Ruthenium-based oxygen evolution catalyst, preparation method and device
By doping transition metals in ruthenium-based catalysts and preparing bimetal oxide catalysts using metal organic frame materials, the problem of poor stability of ruthenium-based catalysts in acidic environments is solved, and efficient acid redox reactions and long-term stability are achieved. Reduces energy consumption and costs.
Patent Information
- Application Number
- CN202411248737.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
The existing ruthenium-based catalysts have poor stability in acidic environments, resulting in high usage of precious metal elements, limiting the commercial application of PEM water electrolysis technology, especially in acidic redox reactions (OERs) and the oxidation release of lattice oxygen and surface. The problem of active site shedding.
Using bimetallic ruthenium-based catalyst, hollow nanopolyhedral structure and metal organic framework (MOF) are used to form a heterogeneous interface by doping transition metal into ruthenium oxide, adjusting electronic structure, optimizing reaction paths, and enhancing the stability and activity of the catalyst. ) The material is used as a skeleton and embedded metal M and Ru ions to form a RuxMyOz catalyst, and a heterogeneous interface is formed through a two-step annealing method to reduce the formation of RuO4.
It significantly improves the stability and activity of the catalyst, extends the working life, reduces energy consumption and costs, improves the water decomposition performance of PEM devices, achieves long-term acidic OER stability, and breaks the bottleneck of catalyst activity and stability.
Smart Images

Figure CN118996520A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst, in particular to a ruthenium-based oxygen evolution catalyst, a preparation method and a device. Background Art
[0002] In recent years, with the continuous improvement of energy transformation and environmental awareness, green hydrogen produced by water electrolysis driven by renewable energy has high energy density and is completely carbon-free, so it is regarded as an ideal alternative to fossil fuels. However, this technology faces some challenges in practical application. Due to the slow kinetics of water electrolysis, high energy is required to drive the reaction, which leads to low energy efficiency and increases the cost of hydrogen production. In particular, the four-electron transfer involved in the oxygen evolution reaction (OER) makes its overpotential much higher than that of the HER reaction, resulting in huge energy consumption. Using polymer-based proton exchange membranes (PEMs) for efficient proton transfer, PEM water electrolysis technology can significantly improve performance and has attracted widespread research interest. However, the large-scale deployment of PEM devices is largely hindered by the lack of active, stable and low-cost acidic OER catalysts. At present, PEM anodes mainly use precious metal catalysts such as iridium (Ir) and ruthenium (Ru). However, the small reserves and high prices of these precious metal catalysts limit the large-scale commercial application of PEM water electrolysis technology. Although Ru has been recognized as an attractive alternative for acidic OER (~7.5 times cheaper than Ir) and its oxide RuO2 has good acidic OER activity, the long-term stability of Ru-based catalysts in PEM is still greatly challenged. In general, the acidic OER stability challenges of Ru-based catalysts are mainly caused by the following two reasons. The first is related to the oxidative release of lattice oxygen, which causes the Ru species to be overoxidized to soluble RuO4. The second is the direct shedding of surface Ru active sites, which also causes the crystal structure collapse of Ru-based catalysts. Therefore, reducing the amount of precious metal elements while maintaining catalytic performance is one of the important ways to promote the practical application of precious metal-based catalysts. However, only a few of the non-precious metal catalysts can remain stable in harsh acidic environments, and many catalysts require extremely high overpotentials. Most of the Ru-based catalysts reported so far are stable at 10 mA cm -2 At low current densities, its stability is still limited to tens of hours, which is far from the requirements for industrial applications. More importantly, due to the significant change in the reaction environment, the stable performance obtained in the standard three-electrode setup in acidic liquid electrolytes may not necessarily translate into practical PEM devices. Summary of the invention
[0003] In order to improve the stability of ruthenium-based catalysts and enhance the electrocatalytic activity, the present invention provides a bimetallic ruthenium-based oxygen evolution catalyst, which enhances the reaction activity and stability of the ruthenium oxide catalyst by doping transition metals into ruthenium oxide.
[0004] The technical solution adopted is: a ruthenium-based oxygen evolution catalyst, the molecular formula of which can be simplified to Ru x M y O z , where M is a transition metal, 0<z≤(4x+3y) / 2. M is doped in the lattice of ruthenium oxide, and ruthenium is doped in the lattice of M oxide, forming a heterostructure of two doped metal oxides. The oxide of metal M and the oxide of Ru are doped to form Ru x M y O z The lattice doping of metal M oxide and Ru oxide is conducive to the formation of a heterogeneous interface, regulating the electronic structure of Ru, optimizing the reaction path of ruthenium oxide in the oxygen evolution reaction, and enhancing the stability of the catalyst. When z < (4x + 3y) / 2, it indicates that there are oxygen vacancies in the lattice structure of the catalyst. Oxygen vacancies optimize the adsorption energy of intermediates in the catalytic reaction process, thereby enhancing the catalytic activity of the catalyst.
[0005] As a preferred embodiment, the catalyst is a hollow nano-polyhedron structure, such as a nano-cage structure, which is beneficial for increasing the oxygen vacancy concentration in the catalyst on the one hand, and for increasing the active surface area of the catalyst and improving the catalytic activity on the other hand.
[0006] As a preferred solution, the nanocage structure is prepared by using a metal organic framework (MOF material) as a skeleton, and embedding metal M ions and Ru ions in the skeleton, preferably a dodecahedral MOF material.
[0007] As a preferred embodiment, the M metal is metal Co and the catalyst molecular formula is Ru x Co y O z In the crystal structure of the catalyst, Co is doped into the ruthenium oxide (RuO2) lattice, and Ru is doped into the cobalt oxide (Co3O4) lattice, forming a heterogeneous interface, causing valence electron transfer between Co and Ru, reducing the average valence state of Co and increasing the average valence state of Ru, thereby promoting the formation of the intermediate *OOH during the reaction process, allowing the catalyst to act in a reaction path that is more conducive to stability and avoiding the formation of soluble RuO4.
[0008] As a preferred solution, x:y is 1:(1-10); preferably x:y=1:1. Catalysts with different atomic ratios have different catalytic properties, and preferably the atomic ratio of Ru and Co is 1:1.
[0009] The present invention also provides a method for preparing a ruthenium-based oxygen evolution catalyst, which can be used to prepare the ruthenium-based catalyst in the above scheme. The preparation method comprises the following steps: (1) obtaining a polyhedral template material, (2) using the polyhedral template material as a skeleton, depositing M ions and Ru ions on the template, and then removing the template material through annealing or other processes to form a bimetallic oxide skeleton of M-Ru-O. The formed new skeleton retains the polyhedral structure of the template material and can expose more active sites.
[0010] As a more preferred solution, the template material in the preparation process of the ruthenium-based catalyst is a MOF material, and the preparation method includes:
[0011] (1) Obtaining MOF material, which is a metal organic framework and plays a role as a skeleton in the catalyst preparation process. The material can be purchased or prepared;
[0012] (2)Ru 3+ Etching MOF material: Ru 3+ It is acidic in aqueous solution and can etch the MOF material to make the MOF material present a hollow structure. The etching steps can be one of the following:
[0013] When the MOF material contains M metal atoms, the MOF material is mixed with Ru 3+ The salt solution is mixed with Ru 3+ Etching the MOF material into a hollow polyhedral structure, wherein Ru ions are embedded in the MOF material;
[0014] When the B MOF material contains M metal atoms or does not contain M metal atoms, the MOF material is mixed with Ru 3+ The salt solution of Ru and the salt solution of M ions are mixed. 3+ Etching MOF materials into hollow polyhedral structures, Ru 3+ , M ions are embedded in MOF materials.
[0015] (3) Annealing: Anneal the etched material in air to obtain a catalyst.
[0016] As a preferred solution, M is preferably cobalt (Co), and the MOF material is preferably a cobalt-based metal organic framework material. Again, the preparation method of the MOF material is: dissolving cobalt nitrate powder (Co(NO3)2·6H2O) and 2-methylimidazole in an organic solvent, uniformly dispersing by ultrasonication, stirring at room temperature, and then standing to obtain polyhedral dimethylimidazole cobalt (ZIF-67); further preferably, the molar ratio of cobalt nitrate (Co(NO3)2·6H2O) to 2-methylimidazole is 1: (1 to 8), preferably 1: 4, and the specific preparation process is: 6 mmol of Co(NO3)2·6H2O and 24 mmol of 2-methylimidazole are mixed in 115 ml of methanol, the stirring speed is 800 rpm, the stirring time is 1 minute, and the stirring is allowed to stand for 20-24 hours to obtain a dodecahedral structure of ZIF-67.
[0017] As a preferred solution, the etching step includes a) dispersing ZIF-67 powder in an organic solvent to prepare a ZIF-67 suspension; b) dissolving a set amount of cobalt salt and ruthenium salt in a mixed solution of H2O and methanol, wherein the molar ratio of H2O to methanol is (0-1):1; and transferring the ZIF-67 suspension to the mixed solution. c) after hydrothermal standing reaction, centrifugation is performed to obtain Ru x Co y O z HND (hollow MOF material loaded with M and Ru, Ru x Co y O z Hollow nano dodecahedron), then washed with water and methanol for several times, and dried to obtain Ru x Co y O z Powder; d Ru x Co y O z The powder was annealed in 10% H2 / Ar (hydrogen content 10%, argon content 90%) to generate Ru x Co y HNDs. Then annealing in air gave the catalyst Ru x Co y O z .
[0018] As a specific implementation scheme, the cobalt salt is CoCl2·xH2O, the ruthenium salt is RuCl3, the mixed molar ratio of ZIF-67, CoCl2·xH2O and RuCl3 is 1:(1-10), the mixed molar ratio of CoCl2·xH2O and RuCl3 will directly affect the molar ratio of the two elements in the catalyst, and the mixed molar ratio of the two salts can be regulated according to the molar ratio of the two elements in the required catalyst. For further optimization, the concentration of ZIF-67 in the suspension is not limited. The suspension is prepared to facilitate the dispersion of ZIF-67. The preferred concentration of ZIF-67 in the suspension is 1 mg / ml. The total amount of CoCl2·xH2O and RuCl3 is 0.072 mol. CoCl2·xH2O and RuCl3 are mixed in 3 ml of water and methanol solution. Mixing in water is conducive to hydrolyzing Ru into an acidic solution, which plays a role in etching ZIF-67. The mixing ratio of water and methanol is (0-1):1.
[0019] As a preferred scheme, the hydrothermal reaction temperature in step c is not specifically limited. When the hydrothermal reaction temperature is high, the reaction time is short, and when the hydrothermal reaction temperature is low, the reaction time is long, based on achieving the desired etching degree. Finally, ZIF-67 is etched into a hollow polyhedral structure. The preferred hydrothermal temperature is 40°C to 60°C, and the hydrothermal reaction time is 1.5h to 2.5h.
[0020] As a preferred solution, the annealing in step d is carried out twice, first annealing in a mixed gas of hydrogen and argon to reduce the bimetallic alloy, and then annealing in an oxygen atmosphere or air atmosphere to oxidize the bimetallic alloy. This annealing method is conducive to doping Co into the RuO2 lattice and Ru into Co3O4, forming a uniformly distributed bimetallic oxide composite material, forming a heterogeneous interface, rather than separately agglomerated Ru clusters and Co clusters, so that the electronic structure can be adjusted, the Ru site can be prevented from being over-oxidized, the adsorption of key intermediates (*OOH) in the reaction path can be optimized, and the acidic OER activity and stability can be improved. In the two-step annealing process, the annealing temperature can be: 350℃~450℃, and the annealing time is 1.5h~2.5h.
[0021] The present invention also provides an electrolysis device, which uses the catalyst mentioned in any of the above schemes to carry out oxygen evolution reaction, and is further optimized. The electrolysis device is a PEM device, the catalyst serves as an anode catalyst of the PEM device, and the PEM device is used for electrolyzing water.
[0022] The beneficial effects of the present invention include:
[0023] (1) MOF is a coordination compound with a periodic structure, which is assembled from metal ions and organic ligands. It has an adjustable coordination structure and a metal atom environment that has an important influence on the actual catalytic performance. The present invention uses a polyhedral MOF material as a skeleton to prepare nanocages, nanowires, nanosheets, and nanoframes of the catalyst, optimize the arrangement of catalyst material atoms and optimize the reaction kinetics, expose more active sites, and enhance the reaction activity and stability of the catalyst.
[0024] (2) The compressive or tensile lattice strain generated by the core-shell structure designed in the present invention, the alloying of precious metals and heteroatoms in different atomic ratios, and the leaching of Co species in acid during the hydrothermal reaction preparation process will produce various defects such as oxygen vacancies. Oxygen vacancies can adjust the adsorption energy of water molecules, thereby optimizing the adsorption energy of intermediates and giving the material better catalytic activity.
[0025] (3) The catalyst prepared by the present invention is a composite catalyst formed by doping metal M with metal Ru oxide. The use of metal M changes the reaction path of the traditional RuO2 catalyst, reduces the solubility of the catalyst, and enhances the stability of the catalyst. When M is Co, the electron cloud density distribution of the Ru active site shifts toward the Co site due to the doping of Co, and the center of the Ru energy band changes, thereby affecting the adsorption energy of oxygen-containing reaction intermediates at the Ru site, promoting the formation of *OOH, and enhancing the activity of the reaction.
[0026] (4) The present invention utilizes a two-step annealing method to form a heterogeneous interface between the Co-O compound and the Ru-O compound, thereby causing electron transfer, preventing excessive oxidation of the Ru site, optimizing the adsorption of the key intermediate (*OOH) in the reaction pathway, and improving the acidic OER activity and stability.
[0027] (5) The present invention utilizes Ru 3+ The acidic characteristics of the MOF material etch the MOF material, making the MOF material present a hollow structure, thereby forming a hollow catalyst crystal, increasing the active sites and improving the catalytic activity.
[0028] (6) The catalyst preparation method of the present invention can freely adjust the catalyst morphology and the Co to Ru component ratio in the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of the preparation process of the catalyst in the present invention;
[0030] Figure 2 Scanning electron microscope image of the ZIF-67 material prepared by the present invention;
[0031] Figure 3(a), Figure 3(b), Figure 3(c), and Figure 3(d) are Ru prepared in Example 3, Example 2, Example 1, and Example 4, respectively.x Co y O z SEM images of the catalyst;
[0032] FIG4( a) is a diagram showing the distribution of various elements in the catalyst prepared in Example 3;
[0033] FIG4( b) is a transmission electron micrograph of the catalyst prepared in Example 3;
[0034] Figure 5 Ru prepared in Example 1-4 x Co y O z X-ray diffraction pattern of the catalyst;
[0035] Figure 6 (a) Figure 6 (b) Ru prepared in Example 3 x Co y O z CV diagram of the catalyst;
[0036] Figure 7 (a) Ru prepared in Examples 1 to 4 x Co y O z LSV plot of the catalyst in H2SO4 at pH = 0;
[0037] Figure 7(b) Ru prepared in Examples 1 to 4 x Co y O z Tafel curve of the catalyst in H2SO4 at pH = 0;
[0038] Figure 8 The catalysts in Examples 1 to 4 were used as electrocatalysts for oxygen evolution reaction in H2SO4 at pH = 0 with a current density of 10 mA / cm 2 The chronopotentiometry curves of
[0039] Fig. 9 Example 3: Ru prepared x Co y O z Comparison of catalyst activity for water splitting in PEM devices;
[0040] Fig.10 Example 3: Ru prepared x Co y O z The catalyst has a water splitting current density of 200 mA / cm in a PEM device. 2 The chronopotentiometry curves of
[0041] Fig.11 Diagram of the action mechanism of c-RuO2. DETAILED DESCRIPTION
[0042] The present invention is further explained in detail below in conjunction with the accompanying drawings and specific embodiments, but it should be understood that the protection scope of the present invention is not limited to the specific embodiments.
[0043] Example 1
[0044] The preparation steps of ruthenium-based catalysts are as follows Figure 1 As shown, it includes (1) preparing the framework material ZIF-67; (2) etching ZIF-67, and growing the bimetallic ions on the framework material; (3) annealing and reducing the bimetallic-ZIF-67 complex in a H2 atmosphere; (4) annealing and reducing in an O2 atmosphere. The preparation method specifically includes the following steps:
[0045] (1) Preparation of ZIF-67 precursor
[0046] a 6 mmol of Co(NO3)2·6H2O powder and 24 mmol of 2-methylimidazole were dissolved in 115 ml of methanol solution, uniformly dispersed by ultrasonication, stirred at 800 rpm for 1 minute at room temperature, and then allowed to stand for 24 h.
[0047] b Centrifuge at 6000 rpm for 10 minutes to obtain ZIF-67 with a dodecahedral structure, and then wash it with water and methanol three times to obtain the crystal structure of ZIF-67 as shown in Figure 2 As shown, the nano-dodecahedrons are smooth, uniform in size, and solid. c ZIF-67 powder was dispersed in 20 ml of methanol to prepare a 1 mg / ml ZIF-67 suspension.
[0048] (2) Etching ZIF-67 precursor
[0049] a 61.2 mmol CoCl2·xH2O and 10.8 mmol RuCl3 were dissolved in 12 ml of a mixed solution of H2O and methanol, with a volume ratio of H2O to methanol of 1:1;
[0050] b. Transfer 2.4 ml of the ZIF-67 suspension in step (1) to the mixed solution (i.e., 2.4 mg of ZIF-67), allow to react at 60°C for 2 h, and centrifuge to obtain Ru 15 Co 85 O z HNDs were then washed three times with water and methanol and dried to obtain Ru 15 Co 85 O z HNDs powder.
[0051] (3) Annealing
[0052] a will Ru 15 Co 85 Oz HNDs powder was annealed at 360 °C for 2 h in 10% H2 / Ar (hydrogen content, 10%) to generate Ru 15 Co 85 HND(Ru 15 Co 85 Hollow nanododecahedron);
[0053] BnB 15 Co 85 HND was annealed at 400℃ in air for 2h to obtain Ru 15 Co 85 O z Catalyst. The catalyst structure is shown in Figure 3(c), Ru 15 Co 85 O z The HNDs powders still retain the polyhedral morphology and size of the precursor ZIF-67 template and show a rougher surface.
[0054] Example 2
[0055] The difference from Example 1 is that step (2) and step (3)
[0056] Step (2) Etching ZIF-67 Precursor
[0057] a 50.4mmolCoCl2·xH2O and 21.6mmolRuCl3 were dissolved in 12ml of a mixed solution of H2O and methanol, the volume mixing ratio of H2O and methanol being 1:1;
[0058] b. Transfer 2.4 ml of the ZIF-67 suspension in step (1) to the mixed solution, let it stand for 2 h at 60 °C, and centrifuge to obtain Ru 30 Co 70 O z HNDs were then washed three times with water and methanol and dried to obtain Ru 30 Co 70 O z HNDs powder;
[0059] Step (3) Annealing
[0060] a Ru 30 Co 70 O z HNDs powder was annealed at 360 °C for 2 h in 10% H2 / Ar (hydrogen content, 10%) to generate Ru 30 Co 70 HNDs;
[0061] BnB 30 Co 70HNDs were annealed at 400℃ for 2h in air to obtain Ru 30 Co 70 O z Catalyst,The catalyst structure is shown in Figure 3(b). It can be seen that the catalyst still maintains the polyhedral morphology and size of the precursor ZIF-67 template, and shows a rougher surface.
[0062] Example 3
[0063] The difference from Example 1 is that step (2) and step (3)
[0064] Step (2) Etching ZIF-67 Precursor
[0065] a 36mmolCoCl2·xH2O and 36mmolRuCl3 were dissolved in 12ml of a mixed solution of H2O and methanol, with a volume ratio of H2O to methanol of 1:1;
[0066] b. Transfer 2.4 ml of the ZIF-67 suspension in step (1) to the mixed solution, let it stand for 2 h at 60 °C, and centrifuge to obtain Ru 50 Co 50 O z HND, then washed with water and methanol three times and dried to obtain Ru 50 Co 50 O z HNDs powder; step (3) annealing
[0067] a Ru 50 Co 50 O z HNDs powder was annealed at 360 °C for 2 h in 10% H2 / Ar (hydrogen content, 10%) to generate Ru 50 Co 50 HND;
[0068] b Annealing at 400℃ in air for 2h to obtain Ru 50 Co 50 O z The catalyst structure is shown in Figure 3(a). It can be seen that the catalyst still maintains the polyhedral shape and size of the precursor ZIF-67 template, and shows a rougher surface. The structure of the catalyst under transmission electron microscopy is shown in Figure 3(a). Figure 4(a) and 4(b)As shown in Figure 4(a), Co, Ru, and O are all distributed on the outer contour of the polyhedral structure. Figure 4(b) shows that the catalyst is a hollow polyhedral structure. Figures 3(c), 4(a), and 4(b) show that the catalyst presents a porous surface structure and a hollow three-dimensional structure, which increases the chemical reaction active area and catalytic active sites of the catalyst, is beneficial to the adsorption of catalytic reaction intermediates, accelerates the catalytic reaction kinetics, and improves the catalytic activity.
[0069] Example 4
[0070] The difference from Example 1 is that step (2) and step (3)
[0071] Step (2) Etching ZIF-67 Precursor
[0072] a Dissolve 72mmol CoCl2·xH2O in 12ml of a mixed solution of H2O and methanol, with a volume ratio of H2O to methanol of 1:1;
[0073] b. Transfer 2.4 ml of the ZIF-67 suspension in step (1) to the mixed solution, let it stand for 2 h at 60 °C, and centrifuge to obtain Co n O w HND, then washed with water and methanol three times and dried to obtain Co n O w HND powder; During the etching process, ZIF67 hydrolyzes to form Co(OH)2, and Co ions are exchanged from the inside of ZIF to the outside, forming an internal hollow structure;
[0074] Step (3) Annealing
[0075] a Co n O w HND powder was annealed at 360℃ for 2h in 10% H2 / Ar (hydrogen content, 10%) to produce Co HND; b was annealed at 400℃ for 2h in air to produce Co n O w catalyst.
[0076] The X-ray diffraction patterns (XRD) of the catalysts obtained in Test Examples 1-4 are as follows: Figure 5 As shown, the X-ray diffraction peaks correspond very accurately to the standard PDF card, indicating that we have indeed synthesized the Ru / Co bimetallic composite oxide structure. At the same time, the peaks of ZIF-67 are basically unobservable, indicating that the ZIF-67 contained in the nanocage has been basically etched completely.
[0077] The X-ray photoelectron spectroscopy (XPS) of the catalyst obtained in Example 3 was tested, and the catalyst was compared with ruthenium oxide RuO2 and cobalt oxide CoO zThe energy spectrum of CoO is compared as shown in Figure 6(a) and Figure 6(b). z The energy spectrum of Example 3 shows that part of the valence electrons of Co in the catalyst obtained in Example 3 have been transferred, and the average valence state has been reduced. Compared with the energy spectrum of RuO2, the high-valence content of Ru element remains at a relatively high level, and the content of +4-valent Ru element has been slightly increased, indicating that part of the valence electrons of Co have been transferred to Ru, and a heterogeneous interface has been formed between cobalt oxide and ruthenium oxide, changing the catalytic reaction path.
[0078] The OER linear sweep voltammetric curves and Tafel curves of the catalyst materials with different Ru / Co ratios of Examples 1-4 are compared, as shown in Figures 7(a) and 7(b). It can be seen that in terms of OER catalytic activity, from strong to weak, they are Example 3, Example 1, Example 2, and Example 4, and the reaction kinetics from strong to weak are Example 3, Example 1, Example 2, and Example 4; the catalyst Ru obtained in Example 3 50 Co 50 O z It has the best OER catalytic activity and the best reaction kinetics.
[0079] The current between the working electrode and the reference electrode was set to 10 mA cm -2 The constant current test is performed to obtain a data curve of the voltage between the electrodes varying with time, namely a chronopotentiometric curve. The chronopotentiometric curve of the catalyst obtained in Example 1-4 as an electrocatalyst for oxygen evolution reaction is as follows: Figure 8 As shown, the current density was 10 mA / cm in H2SO4 at pH = 0. 2 The chronopotentiometry curves show that the stability of the catalysts prepared in Examples 1-3 exceeds that of pure cobalt oxide, especially the Ru prepared in Example 3. 50 Co 50 O z It has a stable duration of more than 500 hours.
[0080] Example 5
[0081] An electrolysis device is provided, wherein the catalyst obtained in Example 3 is used as an anode catalyst, the cathode electrode is commercial platinum carbon supported on hydrophobic carbon paper, and the proton exchange membrane is commercial N115, to prepare a PEM device.
[0082] Comparative Example 1
[0083] The difference from Example 5 is that commercial ruthenium oxide (c-RuO2) is used as the anode catalyst to prepare the PEM device.
[0084] The water decomposition linear sweep voltammetry curves of the PEM devices in Example 5 and Comparative Example 1 were tested. The results are as follows: Fig. 9As shown, it can be seen that the overall water decomposition performance of Example 5 is significantly better than that of commercial ruthenium oxide (c-RuO2) in Comparative Example 1, which indicates that the oxygen vacancies and heterogeneous interfaces present in the catalyst of the present invention are helpful to improve the OER electrocatalytic performance of the PEM device.
[0085] The PEM devices in Example 5 and Comparative Example 1 were tested at a current density of 200 mA / cm 2 The chronopotentiometry curve for water decomposition is shown in Figure 2. Fig.10 As shown, the catalyst in Example 5 has a stability of more than 150 h, far exceeding commercial ruthenium oxide (c-RuO2).
[0086] In summary, the present invention is a wet chemical material synthesis method using a metal organic framework (MOF) as a template, which can controllably synthesize efficient and stable Ru with a hollow cage structure. x Co y O z Bimetallic oxide nanocatalyst with an overpotential of 181 mV and a Tafel slope of 53 mV dec -1 , showing excellent acidic OER performance and outstanding long-term stability (500 hours) in acidic electrolytes. This system can break the bottleneck of catalyst activity and stability, greatly improve the efficiency of water electrolysis, thereby increasing the yield of hydrogen and reducing the energy consumption and cost of PEM devices.
[0087] Abundant oxygen vacancies and heterogeneous interfaces are introduced into the bimetallic oxides with hollow nanocage structures, which enhances the electron transfer from Ru active sites to Co, regulates the electronic structure, and optimizes the adsorption of key intermediates (*OOH) in the reaction path, thereby improving the acidic OER activity. In addition, the strong electronic coupling effect at the heterogeneous interface can effectively prevent the dissolution of the active material RuO2, greatly enhancing the stability of the material.
[0088] The catalytic pathways of traditional commercial ruthenium oxides are as follows: Fig.11 As shown, the OER of RuO2 comes from the adsorption of H2O on the Ru site, followed by two consecutive deprotonation steps to form *OH and *O. Subsequently, the reaction path bifurcates into one of two possible mechanisms: the lattice oxygen mechanism (LOM) or the adsorbed oxygen mechanism (AEM). In the LOM, the surface-adsorbed *O further reacts with the lattice O to generate O2, and the generated O vacancies are refilled by another H2O. After the AEM path, the surface-adsorbed O further reacts with another H2O in the electrolyte to generate *OOH, and then generates the final product O2. The bimetallic composite catalyst in the present invention can be optimized to the LAM path to enhance the stability of the catalyst.
[0089] Comparative Examples 2 to 4
[0090] Comparative Example 2, Comparative Example 3, and Comparative Example 4 are the comparative examples of Example 1, Example 2, and Example 3, respectively. The difference between the comparative examples and the corresponding examples is that the annealing is directly performed in air without a 10% H2 / Ar annealing step. Compared with the catalyst in the example, the obtained catalyst has Co in the form of Co clusters and Ru in the form of Ru clusters, and a heterogeneous interface cannot be formed.
[0091] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A ruthenium-based oxygen evolution catalyst, Features: The molecular formula is Ru x M y O z , x>0, y>0, z>0, wherein M is a transition metal, M is doped in the lattice of ruthenium oxide, and ruthenium is doped in the lattice of M oxide.
2. The ruthenium-based oxygen evolution catalyst according to claim 1, Features: x:y=1:1, 0<z≤(4x+3y) / 2.
3. The ruthenium-based oxygen evolution catalyst according to claim 1, Features: Catalyst Ru x M y O z The nanocage structure is a nanoscale hollow polyhedron structure.
4. The ruthenium-based oxygen evolution catalyst according to claim 1, Features: M is metal cobalt, and the catalyst molecular formula is Ru x Co y O z In the crystal structure of the catalyst, Co is doped into the ruthenium oxide lattice, and Ru is doped into the cobalt oxide lattice; preferably, Ru x Co y O z In the crystal structure of Co and Ru, there is a valence electron transfer between them, which makes Ru x Co y O z The average valence of Co in cobalt oxide is lower than that in Ru x Co y O z The average valence state of Ru in ruthenium is higher than that in ruthenium oxide.
5. A method for preparing a ruthenium-based oxygen evolution catalyst, Features: Using the polyhedral structure material as a template, a polyhedral structure Ru is formed on the template. x M y O z , wherein M is a transition metal, x>0, y>0, z>0.
6. The preparation method according to claim 5, Features: The template is a MOF material, and the preparation method of the ruthenium-based oxygen evolution catalyst comprises the following steps: Obtaining a MOF material, wherein the MOF material is a metal organic framework material with a polyhedral structure; Ru ion etching MOF material: MOF material, M ion salt, and Ru ion salt are mixed in a solvent, and Ru ions are used to etch the MOF material, so that the MOF material is converted into a hollow polyhedral structure, and M ions and Ru ions grow on the hollow MOF material to obtain a hollow MOF material loaded with M and Ru; Annealing: The hollow MOF material loaded with M and Ru is annealed at a set temperature to remove the MOF material and obtain the polyhedral structure catalyst Ru x M y O z .
7. The preparation method according to claim 6, Features: The MOF material is an M-based metal organic framework, preferably M is Co, and the preparation method of the MOF material is more preferably: cobalt nitrate powder (Co(NO 3 ) 2 6H 2 O) and 2-methylimidazole are dissolved in an alcohol solution to react to obtain a polyhedral structure of dimethylimidazole cobalt, and then (Co(NO 3 ) 2 6H 2 The mixing molar ratio of O) to 2-methylimidazole is 1:(1-8).
8. The preparation method according to claim 6 or 7, Features: The M ion salt is a Co ion salt, and the Ru ion etching MOF material comprises the following steps: (1) dispersing cobalt dimethyl imidazole in an organic solution to prepare a cobalt dimethyl imidazole suspension; (2) Add a set amount of CoCl 2 ·nH 2 O and RuCl 3 Dissolved in H 2 In a mixed solution of O and an organic solvent; (3) mixing the suspension in step (1) with the mixed solution in step (2); (4) The hollow MOF material loaded with M and Ru is obtained by reacting at a set temperature.
9. The preparation method according to claim 8, Features: In step (2), CoCl 2 ·nH 2 O and RuCl 3 The mixing molar ratio is 1: (0-1), the organic solvent is methanol, H 2 The volume ratio of O and methanol is (0~1):
1.
10. The preparation method according to claim 6, Features: The annealing step includes: (1) The hollow MOF material loaded with M and Ru was placed in H 2 and inert gas atmosphere to generate Ru x Co y Hollow polyhedral structure; (2) x Co y The hollow polyhedral structure is annealed in air to obtain the catalyst Ru x Co y O z .
11. An electrolysis device, Features: Any catalyst of claims 1-4 or any catalyst prepared by the preparation method of claims 5-9 is used as an oxygen evolution catalyst.
12. The electrolysis device according to claim 11, Features: The electrolysis device is a PEM device, and the oxygen evolution catalyst serves as an anode catalyst of the PEM device.
Citation Information
Cited By
Trace ruthenium modified cobalt-based nanocage catalyst and preparation and application thereof
CN120250065A
POROUS RUTHENIUM OXIDE-BASED CATALYST INCORPORATED WITH d0 METAL IONS FOR OXYGEN EVOLUTION REACTION, METHOD FOR PREPARING SAME, AND PROTON EXCHANGE MEMBRANE WATER ELECTROLYZER COMPRISING SAME
KR103019299B1
Electrocatalyst and electrolyser comprising the same
WO2026123080A1