Fly ash-based hydrated calcium silicate as well as preparation method and application thereof
Calcium silicate hydrate is prepared by thermal activation and hydrothermal reaction of fly ash, which solves the problem of alkali aggregate effect caused by potassium or sodium alkaline solution in the existing technology. It provides a safe and low-cost porous calcium silicate hydrate product that is suitable for building and adsorption materials.
Patent Information
- Application Number
- CN202310503808.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-06
AI Technical Summary
Existing technologies require the addition of potassium or sodium-containing alkaline solutions when preparing hydrated calcium silicate, resulting in the presence of potassium or sodium in the product. This affects the performance of cement concrete and may cause alkali-aggregate effect and environmental pollution. Furthermore, the process is complex and costly.
Using fly ash as raw material, hydrated calcium silicate is prepared through thermal activation and hydrothermal reaction, avoiding the use of alkaline solutions containing potassium or sodium. The preparation process is simple, including mixing, thermal activation, hydrothermal reaction, liquid-solid separation and drying, to obtain hydrated calcium silicate with a porous structure.
The prepared fly ash-based hydrated calcium silicate requires no washing, is safe and harmless, and is suitable for cement and concrete. It does not exhibit alkali return and has high reactivity and a porous structure, making it suitable for building materials, adsorbent materials, and other fields. It is inexpensive and easy to mass-produce.
Smart Images

Figure CN118908234A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to fly ash-based calcium silicate hydrate and a preparation method and application thereof. Background Art
[0002] The basic composition of calcium silicate hydrate (CSH) is xCaO·SiO2·yH2O, which has a complex composition and a calcium-silicon molar ratio between 0.6 and 2.0. Calcium silicate hydrate is the main hydration product of silicate cement and the main source of cement concrete strength. Artificially synthesized calcium silicate hydrate is added to concrete and used together with water reducers and active admixtures to promote cement hydration, improve the structure and strength of cement stone, and make concrete obtain better strength and performance. Artificially synthesized calcium silicate hydrate is loose and porous and rich in active calcium. It can not only adsorb and solidify some heavy metal ions, but also adsorb and recover phosphorus and ammonia nitrogen in sewage. Therefore, in recent years, people have begun to study and explore its use in water treatment and ecological restoration. In addition, most of the silicon and calcium in calcium silicate hydrate are citric acid soluble and easily absorbed by plants. Silicon and calcium are both necessary medium elements for plant growth, so calcium silicate hydrate is also a very important raw material component in soil improvement materials.
[0003] CN107673362A discloses a method for preparing calcium silicate hydrate, wherein a mixture of sodium silicate solution, calcium nitrate solution and water is placed in a plastic container and ultrasonically mixed, and then sodium hydroxide solution is added to make the pH of the mixed solution>13, thereby preparing calcium silicate hydrate with high purity; CN112250076A discloses a method for preparing nanometer calcium silicate hydrate, wherein sodium silicate solution and calcium nitrate solution are used as raw materials to prepare nanometer calcium silicate hydrate by gradually dropping and mixing; CN106542551A discloses a method for extracting aluminum oxide from fly ash, wherein quicklime, fly ash and water are mixed, 5g / L to 100g / L of NaOH is added to adjust the pH value of the slurry, and the mixture is reacted in a high-pressure closed container at a temperature of 120°C to 260°C for 0.5h to 12h, and calcium silicate hydrate for cement concrete is obtained by solid-liquid separation.
[0004] At present, the method of preparing calcium silicate hydrate using fly ash as raw material requires the addition of potassium or sodium alkali solution, which is used to promote the dissolution of SiO2 in fly ash to achieve a better reaction effect. However, the addition of potassium or sodium alkali will change the morphological structure and chain length of calcium silicate hydrate, and cause the calcium silicate hydrate product to contain potassium or sodium, which is difficult to completely remove even with a large amount of water washing. In the application field of cement concrete, it will cause alkali aggregate effect and seriously affect the performance. It is also easy to cause alkali pollution when used for water treatment or ecological restoration.
[0005] Therefore, seeking a preparation method of calcium silicate hydrate with simple process, low cost, outstanding performance, especially without potassium or sodium, is of great significance for its large-scale application as an industrial product. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a fly ash-based hydrated calcium silicate and a preparation method and use thereof. The preparation method has a relatively simple process, the raw materials are derived from solid waste fly ash, and no alkali solution containing potassium or sodium needs to be added during the preparation process. The product does not need to be washed, and no alkali return phenomenon will occur when used in cement or concrete. It is safe and harmless to soil and crops, has a short preparation time, high production capacity, and has very good application prospects.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing fly ash-based calcium silicate hydrate, the preparation method comprising the following steps:
[0009] (1) mixing a calcium source, fly ash and water to obtain a mixed slurry;
[0010] (2) thermally activating the mixed slurry in step (1) to obtain an activated slurry;
[0011] (3) The activated slurry in step (2) is subjected to hydrothermal reaction, liquid-solid separation and drying in sequence to obtain the fly ash-based hydrated calcium silicate.
[0012] The preparation method of fly ash-based calcium silicate hydrate of the present invention uses fly ash as a silicon source raw material and a calcium-containing compound as a calcium source raw material, adds the two into water in a certain proportion to obtain a mixed slurry, and then transforms the fly ash into a calcium silicate hydrate with a loose porous structure and high activity through a special thermal activation (heating-constant temperature-cooling)-hydrothermal reaction process, and the proportion of crystalline tobermorite in the fly ash-based calcium silicate hydrate is 10-40%. The present invention uses solid waste as a raw material source, and does not need to add potassium or sodium-containing alkali solution during the preparation process, has a simple process, low cost, safety and high efficiency, and is a very promising preparation method.
[0013] Preferably, the calcium source in step (1) is an industrial raw material with calcium oxide as the main component.
[0014] Preferably, the calcium source comprises any one of calcium hydroxide, lime, calcium phosphate or calcium sulfate, or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of calcium hydroxide and lime, a combination of calcium phosphate and calcium sulfate, a combination of calcium hydroxide and calcium phosphate, or a combination of calcium sulfate, calcium hydroxide and lime.
[0015] The calcium source of the present invention includes any one of calcium hydroxide, lime, calcium phosphate or calcium sulfate or a combination of at least two thereof. Although they are also alkaline substances, the calcium ions contained therein are different from the alkali solution containing potassium or sodium used in the prior art. The fly ash-based hydrated calcium silicate obtained by the present invention will not cause alkali reversion when used in cement or concrete, and is safe and harmless to soil and crops.
[0016] Preferably, the molar ratio of CaO in the calcium source to SiO2 in the fly ash in step (1) is (0.4-1.4):1, for example, it can be 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1 or 1.4:1, as well as other values other than the above values, which are not exhaustively listed in the present invention due to space limitations and for the sake of simplicity. The molar ratio is preferably (0.8-1.1):1.
[0017] The present invention preferably has a molar ratio of CaO in the calcium source to SiO2 in the fly ash of (0.4-1.4):1, which can increase the content of citric acid-soluble silicon dioxide in the product and also adjust the microscopic morphology of the product, such as the specific surface area and porosity.
[0018] Preferably, the solid-to-liquid ratio of the mixed slurry in step (1) is 1:(10-40) g / mL, for example, it can be 1:10 g / mL, 1:15 g / mL, 1:20 g / mL, 1:25 g / mL, 1:30 g / mL, 1:35 g / mL or 1:40 g / mL, and other values other than the above values, which are not exhaustively listed in the present invention due to space limitations and for simplicity. The mass-to-volume ratio is preferably 1:(15-25) g / mL.
[0019] The solid-liquid ratio of the mixed slurry of the present invention is very critical to the preparation of calcium silicate hydrate. When the mass-to-volume ratio is too high, it is difficult for the reactants in the mixed slurry to mix evenly and the reaction is insufficient. When the mass-to-volume ratio is too low, it causes excessive energy consumption.
[0020] Preferably, the thermal activation in step (2) includes a temperature rise section, a constant temperature section and a temperature drop section, wherein the temperature drop section is a key step of the thermal activation and is essential. During the thermal activation process, the structural type of the silicon-oxygen tetrahedron in the fly ash changes and is transformed into a structure that is easier to be converted into a calcium silicate hydrate, and the reaction activity is greatly enhanced, thereby laying a structural foundation for the next step of hydrothermal synthesis of calcium silicate hydrate. If the thermal activation is not performed in advance and the hydrothermal reaction is directly performed, the content of crystalline tobermorite in the calcium silicate hydrate will be reduced under the same conditions, and the yield of the calcium silicate hydrate will be significantly reduced.
[0021] Preferably, the heating rate of the heating section is 1-10°C / min, for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, as well as other values besides the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.
[0022] Preferably, the temperature of the constant temperature section is 150-250°C, for example, it can be 150°C, 160°C, 180°C, 200°C, 220°C, 240°C or 250°C, and other values other than the above values, which are not exhaustively listed in the present invention due to space limitations and for the sake of simplicity. The temperature is preferably 180-200°C.
[0023] The temperature of the constant temperature section in the present invention is too low, the reaction rate of thermal activation is too slow, the conversion rate is too low, and the tobermorite crystal content and the citric acid-soluble silicon dioxide content in the obtained fly ash-based hydrated calcium silicate are low; the temperature of the constant temperature section is too high, and the industrial cost of preparing the fly ash-based hydrated calcium silicate is relatively high.
[0024] Preferably, the time of the constant temperature section is 0-1h, for example, it can be 0h, 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h or 1h, as well as other values besides the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.
[0025] Preferably, the terminal temperature of the cooling section is 25-80°C, for example, it can be 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, as well as other values besides the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.
[0026] When the terminal temperature of the cooling section of the present invention is too high, the activation is insufficient, the silicon-oxygen tetrahedron structure in the fly ash is not completely transformed, and the tobermorite crystal content and the citric acid-soluble silicon dioxide content in the obtained fly ash-based hydrated calcium silicate are low; when the terminal temperature of the cooling section is too low, the cooling time is too long, and the cost of preparing the fly ash-based hydrated calcium silicate increases.
[0027] Preferably, the cooling period is 0.1-3 h, for example, 0.1 h, 0.2 h, 0.3 h, 0.5 h, 0.7 h, 1 h, 1.5 h, 2 h, 2.5 or 3 h, as well as other values other than the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.
[0028] When the cooling section of the present invention is too short, the transformation of the silicon-oxygen tetrahedral structure in the fly ash is difficult to complete, which affects the activation effect, and the tobermorite crystal content and the citric acid-soluble silica content in the obtained fly ash-based hydrated calcium silicate are low; when the cooling section is too long, the cost of preparing the fly ash-based hydrated calcium silicate increases.
[0029] Preferably, the temperature of the hydrothermal reaction in step (3) is 150-250°C, for example, 150°C, 160°C, 180°C, 200°C, 220°C, 240°C or 250°C, and other values other than the above values, which are not exhaustively listed in the present invention due to space limitations and for the sake of simplicity. The temperature is preferably 180-220°C.
[0030] Preferably, the hydrothermal reaction time of step (3) is 0.5-6h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h, and other values other than the above values, which are not exhaustively listed in the present invention due to space limitations and for the sake of simplicity. The time is preferably 1-3h.
[0031] The present invention will keep appropriate temperature during the hydrothermal reaction. When the temperature of the hydrothermal reaction is too low, the reaction can not be fully carried out. Crystalline tobermorite and citric acid soluble silica content are relatively low. When the temperature of the hydrothermal reaction is too high, energy consumption increases and cost increases. When the time of the hydrothermal reaction is too short, the reaction is not completely carried out. Crystalline tobermorite and citric acid soluble silica content are relatively low. When the time of the hydrothermal reaction is too long, energy consumption will be increased and cost will be increased. The preferred temperature and time can reduce energy consumption to the greatest extent under the conditions of guaranteeing crystalline tobermorite and citric acid soluble silica content, saving cost.
[0032] In the present invention, the liquid-solid separation in step (3) does not need to be washed, and the calcium silicate hydrate product can be obtained directly after drying. The liquid-solid separation and drying can be carried out using conventional equipment in the art.
[0033] There is no limitation on the solid-liquid separation in the present invention, and any method known to those skilled in the art for solid-liquid separation may be used, such as filtration, sedimentation or centrifugation.
[0034] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0035] (1) mixing a calcium source, fly ash and water to obtain a mixed slurry; the calcium source comprises any one of calcium hydroxide, lime, calcium phosphate or calcium sulfate or a combination of at least two thereof; the molar ratio of CaO in the calcium source to SiO2 in the fly ash is (0.4-1.4):1; the solid-liquid ratio of the mixed slurry is 1:(10-40) g / mL;
[0036] (2) The mixed slurry of step (1) is thermally activated to obtain an activated slurry; the thermal activation includes a temperature rising section, a constant temperature section and a temperature falling section; the temperature rising rate of the temperature rising section is 1-10°C / min; the temperature of the constant temperature section is 150-250°C and the time is 0-1h; the terminal temperature of the temperature falling section is 25-80°C and the time is 0.1-3h;
[0037] (3) The activated slurry in step (2) is subjected to a hydrothermal reaction at a temperature of 150-250° C. for 0.5-6 h, liquid-solid separation and drying to obtain the fly ash-based hydrated calcium silicate.
[0038] In a second aspect, the present invention further provides a fly ash-based calcium silicate hydrate, wherein the fly ash-based calcium silicate hydrate is prepared by the method for preparing the fly ash-based calcium silicate hydrate according to any one of claims 1 to 7.
[0039] Preferably, the proportion of crystalline tobermorite in the fly ash-based hydrated calcium silicate is 10-40%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35% or 40%, as well as specific point values between the above values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0040] In a third aspect, the present invention further provides a use of the fly ash-based calcium silicate hydrate as described in the second aspect in building materials, adsorption materials, soil improvement materials, thermal insulation materials, and sound insulation materials.
[0041] Compared with the prior art, the present invention has at least the following beneficial effects:
[0042] (1) The preparation method of fly ash-based calcium silicate hydrate provided by the present invention adopts a new method of pre-heat activation to stimulate the conversion of silicate structure in fly ash, which can greatly improve the reaction activity of aluminum silicate in fly ash. This process can replace the role of alkali activators (caustic soda, water glass, etc.) in traditional processes. No alkali metal ions containing potassium or sodium are introduced into the overall process, and no washing process is required. The problems of alkali aggregate reaction, alkali blooming and environmental pollution caused by alkali metal ions containing potassium or sodium can be eliminated from the source;
[0043] (2) The crystalline form of the fly ash-based hydrated calcium silicate provided by the present invention is tobermorite, accounting for more than 30%, and its microscopic morphology is a porous fibrous structure, which is similar to the structure after cement hydration, and has the application basis of being used as cement hydration induction crystal seeds, accelerating cement hydration, and increasing cement strength; at the same time, the fly ash-based hydrated calcium silicate prepared by the present invention is rich in citric acid-soluble silicon dioxide and has strong water retention capacity, and has the functions of adsorbing heavy metal ions, sound insulation, heat insulation, air permeability, etc., and can be widely used in the fields of adsorption materials, sound insulation and heat insulation materials, soil conditioners, etc., and is a calcium silicate hydrate product with huge application prospects and strong practicality;
[0044] (3) The preparation method of fly ash-based calcium silicate hydrate provided by the present invention is simple and easy to implement, has a short preparation time, low cost, and is easy to carry out large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The present invention provides a process flow chart of a method for preparing fly ash-based hydrated calcium silicate.
[0046] Figure 2 This is the microscopic morphology of the fly ash-based hydrated calcium silicate obtained in Example 1. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0048] The present invention provides a method for preparing fly ash-based calcium silicate hydrate, and its process flow chart is as follows: Figure 1 The preparation method comprises the following steps:
[0049] (1) mixing a calcium source, fly ash and water to obtain a mixed slurry;
[0050] (2) thermally activating the mixed slurry in step (1) to obtain an activated slurry;
[0051] (3) The activated slurry in step (2) is subjected to hydrothermal reaction, liquid-solid separation and drying in sequence to obtain the fly ash-based hydrated calcium silicate.
[0052] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0053] Example 1
[0054] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate, the preparation method comprising the following steps:
[0055] (1) mixing calcium hydroxide, fly ash from a power plant in Ximeng, Inner Mongolia, and water, controlling the solid-liquid ratio to be 1:20 g / mL, to obtain a mixed slurry; the molar ratio of CaO in the calcium hydroxide to SiO2 in the fly ash is 1.05:1;
[0056] (2) The mixed slurry in step (1) is thermally activated to obtain an activated slurry; the thermal activation includes a heating section, a constant temperature section and a cooling section; the heating rate of the heating section is 5°C / min, the temperature is raised to 180°C, the constant temperature time is 0.5h, and after the constant temperature is completed, cooling water is passed to cool the temperature to 40°C, and the cooling time is 1h;
[0057] (3) The activated slurry in step (2) is subjected to a hydrothermal reaction at a temperature of 200° C. for 1 hour, filtered and separated, and dried to obtain the fly ash-based hydrated calcium silicate.
[0058] The specific surface area of the fly ash-based calcium silicate hydrate prepared in this example is 35.13 m 2 / g, the porosity is 92.51%, and its microscopic morphology is as follows Figure 2 shown.
[0059] Example 2
[0060] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate, the preparation method comprising the following steps:
[0061] (1) mixing calcium hydroxide, fly ash from a power plant in Ximeng, Inner Mongolia, and water, controlling the solid-liquid ratio to be 1:20 g / mL, to obtain a mixed slurry; the molar ratio of CaO in the calcium hydroxide to SiO2 in the fly ash is 1.05:1;
[0062] (2) The mixed slurry in step (1) is thermally activated to obtain an activated slurry; the thermal activation includes a heating section, a constant temperature section and a cooling section; the heating rate of the heating section is 10°C / min, the temperature is raised to 200°C, the constant temperature time is 0h, and after the constant temperature is completed, cooling water is passed to cool the temperature to 25°C, and the cooling time is 3h;
[0063] (3) The activated slurry in step (2) is subjected to a hydrothermal reaction at a temperature of 200° C. for 1 hour, filtered and separated, and dried to obtain the fly ash-based hydrated calcium silicate.
[0064] Example 3
[0065] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate, the preparation method comprising the following steps:
[0066] (1) mixing calcium hydroxide, fly ash from a power plant in Ximeng, Inner Mongolia, and water, controlling the solid-liquid ratio to be 1:20 g / mL, to obtain a mixed slurry; the molar ratio of CaO in the calcium hydroxide to SiO2 in the fly ash is 1.05:1;
[0067] (2) The mixed slurry in step (1) is thermally activated to obtain an activated slurry; the thermal activation includes a heating section, a constant temperature section and a cooling section; the heating rate of the heating section is 1°C / min, the temperature is raised to 180°C, the constant temperature time is 1 hour, and after the constant temperature is completed, cooling water is passed to cool the temperature to 80°C, and the cooling time is 3 hours;
[0068] (3) The activated slurry in step (2) is subjected to a hydrothermal reaction at a temperature of 200° C. for 0.1 h, filtered and separated, and dried to obtain the fly ash-based hydrated calcium silicate.
[0069] Example 4
[0070] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate, the preparation method comprising the following steps:
[0071] (1) mixing calcium hydroxide, fly ash from a power plant in Ximeng, Inner Mongolia, and water, controlling the solid-liquid ratio to be 1:20 g / mL, to obtain a mixed slurry; the molar ratio of CaO in the calcium hydroxide to SiO2 in the fly ash is 1.05:1;
[0072] (2) The mixed slurry of step (1) is thermally activated to obtain an activated slurry; the thermal activation includes a heating section, a constant temperature section and a cooling section; the heating rate of the heating section is 7°C / min, the temperature is raised to 200°C, the constant temperature time is 1 hour, and after the constant temperature is completed, cooling water is passed to cool the temperature to 50°C, and the cooling time is 0.5 hour;
[0073] (3) The activated slurry in step (2) is subjected to a hydrothermal reaction at a temperature of 200° C. for 1 hour, filtered and separated, and dried to obtain the fly ash-based hydrated calcium silicate.
[0074] Example 5
[0075] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate, the preparation method comprising the following steps:
[0076] (1) mixing calcium hydroxide, fly ash from a power plant in Ximeng, Inner Mongolia, and water, controlling the solid-liquid ratio to be 1:10 g / mL, to obtain a mixed slurry; the molar ratio of CaO in the calcium hydroxide to SiO2 in the fly ash is 0.8:1;
[0077] (2) The mixed slurry in step (1) is thermally activated to obtain an activated slurry; the thermal activation includes a heating section, a constant temperature section and a cooling section; the heating rate of the heating section is 10°C / min, the temperature is raised to 220°C, the constant temperature time is 1h, and after the constant temperature is completed, cooling water is passed to cool the temperature to 25°C, and the cooling time is 3h;
[0078] (3) The activated slurry in step (2) is subjected to a hydrothermal reaction at a temperature of 220° C. for 0.5 h, filtered, separated and dried to obtain the fly ash-based hydrated calcium silicate.
[0079] Example 6
[0080] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate, the preparation method comprising the following steps:
[0081] (1) mixing calcium hydroxide, fly ash from a power plant in Ximeng, Inner Mongolia, and water, controlling the solid-liquid ratio to be 1:30 g / mL, to obtain a mixed slurry; the molar ratio of CaO in the calcium hydroxide to SiO2 in the fly ash is 1.2:1;
[0082] (2) The mixed slurry in step (1) is thermally activated to obtain an activated slurry; the thermal activation includes a heating section, a constant temperature section and a cooling section; the heating rate of the heating section is 1°C / min, the temperature is raised to 160°C, the constant temperature time is 0h, and after the constant temperature is completed, cooling water is passed to cool the temperature to 80°C, and the cooling time is 0.5h;
[0083] (3) The activated slurry in step (2) is subjected to a hydrothermal reaction at a temperature of 160° C. for 6 hours, filtered, separated and dried to obtain the fly ash-based hydrated calcium silicate.
[0084] Example 7
[0085] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate. The preparation method is the same as that of Embodiment 1 except that the temperature of the constant temperature section in step (2) is 150° C.
[0086] Example 8
[0087] This embodiment provides a method for preparing fly ash-based calcium silicate hydrate, which is the same as that of Embodiment 1 except that the terminal temperature of the cooling section in step (2) is 90° C. and the cooling time is 0.1 h.
[0088] Comparative Example 1
[0089] This comparative example provides a method for preparing fly ash-based calcium silicate hydrate, which is the same as Example 2 except that the thermal activation in step (2) is not performed.
[0090] The fly ash-based calcium silicate hydrate prepared in this comparative example does not produce fibrous particles or particles with special morphology.
[0091] Comparative Example 2
[0092] This comparative example provides a method for preparing fly ash-based calcium silicate hydrate, which is the same as Example 2 except that the cooling stage in the thermal activation of step (2) is omitted and step (3) is directly performed.
[0093] The fly ash-based calcium silicate hydrate prepared in this comparative example does not produce fibrous particles or particles with special morphology.
[0094] The content of crystalline tobermorite in the fly ash-based calcium silicate hydrate prepared in the above examples and comparative examples was determined by adding an internal standard and using XRD Rietvel analysis method;
[0095] The content of citric acid-soluble silicon dioxide in the fly ash-based calcium silicate hydrate prepared in the above examples and comparative examples was determined by dissolving in 1.5 mol / L hydrochloric acid using an ICP element quantitative method.
[0096] The particle morphology of the fly ash-based calcium silicate hydrate prepared in the above examples and comparative examples was observed and measured using an electron scanning microscope (SEM) test and analysis method. The results are shown in Table 1.
[0097] Table 1
[0098]
[0099] From Table 1 we can see that:
[0100] (1) It can be seen from Examples 1 to 6 that the method for preparing fly ash-based hydrated calcium silicate provided by the present invention has a simple process, and the content of crystalline tobermorite in the prepared fly ash-based hydrated calcium silicate can reach 38%, and the content of citric acid-soluble silicon dioxide can reach 25.32%. The microscopic morphology is a porous structure, the particle size is small, and it has a good adsorption effect;
[0101] (2) Combining Example 1 and Example 7, it can be seen that the temperature of the constant temperature section in Example 7 is 150° C., which is lower than the preferred temperature range of 180-200° C. of the constant temperature section of the present invention. The content of crystalline tobermorite in the prepared fly ash-based hydrated calcium silicate is low, only 19%, and the content of citric acid-soluble silica is also reduced to 16.46%. In addition, the microscopic morphology is amorphous and the particle size is large. When used as a building material in the future, the pore structure of the building material is large and the strength is low. When the temperature of the constant temperature section is high, it will cause high energy consumption and high preparation cost of fly ash-based hydrated calcium silicate.
[0102] (3) Combining Example 1 and Example 8, it can be seen that the terminal temperature of the cooling section in Example 8 is 90°C, which is higher than the terminal temperature range of 25-80°C of the cooling section of the present invention. The content of crystalline tobermorite in the prepared fly ash-based hydrated calcium silicate is low, which is 21%, and the content of citric acid-soluble silicon dioxide is also reduced to 18.74%. Moreover, the microscopic morphology is amorphous and the particle size is large. When used as a building material in the subsequent process, the pore structure of the building material is large and the strength is low. The terminal temperature of the constant temperature section in the present invention does not need to be lower.
[0103] (4) It can be seen from Example 2 and Comparative Examples 1 and 2 that the thermal activation in step (2) and the cooling stage in the thermal activation in step (2) of the present invention can greatly increase the content of crystalline tobermorite and the content of citric acid-soluble silicon dioxide in the prepared fly ash-based hydrated calcium silicate, and the particle size is smaller.
[0104] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing fly ash-based calcium silicate hydrate, characterized in that: The preparation method comprises the following steps: (1) mixing a calcium source, fly ash and water to obtain a mixed slurry; (2) thermally activating the mixed slurry in step (1) to obtain an activated slurry; (3) The activated slurry in step (2) is subjected to hydrothermal reaction, liquid-solid separation and drying in sequence to obtain the fly ash-based hydrated calcium silicate.
2. The preparation method according to claim 1, characterized in that: The calcium source in step (1) is an industrial raw material with calcium oxide as the main component; Preferably, the calcium source includes any one of calcium hydroxide, lime, calcium phosphate or calcium sulfate, or a combination of at least two thereof.
3. The preparation method according to claim 1 or 2, characterized in that: The molar ratio of CaO in the calcium source in step (1) to SiO2 in fly ash is (0.4-1.4):1, preferably (0.8-1.1):
1.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The solid-to-liquid ratio of the mixed slurry in step (1) is 1:(10-40) g / mL, preferably 1:(15-25) g / mL.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The thermal activation in step (2) includes a temperature rising section, a constant temperature section and a temperature falling section; Preferably, the heating rate of the heating section is 1-10°C / min; Preferably, the temperature of the constant temperature section is 150-250°C, preferably 180-200°C; Preferably, the constant temperature period is 0-1h; Preferably, the terminal temperature of the cooling section is 25-80°C; Preferably, the temperature reduction period is 0.1-3 hours.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The temperature of the hydrothermal reaction in step (3) is 150-250°C, preferably 180-220°C.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The time of the hydrothermal reaction in step (3) is 0.5-6h, preferably 1-3h.
8. A fly ash-based calcium silicate hydrate, characterized in that: The fly ash-based calcium silicate hydrate is prepared by the preparation method of fly ash-based calcium silicate hydrate according to any one of claims 1 to 7.
9. The fly ash-based calcium silicate hydrate according to claim 8, characterized in that: The proportion of crystalline tobermorite in the fly ash-based hydrated calcium silicate is 10-40%.
10. Use of the fly ash-based calcium silicate hydrate as claimed in claim 8 or 9 in building materials, adsorption materials, soil improvement materials, thermal insulation materials, and sound insulation materials.
Citation Information
Patent Citations
Method of preparing tobermorite from fly ash and application thereof
CN104828834A
Method of producing calcium silicate crystal whiskers with fly ash desilication liquid
CN105839188A
Method for co-producing dawsonite and tobermorite from fly ash
CN106542551A
Treatment for rendering fly ash from dust incineration harmless
JP1996173930A
Method for co-producing alumina and activated calcium silicate from high-alumina fly ash
US20130343971A1
Cited By
Preparation method and application of tobermorite-rich high-ash coal slime-based silicon-calcium-potassium fertilizer
CN119822893A
Tobermorite type calcium silicate hydrate soil treatment agent as well as preparation method and application thereof
CN122403465A
Tobermorite-type calcium silicate hydrate soil treatment and methods of making and using same