Preparation method of preheated rubber powder concrete

By preheating the rubber powder to control its morphology and particle size, and combining it with panthenol, sodium phytate and allantoin coating treatment, the problems of high preparation cost and poor mechanical properties of rubber concrete were solved, and the high bonding strength between rubber powder and cement paste and the improvement of the mechanical properties of concrete were achieved.

CN118908658APending Publication Date: 2024-11-08ZHEJIANG COMMUNICATIONS CONSTRUCTION NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411001489.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies for rubber concrete have high preparation costs, rubber powder is prone to floating and stratification, and the modification process is complex, resulting in poor mechanical properties and insufficient bonding strength between modified rubber powder and cement paste.

Method used

By preheating the rubber powder to regulate its morphology and form a hard shell, the particle size is controlled and it replaces fine aggregates. Combined with panthenol, sodium phytate and allantoin coating treatment, the bonding strength and mechanical properties of the rubber powder and cement paste are improved.

Benefits of technology

It effectively solves the problems of high preparation cost and stratification of rubber concrete, and improves the bonding strength between rubber powder and cement paste and the mechanical properties of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908658A_ABST
    Figure CN118908658A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of preheated rubber powder concrete, which comprises the following steps: S1, carrying out high-temperature heating reaction on waste rubber powder, and after the reaction is finished, carrying out post-treatment to obtain preheated rubber powder; s2, preparing raw materials of the concrete; s3, firstly adding the aggregate into a stirrer, stirring for 1-2 minutes, then adding half of the water in parts by weight, stirring for 1-2 minutes, then adding the rest raw materials of the concrete by a co-doping method, and carrying out wet stirring for 2-3 minutes until the mixture is uniformly dispersed; s4, the mixture is added into a test mold in a layered and graded mode, vibrating and compacting are conducted, demolding and curing are conducted after forming is conducted for 12-24 h, and the concrete is obtained. The morphology of the rubber powder is regulated and controlled in a preheating mode, and the preheated rubber powder is used for partially replacing fine aggregate, so that the problems that the existing rubber concrete is high in preparation cost, easy to stir and layer and poor in mechanical property are solved; the preheating rubber powder has the advantages that the mechanical property of the preheating rubber powder, the bonding strength of the preheating rubber powder and cement paste and the mechanical property of concrete are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete, and in particular to a method for preparing preheated rubber powder concrete. Background Art

[0002] A large number of waste tires are sent to landfills, which will cause serious environmental problems. Using rubber tires as a substitute for part of the aggregate in concrete is a feasible solution. Studies have shown that after waste rubber particles are applied to cement-based materials, the elasticity of cement-based materials increases, which can improve its impact resistance, frost resistance, crack resistance, sound absorption, thermal insulation, and heat insulation. It also has anti-skid, sound absorption, anti-salt spray corrosion, and anti-foundation alkali properties. However, due to the hydrophobicity of rubber, the surrounding cement slurry curing efficiency is low. At the same time, the rubber particles have low stiffness and large deformation under stress, which leads to rapid crack development in the surrounding cement slurry and low concrete strength. Existing methods mostly use physical or chemical treatment to modify the surface of rubber particles to change their hydrophobicity, thereby increasing their bonding with cement and improving compressive strength. The main methods include ultrasonic water washing, ozone or sulfur trioxide activation, NaOH solution cleaning, etc. to make the rubber powder surface bind hydrophilic polar groups, such as carboxyl and sulfonic acid groups, to prepare the corresponding modified rubber powder. However, there are large deviations in the test results of these methods, and the strength improvement effect is not obvious.

[0003] The Chinese patent with the authorization announcement number CN115159902B discloses a rubber concrete, whose raw materials include, by weight: 200-250 parts of cement, 350-500 parts of sand, 1100-1300 parts of crushed stone, 50-80 parts of modified rubber powder, 3-5 parts of reinforcing agent, 3-5 parts of water reducer and 90-135 parts of water; the modified rubber powder is: waste rubber powder is treated with alkaline aqueous solution, then oxidized with potassium permanganate aqueous solution under acidic conditions; then sulfonated with dodecylbenzene sulfonic acid solution; and then coated with peach tree resin, and finally crushed. The rubber powder is coated with peach tree resin to form a composite structure with organic waste rubber powder as the core and organic peach tree resin as the shell. The composite structure takes into account the advantages of both materials. The rubber powder as an elastomer can improve the crack resistance of concrete; and the resin can improve the bonding strength of the rubber powder. The rubber powder coated with peach tree resin is used to prepare rubber concrete, which has good compatibility, high interface bonding strength, and can significantly improve the anti-permeability and insulation properties of concrete.

[0004] The above-mentioned prior art solutions have the following defects: the above-mentioned concrete improves the mechanical properties of concrete by applying organic peach tree resin modified rubber powder, but in the actual preparation process, since the density of the modified rubber powder is much smaller than the density of the slurry, the modified rubber powder is easy to float on the surface of the slurry, thereby causing mixing stratification, and the modification process of the modified rubber powder is complicated and the preparation cost is too high, so it is not suitable for large-scale promotion and use; in addition, the shell-core composite structure interface of the modified rubber powder is soft. Although it can be well deformed in coordination with the cement around the interface when subjected to force, its surface mechanical properties are not good, and the bonding strength with the cement slurry is still insufficient, which is not conducive to improving the performance of concrete. Summary of the invention

[0005] The problem to be solved by the present invention is to provide a method for preparing preheated rubber powder concrete in view of the above-mentioned deficiencies in the prior art. The method regulates the morphology of the rubber powder by preheating, and partially replaces the fine aggregate with the preheated rubber powder, thereby solving the problems of high preparation cost, easy mixing and stratification, and poor mechanical properties of the existing rubber concrete. The method has the advantages of improving the mechanical properties of the preheated rubber powder, the bonding strength between the preheated rubber powder and cement paste, and the mechanical properties of the concrete.

[0006] The above-mentioned object of the present invention is achieved through the following technical solutions:

[0007] A method for preparing preheated rubber powder concrete comprises the following steps:

[0008] S1: heating the waste rubber powder at high temperature for reaction, and then post-treating the waste rubber powder after the reaction to obtain preheated rubber powder;

[0009] S2 preparing the raw materials of the concrete, wherein each cubic meter of the concrete comprises 325.00-375.00 kg of cement, 1700.00-1900.00 kg of aggregate, 45.00-55.00% of water accounting for the total weight of the cement, and 0.50-0.60% of the total weight of the cement as a water reducer, the aggregate comprises coarse aggregate, 50.00-75.50% of the total weight of the coarse aggregate as fine aggregate, and 3.50-15.00% of the preheated rubber powder accounting for the total weight of the coarse aggregate;

[0010] S3: first add the aggregate into the mixer, mix for 1-2 minutes, then add half the weight of the water, mix for 1-2 minutes, then add the remaining raw materials of the concrete by the same mixing method, wet mix for 2-3 minutes, until the mixture is evenly dispersed;

[0011] S4: adding the mixture into the test mold in layers and batches, vibrating and compacting, demolding after molding for 12 to 24 hours, and curing to obtain the concrete.

[0012] By adopting the above technical scheme, the waste rubber powder can effectively control the morphology of the rubber powder after high-temperature heating reaction at a predetermined heating temperature and heating time, so that most of the impurities and fibers attached to the surface of the waste rubber powder are removed, the surface cracks and roughness are reduced, and the particle size of the rubber particles is controlled to be 40 meshes to 3 mm, which is helpful to improve the bonding strength between the preheated rubber powder and the cement paste, and at the same time, a hard shell can be formed on the surface of the rubber particles, reducing the softness of the preheated rubber powder at the interface and improving its mechanical properties; at the same time, by regulating the replacement rate of the preheated rubber powder for fine aggregate, the preheated rubber powder can be embedded with the fine aggregate to limit the upward segregation and stratification of the preheated rubber powder and evenly disperse it in the concrete, thereby greatly improving the mechanical properties of the concrete.

[0013] Furthermore, in S1, the heating temperature is controlled to be 175-225°C, and the heating time is 45-75 minutes. Preferably, the heating temperature is controlled to be 200°C, and the heating time is 60 minutes.

[0014] Furthermore, in S1, the post-treatment includes cooling, crushing, and sieving to control the particle size of the pre-heated rubber powder to be 40 mesh to 3 mm and the bulk density to be 500 to 550 kg / m³. The morphology of the pre-heated rubber powder has a great influence on the performance of concrete, and the post-treatment can separate the rubber particles aggregated after cooling to control the particle size of the pre-heated rubber powder within a predetermined range.

[0015] Furthermore, in S1, after the waste rubber powder is subjected to high-temperature heating reaction for 10 to 15 minutes, the solution of panthenol, sodium phytate and allantoin is sprayed in sequence by atomization, and the waste rubber powder is stirred while spraying. After the spraying is completed, the high-temperature heating reaction is continued to the predetermined heating time. After the waste rubber powder is preheated for a period of time for surface modification, panthenol, sodium phytate and allantoin are introduced for coating. In the subsequent high-temperature heating process, these components will partially penetrate into the hard shell on the surface of the rubber particles, so as to be combined with limestone and natural river sand and distributed in the CS-Si gel. When the preheated rubber powder is blended with cement, its dispersion is more uniform, which can make the cement hydration degree more, and can effectively improve the slurry packing density of the concrete, thereby achieving the purpose of improving the mechanical properties of the concrete such as impermeability, tensile strength and compression.

[0016] Furthermore, in S1, the concentrations of panthenol, sodium phytate and allantoin are controlled to be 10-15wt% respectively, the atomized particle size is 150-250μm, the atomized spray coverage is ≥95%, and the stirring speed is 1200-1500r / min. Under these conditions, panthenol, sodium phytate and allantoin can be effectively penetrated into the hard shell on the surface of the rubber particles without affecting the further formation of the hard shell in the subsequent high-temperature heating process.

[0017] Further, in S2, the coarse aggregate is small limestone with a particle size of less than 10 mm and large limestone with a particle size of 10-20 mm and a total weight of 2.00-2.50 times that of the small limestone. Preferably, the mass ratio of the small limestone to the large limestone is 1:2.34.

[0018] Furthermore, the specific gravity of the coarse aggregate is 2.70-2.75 and the bulk density is 1570-1630 kg / m³.

[0019] Furthermore, in S2, the fine aggregate is natural river sand with a particle size of less than 5 mm. Compared with machine-made sand and dredged sea sand, the concrete prepared by combining natural river sand with preheated rubber powder has better performance.

[0020] Furthermore, the specific gravity of the fine aggregate is 2.63-2.68 and the bulk density is 1400-1450 kg / m³.

[0021] By preheating the rubber powder to replace the fine aggregate in different proportions, it is not only easier to disperse the preheated rubber powder in the concrete, but also possible to prepare concrete of different strength grades, which is convenient for on-site construction adjustments.

[0022] Further, in S2, the strength grade of the concrete is C40, and the aggregate includes 1042.00 kg of coarse aggregate, 783.00 kg of fine aggregate, and 39.10 kg of preheated rubber powder.

[0023] Alternatively, in S2, the strength grade of the concrete is C30, and the aggregate includes 1042.00 kg of coarse aggregate, 696.00 kg of fine aggregate, and 78.10 kg of preheated rubber powder.

[0024] Alternatively, in S2, the strength grade of the concrete is C20, and the aggregate includes 1042.00 kg of coarse aggregate, 522.00 kg of fine aggregate, and 156.20 kg of preheated rubber powder.

[0025] In summary, the beneficial technical effects of the present invention are as follows: by means of reasonable high-temperature heating and controlling the particle size of rubber particles, most of the impurities and fibers attached to the surface of the rubber particles are removed, which helps to strengthen the bonding strength between the rubber particles and the cement paste, and at the same time forms a hard shell on the rubber particles, reducing its softness at the interface, improving the mechanical properties of the rubber particle surface, and thus improving the strength of the rubber concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is the SEM picture of the waste rubber powder of Example 1 of the present invention.

[0027] Figure 2is a SEM image of the preheated rubber powder of Example 1 of the present invention.

[0028] Figure 3 (a) is a SEM image of the interface between waste rubber powder and cement paste in Example 1 of the present invention.

[0029] Figure 3 (b) is a SEM image of the interface between the preheated rubber powder and cement paste in Example 1 of the present invention.

[0030] Figure 4 (c) is a SEM image of the interface between waste rubber powder and cement paste in Comparative Example 1 of the present invention.

[0031] Figure 4 (d) is a SEM image of the interface between the preheated rubber powder and cement paste in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0032] In order to make the technical means, creative features, objectives and functions achieved by the present invention clearer and easier to understand, the present invention is further explained below in conjunction with the accompanying drawings and specific implementation methods.

[0033] Embodiment 1: A method for preparing preheated rubber powder concrete disclosed in the present invention comprises the following steps:

[0034] S1: The waste rubber powder is subjected to high temperature heating reaction, the heating temperature is controlled to be 200°C, the heating time is 60 minutes, and after the reaction is completed, it is cooled, crushed, and sieved to obtain preheated rubber powder with a particle size of 40 mesh and a bulk density of 530kg / m³;

[0035] S2 prepares the raw materials of concrete, wherein each cubic meter of concrete includes 351 kg of cement, 1864.10 kg of aggregate, 50.14% of water accounting for the total weight of cement, and 0.55% of water reducing agent accounting for the total weight of cement, and the aggregate includes coarse aggregate, fine aggregate accounting for 75.14% of the total weight of coarse aggregate, and preheated rubber powder accounting for 3.75% of the total weight of coarse aggregate; wherein,

[0036] The cement is PO42.5 cement;

[0037] Coarse aggregate is small limestone with a particle size of less than 10mm and large limestone with a particle size of 10-20mm, which is 2.35 times the total weight of small limestone. The specific gravity of coarse aggregate is 2.72 and the bulk density is 1590kg / m³.

[0038] Fine aggregate is natural river sand with a particle size of less than 5mm, with a specific gravity of 2.65 and a bulk density of 1420kg / m³;

[0039] The water reducing agent is a polycarboxylate water reducing agent;

[0040] S3: First add aggregate into the mixer, mix for 1 minute, then add half the weight of water, mix for 1 minute, then add the remaining raw materials of concrete by the same mixing method, wet mix for 2 minutes, until the mixture is evenly dispersed;

[0041] S4: Add the mixture into the test mold in layers and batches, vibrate and compact it, demould it after 12 hours of molding, and cure it to obtain concrete.

[0042] Embodiment 2: A method for preparing preheated rubber powder concrete disclosed in the present invention, which is different from Embodiment 1 in that it comprises the following steps:

[0043] S1: The waste rubber powder is subjected to high temperature heating reaction, the heating temperature is controlled to be 175°C, the heating time is 45 minutes, and after the reaction is completed, it is cooled, crushed, and sieved to obtain preheated rubber powder with a particle size of 40 mesh and a bulk density of 500kg / m³;

[0044] S2 prepares raw materials for concrete, wherein each cubic meter of concrete includes 325.00 kg of cement, 1700.00 kg of aggregate, 45.00% of water accounting for the total weight of cement, and 0.50% of water reducing agent accounting for the total weight of cement, and the aggregate includes coarse aggregate, fine aggregate accounting for 50.00% of the total weight of coarse aggregate, and preheated rubber powder accounting for 15.00% of the total weight of coarse aggregate; wherein,

[0045] The cement is PO42.5 cement;

[0046] Coarse aggregate is small limestone with a particle size of less than 10mm and large limestone with a particle size of 10~20mm, which is 2.00 times the total weight of small limestone. The specific gravity of coarse aggregate is 2.70 and the bulk density is 1570kg / m³.

[0047] Fine aggregate is natural river sand with a particle size of less than 5mm, with a specific gravity of 2.63 and a bulk density of 1400kg / m³;

[0048] The water reducing agent is a polycarboxylate water reducing agent;

[0049] S3: First add aggregate into the mixer, mix for 1 minute, then add half the weight of water, mix for 1 minute, then add the remaining raw materials of concrete by the same mixing method, wet mix for 2 minutes, until the mixture is evenly dispersed;

[0050] S4: Add the mixture into the test mold in layers and batches, vibrate and compact it, demould it after 12 hours of molding, and cure it to obtain concrete.

[0051] Embodiment 3: A method for preparing preheated rubber powder concrete disclosed in the present invention, which is different from Embodiment 1 in that it comprises the following steps:

[0052] S1: The waste rubber powder is subjected to high temperature heating reaction, the heating temperature is controlled to be 225°C, the heating time is 75 minutes, and after the reaction is completed, it is cooled, crushed, and sieved to obtain preheated rubber powder with a particle size of 3mm and a bulk density of 550kg / m³;

[0053] S2 prepares the raw materials of concrete, wherein each cubic meter of concrete includes 375.00 kg of cement, 1900.00 kg of aggregate, 55.00% of water accounting for the total weight of cement, and 0.60% of water reducing agent accounting for the total weight of cement, and the aggregate includes coarse aggregate, fine aggregate accounting for 75.50% of the total weight of coarse aggregate, and preheated rubber powder accounting for 3.50% of the total weight of coarse aggregate; wherein,

[0054] The cement is PO42.5 cement;

[0055] Coarse aggregate is small limestone with a particle size of less than 10mm, and large limestone with a particle size of 10~20mm, which is 2.00~2.50 times the total weight of small limestone. The specific gravity of coarse aggregate is 2.75 and the bulk density is 1630kg / m³.

[0056] Fine aggregate is natural river sand with a particle size of less than 5mm, with a specific gravity of 2.68 and a bulk density of 1450kg / m³;

[0057] The water reducing agent is a polycarboxylate water reducing agent;

[0058] S3: First add aggregate into the mixer, mix for 1 minute, then add half the weight of water, mix for 1 minute, then add the remaining raw materials of concrete by the same mixing method, wet mix for 2 minutes, until the mixture is evenly dispersed;

[0059] S4: Add the mixture into the test mold in layers and batches, vibrate and compact it, demould it after 12 hours of molding, and cure it to obtain concrete.

[0060] Example 4: A method for preparing preheated rubber powder concrete disclosed in the present invention, which is different from Example 1 in that, in S1, after the waste rubber powder is subjected to high-temperature heating reaction for 15 minutes, solutions of panthenol, sodium phytate and allantoin are sprayed in sequence by atomization, and the concentrations of the solutions of panthenol, sodium phytate and allantoin are controlled to be 10, 12 and 15wt%, respectively, the atomized particle size is 220μm, the atomized spray coverage is ≥95%, and the waste rubber powder is stirred while spraying, and the stirring speed is controlled to be 1300r / min. After the spraying is completed, the high-temperature heating reaction is continued to the predetermined heating time.

[0061] Examples 5 to 8 are a method for preparing preheated rubber powder concrete disclosed in the present invention. The difference from Example 1 is that the technical parameters of the preheated rubber powder, natural river sand and rubber concrete are shown in Table 1.

[0062] Comparative Examples 1 to 10 are a preparation method of preheated rubber powder concrete disclosed in the present invention, which is different from Example 1 in that the technical parameters of the preheated rubber powder, natural river sand, and rubber concrete are shown in Table 1.

[0063] Table 1

[0064] Relative content of preheated rubber powder / % Preheating rubber powder size Heating time / h Natural river sand dosage / kg / m³ Preheating rubber powder dosage / kg / m³ 7d compressive strength / MPa 28d compressive strength / MPa 28d indirect tensile strength / MPa Example 1 10 40 mesh 1.0 783 39.1 33.4±2.30 50.1±0.03 5.2±0.30 Example 4 10 40 mesh 1.0 783 39.1 31.4±0.56 52.8±0.12 6.2±0.14 Example 5 20 40 mesh 1.0 696 78.1 30.3±0.36 42.8±0.48 4.6±0.23 Example 6 40 40 mesh 1.0 522 156.2 23.5±0.40 31.3±0.97 3.6±0.02 Example 7 20 30 mesh 1.0 696 78.1 29.5±0.44 41.6±2.31 4.5±0.08 Example 8 20 1~3mm 1.0 696 78.1 26.3±0.66 39.2±0.89 4.2±0.02 Comparative Example 1 20 2~5mm 1.0 696 78.1 24.8±0.15 34.6±1.80 4.0±0.23 Comparative Example 2 20 2~5mm 1.5 696 78.1 26.0±0.27 36.9±0.71 4.5±0.17 Comparative Example 3 20 2~5mm 2.0 696 78.1 26.1±0.08 37.2±0.70 4.1±0.11 Comparative Example 4 0 / / 869 0 37.5±0.12 50.9±1.65 4.9±0.09 Comparative Example 5 10 40 mesh 0 783 37.7 29.4±0.40 40.0±0.24 4.2±0.10 Comparative Example 6 20 40 mesh 0 696 75.5 20.2±2.50 30.5±0.69 3.2±0.15 Comparative Example 7 40 40 mesh 0 522 151 10.1±1.00 13.7±1.41 1.9±0.01 Comparative Example 8 20 30 mesh 0 696 75.5 23.5±0.05 32.5±0.18 3.2±0.10 Comparative Example 9 20 1~3mm 0 696 75.5 24.0±0.65 33.3±0.11 3.6±0.10 Comparative Example 10 20 2~5mm 0 696 75.5 24.4±0.96 33.6±0.61 3.8±0.06

[0065] As can be seen from Table 1, when the rubber powder addition amount is 10%, 20% and 40%, the compressive strength loss after heat treatment is recovered by 49%, 58% and 49% within 7 days, 93%, 60% and 47% within 28 days, and the tensile strength is recovered by 106%, 82% and 57%. Considering the influence of different rubber particle sizes, the smaller the rubber powder particle size, the higher the strength recovery rate that can be achieved by heat treatment. When using 40 mesh, #0 mesh, 1~3mm and 2~5mm rubber sizes, the compressive strength loss of rubber after heat treatment is recovered by 58%, 43%, 17% and 3% within 7 days, and the compressive strength loss is recovered by 60%, 49%, 33% and 6% within 28 days. With the extension of heating time, the stiffness of rubber powder increases and the strength recovery also increases slightly. After heating for 1h, 1.5h and 2h, the compressive strength of the rubber increased by 1.6%, 6.6% and 7.0% respectively at 7 days, and by 3.0%, 9.8% and 10.7% respectively at 28 days.

[0066] from Figures 1 to 4 It can be seen that the rubber powder consists of rubber particles and impurities attached to it, and the impurities will hinder the effective connection between the rubber particles and the surrounding concrete. After heat treatment, the impurities around the rubber powder basically disappear, the interface gap is reduced, and there is a higher bonding force between the rubber particles and the surrounding cementitious materials.

[0067] Comparative Examples 11 to 31 are a method for preparing preheated rubber powder concrete disclosed in the present invention. The difference from Example 1 is that the modification method of the rubber powder and the technical parameters of the concrete are shown in Table 2, wherein CRC, ARCRC, and TT CRC are concrete without adding rubber powder, concrete with adding unmodified rubber powder, and concrete with adding modified rubber powder, respectively.

[0068] Table 2

[0069] Modification method Relative content of modified rubber powder / % CRC-28d compressive strength / MPa AR CRC-28d compressive strength / MPa TT CRC-28d compressive strength / MPa Concrete strength recovery rate / % Comparative Example 11 KMnO4 modification for 2h, NaHso3 modification for 1h 4 49.2 23.6 35.1 44.9 Comparative Example 12 Limestone powder pre-coating 5 40.0 34.0 36.5 41.7 Example 1 High temperature heating for 1h 10 50.9 40.0 50.1 92.7 Comparative Example 13 Limestone powder pre-coating 10 40.0 305 33.0 26.3 Comparative Example 14 CaCl2 modification 24h 15 51.3 37.1 42.3 36.6 Comparative Example 15 MgSO4 modification 24h 15 51.3 37.1 39.5 16.9 Comparative Example 16 Limestone powder pre-coating 15 40.0 25.3 27.5 15.0 Example 5 High temperature heating for 1h 20 50.9 30.5 42.8 60.3 Comparative Example 17 NaOH cleaning 30min 20 53.5 41.6 48.1 54.6 Comparative Example 18 NaOH cleaning 30min 20 520 37.0 42.8 38.7 Comparative Example 19 NaOH cleaning 30min 20 53.5 35.9 42.1 35.2 Comparative Example 20 NaOH cleaning 24h 20 55.6 27.0 35.0 28.0 Comparative Example 21 Soak in water for 24 hours 20 55.6 27.0 34.9 27.6 Comparative Example 22 Soak in water for 24 hours 20 35.4 215 246 22.3 Comparative Example 23 NaOH cleaning 1h 20 53.5 35.9 38.6 15.3 Comparative Example 24 NaOH cleaning for 2h 20 53.5 35.9 37.2 7.4 Comparative Example 25 Cement and silane pre-coating 30 38.0 23.0 28.5 36.7 Comparative Example 26 NaOH cleaning 24h 30 63.0 27.4 31.4 11.2 Comparative Example 27 Soak in water for 24 hours 30 63.0 27.4 30.9 9.8 Comparative Example 28 Cement slurry pre-coating 38 54.0 32.0 37.0 22.7 Comparative Example 29 Washing 38 54.0 32.0 33.5 6.8 Comparative Example 30 NaOH cleaning 20min 38 54.0 32.0 33.0 4.5 Example 6 High temperature heating for 1h 40 50.9 13.7 31.3 47.3 Comparative Example 31 Washing 40 46.8 22.4 26.2 15.6

[0070] It can be seen from Table 2 that the heat treatment method proposed in the present invention can achieve the largest concrete strength recovery ratio, which is 92.7%. The rubber content is divided into three categories: 4-10%, 15-20% and 30-40%. The degree of improvement of the strength by the heat treatment method in each category is still better than that of similar products.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing preheated rubber powder concrete, characterized in that: The following steps are included: S1: heating the waste rubber powder at high temperature for reaction, and then post-treating the waste rubber powder after the reaction to obtain preheated rubber powder; S2 preparing the raw materials of the concrete, wherein each cubic meter of the concrete comprises 325.00-375.00 kg of cement, 1700.00-1900.00 kg of aggregate, 45.00-55.00% of water accounting for the total weight of the cement, and 0.50-0.60% of the total weight of the cement as a water reducer, the aggregate comprises coarse aggregate, 50.00-75.50% of the total weight of the coarse aggregate as fine aggregate, and 3.50-15.00% of the preheated rubber powder accounting for the total weight of the coarse aggregate; S3: first add the aggregate into the mixer, mix for 1-2 minutes, then add half the weight of the water, mix for 1-2 minutes, then add the remaining raw materials of the concrete by the same mixing method, wet mix for 2-3 minutes, until the mixture is evenly dispersed; S4: adding the mixture into the test mold in layers and batches, vibrating and compacting, demolding after molding for 12 to 24 hours, and curing to obtain the concrete.

2. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: In S1, the heating temperature is controlled to be 175-225° C., and the heating time is controlled to be 45-75 min.

3. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: In S1, the post-treatment includes cooling, crushing, and sieving to control the particle size of the preheated rubber powder to be 40 mesh to 3 mm and the bulk density to be 500 to 550 kg / m³.

4. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: In S2, the coarse aggregate is small limestone with a particle size of less than 10 mm, and large limestone with a particle size of 10 to 20 mm, which accounts for 2.00 to 2.50 times the total weight of the small limestone.

5. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: The specific gravity of the coarse aggregate is 2.70-2.75, and the bulk density is 1570-1630 kg / m³.

6. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: In S2, the fine aggregate is natural river sand with a particle size of less than 5 mm.

7. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: The specific gravity of the fine aggregate is 2.63-2.68 and the bulk density is 1400-1450 kg / m³.

8. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: In S2, the strength grade of the concrete is C40, and the aggregates include 1042.00 kg of coarse aggregate, 783.00 kg of fine aggregate, and 39.10 kg of preheated rubber powder.

9. The method for preparing preheated rubber powder concrete according to claim 1, characterized in that: In S2, the strength grade of the concrete is C30, and the aggregates include 1042.00 kg of coarse aggregate, 696.00 kg of fine aggregate, and 78.10 kg of preheated rubber powder.