along the signal transmission line, which is used to separate the line portion and the copper layer portion to be removed. Internal filling is the route along which the laser travels in the copper layer portion to be removed.

[0024] Furthermore, the internal filling includes horizontal filling, vertical filling and vertical and horizontal filling.

[0025] Further, according to the thickness of the substrate of the thick copper microwave board, the thin copper and protective film remaining on the thick copper microwave board after the laser thinning process are removed, including:

[0026] If the substrate thickness of the thick copper microwave board is greater than a preset threshold thickness, the thin copper remaining on the thick copper microwave board after the laser thinning process is removed by laser thinning or sandblasting, and after the residual thin copper is removed by laser thinning, the protective film is removed by a film removal solution;

[0027] If the substrate thickness of the thick copper microwave board is not greater than a preset threshold thickness, the thin copper remaining on the thick copper microwave board after the laser thinning process is removed by chemical etching, and then the protective film is removed by a film stripping solution.

[0028] Furthermore, the film removal solution is a NaOH solution.

[0029] The beneficial effects of the present invention are:

[0030] 1. The present invention improves the problem of transmission line characteristic impedance not meeting the standard due to the difficulty in controlling the external dimensions after chemical etching with a large depth of etching by thinning a specific area with laser. The effect is more obvious especially for thick copper microwave plates. The high-precision characteristics of laser can ensure the accuracy of the transmission line. Whether it is a straight area, an inner right angle area, an outer right angle area, or a side wall, an ideal external effect can be obtained. The thickness of the copper after thinning can be controlled within the range of 0-36um, the etching depth is very small, and the side etching and tip over-etching problems caused by chemical etching are greatly improved.

[0031] 2. The present invention utilizes the high-precision characteristics of lasers to achieve precise preparation of signal transmission lines. First, the thick copper at the location where the thick copper needs to be removed is thinned by laser vertical and horizontal filling, and then a mask is covered and patterning is completed by chemical etching. By controlling the laser travel speed and the switching light delay, the overall flatness after the thick copper is thinned can be guaranteed. Chemical etching is performed after the thick copper is thinned to a range of 0-30um. Since the thickness of the copper layer is already very low, the part that needs chemical etching is already very small. The side etching and tip over-etching problems caused by chemical etching can be controlled within a range that does not affect the output of the microwave signal. Laser thinning is based on the standard of removing as much copper layer as possible without damaging the substrate. The thickness of the retained copper layer is related to the thickness uniformity of the copper layer itself. The more uniform the copper layer thickness is, the thinner the copper layer needs to be retained after thinning, the less obvious the side etching and tip over-etching effects caused by chemical etching are, and the better the overall effect is. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:

[0033] Figure 1 is a flow chart of a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0034] Figure 2 Schematic diagram of the formation mechanism of the side erosion problem in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0035] Figure 3 is a schematic diagram of tip overetching in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0036] Figure 4 is a schematic diagram of circuit design optimization in a laser-assisted thick copper microwave board processing method according to an embodiment of the present invention;

[0037] Figure 5 is a schematic diagram of the principle of a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0038] Figure 6 is a schematic diagram of the principle of laser thinning in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0039] Figure 7 is a schematic diagram of a laser thinning processing method in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0040] Figure 8 is a schematic diagram of three filling methods in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0041] Fig. 9 is a schematic diagram of two reciprocating motion trajectories of a light spot in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0042] Fig.10 is a schematic diagram of ensuring energy uniformity by overlapping light spots in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0043] Fig.11 is a schematic diagram of a spot spacing control method in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0044] Fig.12 is a schematic diagram of the problem of uneven thinning caused by temperature change in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0045] Fig.13 is a schematic diagram of ensuring thinning uniformity by superposition compensation in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0046] Fig.14 is a schematic diagram of the morphology of a copper layer after laser thinning in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0047] Fig.15 is a schematic diagram of the copper residue state after thinning in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention;

[0048] Fig.16 It is a schematic diagram of a laser thinning and removal of residual copper in a laser-assisted thick copper microwave plate processing method according to an embodiment of the present invention. DETAILED DESCRIPTION

[0049] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.

[0050] According to an embodiment of the present invention, a laser-assisted thick copper microwave plate processing method is provided.

[0051] The present invention will now be further described with reference to the accompanying drawings and specific embodiments. Figure 1 -As shown, according to the laser-assisted thick copper microwave plate processing method of an embodiment of the present invention, the method comprises the following steps:

[0052] S1. Coating a protective film on the surface of the copper layer of the thick copper microwave board;

[0053] Specifically, the protective film is a dry film after exposure or a wet film after exposure;

[0054] The exposed dry film is a semi-solid photosensitive etching dry film, and the exposed wet film is a liquid photoresist. For the above-mentioned exposed dry film or exposed wet film, from the perspective of protection effect, the wet film is preferably used as the protective film.

[0055] In addition, the protective glue can be selected from the exposed dry film or the exposed wet film. The dry film can be attached by laminating, and the wet film can be attached by screen printing or spin coating.

[0056] Semi-solid photosensitive etching dry film consists of PE film (polyethylene film), UV-curable intermediate film layer (a special coating or film that can be quickly cured under the action of ultraviolet light to form a stable structure) and PET film (polyethylene terephthalate film). The main working part is the UV-curable intermediate film layer, which is attached to the surface of the copper layer by a special film laminating machine. The advantages of dry film are good uniformity of film thickness and high sensitivity to ultraviolet light; the disadvantages are that because the film layer is semi-solid, the bonding with the copper layer is relatively poor, and the price is relatively high. After the dry film is attached, the whole is exposed to ultraviolet light or natural light to generate a protective film with a certain strength. The protective film has a certain physical strength, a certain acid resistance and weak alkali resistance, but it will dissolve in strong alkali.

[0057] Liquid photoresist (also called photoresist, including cross-linked photoresist and degradable photoresist) is composed of liquid resin (such as acrylic resin), solvent (used to adjust the viscosity and fluidity of the photoresist, such as acetone), monomer (low molecular weight compound, such as styrene), initiator (compound capable of initiating polymerization reaction, such as benzophenone) and filler (inorganic or organic material added to the photoresist to improve its performance, such as silicon dioxide). The coating equipment matched with it includes spin coater or screen printer. Some common polymer names of cross-linked photoresist include: polyethylene, polypropylene, polystyrene, polyacrylic acid, polymethyl acrylate, polyacrylamide, polyethylene glycol alkali base, polyethylene glycol methyl ether, etc. Some common polymer names of degradable photoresist include: polyisobutylene, poly-α-methylstyrene, polymethyl methacrylate, polymethacrylamide, polymethylisopropenyl ketone, etc.

[0058] The advantage of wet film is that it is relatively cheap, and because it is in liquid form, it can fill surface scratches and pits, and has better bonding with the substrate; the disadvantage is that the film thickness is uneven and the sensitivity to ultraviolet light is low. After the wet film is attached, the whole is exposed to ultraviolet light or natural light to generate a protective film with a certain strength. Compared with dry film, this protective film has higher physical protection strength, and also has certain acid resistance and weak alkali resistance, but it will dissolve in strong alkali.

[0059] It should be noted that the protective film needs to be coated before laser thinning, so that the protective film can better ensure the consistency of the laser thinning and subsequent residual copper removal positions. If the protective film is coated after laser thinning, additional exposure, development and etching processes are required, and it is difficult to ensure that the film alignment and the laser thinning position are completely overlapped. However, this problem does not exist if the protective film is coated in advance before laser thinning, because the laser thinning position is the position of the protective film opening, which is generated by the laser thinning process.

[0060] The functions of the protective film include: 1. During the laser thinning stage, the thinning spatter falls on the protective film, and in the subsequent removal process, it will be removed together with the protective film. This will prevent the copper layer from being contaminated by spatter. 2. In the subsequent residual copper removal stage, the protective film can protect the copper layer surface and prevent the surface copper layer from being contaminated or corroded.

[0061] S2, performing laser thinning processing on the copper layer surface of the thick copper microwave board coated with the protective film by a laser;

[0062] As a preferred embodiment, performing laser thinning on the copper layer surface of the thick copper microwave board coated with a protective film by a laser comprises:

[0063] S21, using a laser to focus the laser on the copper layer surface of the thick copper microwave board coated with a protective film to form a light spot;

[0064] Specifically, the diameter of the light spot is 10um-100um, the movement mode of the light spot is reciprocating along the laser processing path, and the overlap rate between two adjacent groups of light spots is 20%-50%.

[0065] S22. The laser within the spot range vaporizes the copper layer surface into copper vapor, and the copper vapor is sucked away by the dust collection system.

[0066] S23, the laser performs laser thinning processing on the copper layer surface of the thick copper microwave board coated with the protective film along the laser processing path.

[0067] Among them, the laser processing path includes outer shape segmentation and internal filling. Outer shape segmentation is the route that the laser travels along the signal transmission line, which is used to divide the line part and the copper layer part to be removed. Internal filling is the route that the laser travels in the copper layer part to be removed.

[0068] Specifically, the laser thinning process uses the concentration of laser energy. The laser is focused on the surface of the copper layer to form a small spot with a diameter of 10um-100um. The laser energy is highly concentrated within the spot range, vaporizing the copper surface into copper vapor, which is then taken away by the vacuum system to complete the removal of copper within the spot range. Through the laser path design, the spot can be evenly distributed in the removal area to achieve overall thinning of the copper layer. This process can be repeated many times, and the thickness of the copper layer thinned each time is determined by factors such as laser energy and spot overlap rate. The principle of laser thinning is as follows: Figure 6 shown.

[0069] The thick copper removal process preferably uses nanosecond, picosecond, and femtosecond lasers. Because copper has a high absorption rate for ultraviolet light, the overall processing efficiency will be improved to a certain extent; in contrast, the absorption rate of green light is lower; and the absorption rate of infrared light is the worst. Therefore, it is best to use ultraviolet lasers for processing.

[0070] During the thinning process, the laser uses a galvanometer to achieve the laser path design for the copper layer to be processed. The core components of the galvanometer are two reflective lenses. The laser is incident on the first reflective mirror, reflected on the second reflective mirror, and then reflected to the light outlet through the second reflective mirror. The two reflective lenses are controlled by their corresponding motors respectively. The software controls the rotation angle of the reflective lens through the motor, thereby controlling the laser's light output angle and light output position. Ultimately, the purpose of designing the laser processing path is achieved through software.

[0071] The laser is a pulsed laser that outputs laser pulses. One laser pulse will produce a light spot on the workpiece. While the laser produces the light spot, it moves driven by the galvanometer. The final light spot trajectory is the laser processing line.

[0072] In addition, the laser processing path is divided into two parts: outer shape segmentation and internal filling. The outer shape segmentation line is the route along which the laser travels along the signal transmission line, which is used to separate the line part and the copper layer part to be removed. The internal filling is the route of the laser in the copper layer part to be removed. By reciprocating in this area, the purpose of uniform thinning is achieved. After many tests, it was found that the best effect is to first segment the outer shape and then fill the internal part, and the multiple thinning effects are the best. If only filling is performed without segmentation, the edge quality of the transmission line will not be very good, and the verticality of the side wall will not be good; if filling is performed first and then segmentation, the segmented line part will have the problem of over-removal, which can easily damage the underlying substrate. The thinning path design processing method is as follows: Figure 7 shown.

[0073] In addition, the laser filling methods are divided into horizontal filling, vertical filling, and vertical and horizontal filling. The filling method with the best test result uniformity is vertical and horizontal filling. Figure 8 shown.

[0074] The light spot movement mode is that the galvanometer controls the light spot to reciprocate along the set path. There are two types of reciprocating motion trajectories of the light spot, one is on the same side of the laser starting position, and the other is alternating back and forth between the laser starting position. The movement mode on the same side of the starting position is easier to adjust the filling effect by controlling the laser switch delay, but the jump path is longer and the efficiency is lower; the laser starting position alternating mode has a very short jump path and higher efficiency, but the filling effect is relatively difficult to control. The two motion trajectories are as follows: Fig. 9 shown.

[0075] There needs to be a certain overlap rate between the light spots. If the overlap rate is too low, it will cause uneven thickness after thinning; if the overlap rate is too high, it will affect the thinning efficiency. The theoretical basis for achieving uniform thinning requirements through light spot overlap is the light spot energy density distribution. At present, the energy of conventional laser spots is Gaussian distribution. Through light spot overlap, the consistency of laser energy distribution can be better guaranteed. Fig.10 As shown. The best effect tested so far is an overlap rate of 20%-50%, that is, the spot spacing is designed to be 50%-80% of the spot diameter. Spot overlap rate = 1-spot spacing / spot diameter. During the processing, the spot diameter is a constant, and the only factor affecting the spot overlap rate is the spot spacing. The design of the spot overlap rate is achieved by controlling the spot travel speed, frequency and processing path spacing. In the direction of laser travel, the number of spots emitted by the laser within 1 second is the frequency; the distance the laser travels is the travel speed. In the direction of spot travel, it can be approximately considered that "spot spacing = travel distance / number of spots = travel speed / frequency"; perpendicular to the direction of spot travel, it can be considered that "spot spacing = path spacing". The spot spacing control method is as follows Fig.11 shown.

[0076] It should also be noted that since the laser absorption rate of the copper layer will increase significantly with the increase of temperature, the method of filling from one direction to the other will cause the problem of less thinning on one side and more thinning on the other side. This phenomenon may not be obvious in a single thinning process, but under the accumulation effect of multiple thinning, the thinning difference will become more and more prominent. Fig.12 As shown in the figure, in order to ensure the uniformity of the thinning thickness, it is best to alternate the filling direction. For example, the first thinning direction is from left to right, and the second thinning direction is from right to left. By superimposing and compensating for the unevenness twice, the overall uniformity of the thinning can be ensured as much as possible. Fig.13 shown.

[0077] Through the laser thinning process, the morphology of the copper layer of the thick copper microwave board shows an almost ideal state. Fig.14 shown.

[0078] At present, based on the high-precision characteristics of lasers, the precision of thinned graphics can be guaranteed. The processing range of a single galvanometer of laser equipment is generally 50mm*50mm, and the processing accuracy within the processing range can be controlled within 5um. Based on this, the following conclusions are drawn:

[0079] 1. Through laser path fine-tuning, it is easy to achieve a dimensional accuracy deviation within 5um. The substantial improvement in the dimensional accuracy of the signal transmission line can greatly reduce the distortion of high-frequency signals and improve the quality and efficiency of signal transmission.

[0080] 2. The distortion of the tip position is greatly reduced, and neither the inner right angle nor the outer right angle will be significantly distorted due to tip over-etching, and the straightness of the straight area can be well guaranteed. The difference between the overall graphic state and the ideal state can be controlled within 5um, ensuring the stability and consistency of the high-frequency signal output by the signal transmission line.

[0081] 3. Since the laser processing direction is vertical downward, the edge sidewalls of the processed graphics are also close to vertical, and there is no sidewall tilt problem caused by side etching. The effect of the vertical sidewall provides a good foundation for subsequent chemical etching.

[0082] S3. According to the substrate thickness of the thick copper microwave board, the thin copper and protective film remaining on the thick copper microwave board after the laser thinning process are removed.

[0083] As a preferred embodiment, according to the substrate thickness of the thick copper microwave board, removing the thin copper and protective film remaining on the thick copper microwave board after the laser thinning process includes:

[0084] If the substrate thickness of the thick copper microwave board is greater than a preset threshold thickness, the thin copper remaining on the thick copper microwave board after the laser thinning process is removed by laser thinning or sandblasting, and after the residual thin copper is removed by laser thinning, the protective film is removed by a film removal solution;

[0085] If the substrate thickness of the thick copper microwave board is not greater than a preset threshold thickness, the thin copper remaining on the thick copper microwave board after the laser thinning process is removed by chemical etching, and then the protective film is removed by a film stripping solution.

[0086] It should be noted that there are three ways to remove the thin copper remaining after thinning, namely laser removal, sandblasting removal, and chemical etching removal, and each of the three methods has its own advantages and disadvantages.

[0087] Through testing, it is known that the thickness of the copper layer after thinning can easily be less than 20um. Under the condition of good control of the thinning thickness, it can also be controlled below 10um. Generally, the time point for stopping laser thinning and switching to other processing methods is when part of the copper layer has been removed and the substrate begins to be exposed. The situation of thin copper residue at this time is as follows Fig.14 shown.

[0088] Among them, Fig.15 As shown in the figure, laser removal is to continue to use laser thinning to remove, and the thin copper layer is heated by laser to turn it into copper vapor. The advantage of this removal method is that the overall process is simple, and one laser device can complete the entire processing flow, and no other equipment is needed. But its disadvantages are also obvious. If the copper layer is to be removed cleanly, the problem of excessive removal must be involved. Because laser removal is an undifferentiated overall removal, if the copper layer is to be completely removed, the total removal amount must exceed the maximum copper layer thickness. If the residual copper layer thickness is 20um, 25um needs to be removed as a whole, and 25um is also removed from the substrate at the position where the substrate is exposed. If the substrate thickness is sufficient, there is no need to consider the substrate damage problem too much; or if the copper layer uniformity is sufficient, the maximum copper layer thickness is small enough, and the substrate damage can be controlled within a certain range, then laser can be considered to complete the copper layer removal. The protective film is retained during the laser removal process, and the protective film needs to be removed chemically after the laser removal process. Taking advantage of the property that the protective film is soluble in strong alkali, the NaOH solution is applied to the protective film by spraying or soaking to dissolve it.

[0089] Sandblasting is another indiscriminate removal method. It uses compressed air as a power source to form a high-speed jet beam and spray the material onto the surface of the object. The high-speed jet has an impact and cutting effect on the surface of the product, thereby achieving the effect of overall removal. As an indiscriminate cleaning method, sandblasting faces the same problem as laser removal and will damage the substrate to a certain extent. In addition, since the sandblasting process cannot select the removal area, the position of the protective film will also be affected by the sandblasting process. The protective film will be removed and no other methods are needed to remove the protective film.

[0090] Chemical etching is a mature process for circuit board factories at present. It is a process of removing metal materials through chemical solutions. Its core is the corrosive solution used to corrode the copper layer. The copper corrosive solution is generally an acidic solution, which oxidizes copper into cuprous ions in an acidic environment. The corrosive solution only works on metals and has no effect on protective films and substrates. There are many ways to implement chemical etching, such as convection, spraying, and two-fluid, which are relatively mature processes. If there is a process requirement that the substrate is not damaged, the last part of the thin copper is processed by chemical etching. In most thick copper application scenarios, it is a better choice to use chemical etching to process the last part of the residual thin copper.

[0091] Since the thickness of the residual copper layer is controlled at a very low level, the impact of side etching and tip overetching caused by chemical etching can be controlled within a very small range. Under the premise that the maximum thickness of the residual copper layer is within 20um, the impact of side etching can be controlled within 7um, and the impact of tip overetching can be controlled within 10um. Considering the accuracy deviation within 5um caused by laser thinning, the overall accuracy deviation can be controlled within 15um; if corresponding compensation is considered in the design stage of the processing path of laser thinning, the overall accuracy deviation can be controlled within 10um. Compared with the accuracy deviation of more than 40um in pure chemical etching, there is a significant improvement. After completing chemical etching, the protective film needs to be removed. Taking advantage of the property that the protective film is soluble in strong alkali, the NaOH solution is applied to the protective film by spraying or immersion to dissolve it.

[0092] At this point, the preparation of the thick copper microwave board signal transmission line is completed.

[0093] In summary, with the help of the above technical scheme of the present invention, the present invention improves the problem of substandard characteristic impedance of the transmission line caused by the difficulty in controlling the external dimensions after chemical etching with a large depth of etching, by means of laser thinning of specific areas. Especially for thick copper microwave plates, the effect is more obvious. The high-precision characteristics of the laser can ensure the accuracy of the transmission line. Whether it is a straight area, an inner right angle area, an outer right angle area, or a side wall, an ideal external effect can be obtained, and the thickness of the copper after thinning can be controlled within the range of 0-36um, the etching depth is very small, and the side etching and tip over-etching problems caused by chemical etching are greatly improved. The present invention utilizes the high-precision characteristic of laser to realize accurate preparation of signal transmission lines. First, the thick copper at the position where the thick copper needs to be removed is thinned by laser vertical and horizontal filling, and then a mask is covered and patterning is completed by chemical etching. By controlling the laser travel speed and the switching light delay, the overall flatness of the thick copper after thinning can be guaranteed. Chemical etching is performed after the thick copper is thinned to a range of 0-30um. Since the thickness of the copper layer is already very low, the part that needs chemical etching is already very small. The side etching and tip over-etching problems caused by chemical etching can be controlled within a range that does not affect the output of microwave signals. Laser thinning is based on the standard of removing as much copper layer as possible without damaging the substrate. The thickness of the retained copper layer is related to the thickness uniformity of the copper layer itself. The more uniform the copper layer thickness is, the thinner the copper layer needs to be retained after thinning, the less obvious the side etching and tip over-etching effects caused by chemical etching are, and the better the overall effect is.

[0094] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A laser-assisted thick copper microwave plate processing method, characterized in that: The method comprises the following steps: S1. Coating a protective film on the surface of the copper layer of the thick copper microwave board; S2, performing laser thinning processing on the copper layer surface of the thick copper microwave board coated with the protective film by a laser; S3. According to the substrate thickness of the thick copper microwave board, the thin copper and protective film remaining on the thick copper microwave board after the laser thinning process are removed.

2. A laser-assisted thick copper microwave plate processing method according to claim 1, characterized in that: The protective film is a dry film after exposure or a wet film after exposure; The exposed dry film is a semi-solid photosensitive etching dry film, and the exposed wet film is a liquid photoresist.

3. A laser-assisted thick copper microwave plate processing method according to claim 2, characterized in that: The semi-solid photosensitive etching dry film consists of a PE film, an ultraviolet light-curable intermediate film layer and a PET film.

4. The laser-assisted thick copper microwave plate processing method according to claim 2, characterized in that: The liquid photoresist is composed of liquid resin, solvent, monomer, initiator and filler.

5. The laser-assisted thick copper microwave plate processing method according to claim 1, characterized in that: The laser thinning process performed on the copper layer surface of the thick copper microwave board coated with the protective film by a laser comprises: S21, using a laser to focus the laser on the copper layer surface of the thick copper microwave board coated with a protective film to form a light spot; S22. The laser within the spot range vaporizes the copper layer surface into copper vapor, and the copper vapor is sucked away by the dust collection system. S23, the laser performs laser thinning processing on the copper layer surface of the thick copper microwave board coated with the protective film along the laser processing path.

6. A laser-assisted thick copper microwave plate processing method according to claim 5, characterized in that: The diameter of the light spot is 10um-100um, and the movement mode of the light spot is reciprocating along the laser processing path. The overlap rate between two adjacent groups of light spots is 20%-50%.

7. A laser-assisted thick copper microwave plate processing method according to claim 6, characterized in that: The laser processing path includes outer segmentation and internal filling. The outer segmentation is the route along which the laser travels along the signal transmission line, which is used to separate the line part and the copper layer part to be removed. The internal filling is the route along which the laser travels in the copper layer part to be removed.

8. The laser-assisted thick copper microwave plate processing method according to claim 7, characterized in that: The internal filling includes horizontal filling, vertical filling and vertical and horizontal filling.

9. The laser-assisted thick copper microwave plate processing method according to claim 1, characterized in that: The method of removing the thin copper and protective film remaining on the thick copper microwave board after the laser thinning process according to the substrate thickness of the thick copper microwave board comprises: If the substrate thickness of the thick copper microwave board is greater than a preset threshold thickness, the thin copper remaining on the thick copper microwave board after the laser thinning process is removed by laser thinning or sandblasting, and after the residual thin copper is removed by laser thinning, the protective film is removed by a film removal solution; If the substrate thickness of the thick copper microwave board is not greater than a preset threshold thickness, the thin copper remaining on the thick copper microwave board after the laser thinning process is removed by chemical etching, and then the protective film is removed by a film stripping solution.

10. A laser-assisted thick copper microwave plate processing method according to claim 9, characterized in that: The defilming solution is a NaOH solution.

Citation Information

Patent Citations

  • Laser machining method, for providing flat recess in workpiece surface, has laser beam moved along recess contour line for providing slot around central region removed subsequently

    DE10062706C1

  • Processing of printed circuit boards

    GB1583192A

  • Laser sculpturing method

    JP1994304769A

  • Patterning method using dry-film photoresist

    KR1020090063979A

  • Method of manufacturing a circuit carrier and the use of the method

    US20070163887A1

Cited By

  • Production method of thick copper circuit board and thick copper circuit board

    CN120881881A