Rubber composition for tire shoulder pad rubber and preparation method thereof
By using trans polyoctene rubber and specific carbon black and sulfur in the shoulder pad, the thermal oxygen aging resistance and dimensional stability of the shoulder pad pad is improved, and the performance deficiency and production in the existing technology are solved. The problem of low efficiency has achieved efficient preparation of shoulder pads.
Patent Information
- Application Number
- CN202411108438.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-08
AI Technical Summary
The existing shoulder pads have shortcomings in thermal oxygen aging resistance and dimensional stability, and are low in production efficiency, which makes them prone to edge breaking problems.
Using natural rubber as the matrix, trans polyoctene rubber is introduced as a compatibilizer, and carbon black with specific iodine absorption and oil absorption values, as well as insoluble sulfur and sulfur donors, combined with specific process steps and formulas to enhance the product resilience, mechanical properties and dimensional stability.
It achieves high resilience, mechanical properties and dimensional stability, and has good thermal oxygen aging resistance, improved production efficiency, and avoids edge breaking problems.
Smart Images

Figure BDA0004991488210000061 
Figure BDA0004991488210000071 
Figure BDA0004991488210000072
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber, and in particular to a rubber composition for tire shoulder pads and a preparation method thereof. Background Art
[0002] The tire shoulder pad is located below the tread, outside the belt layer, above the carcass, and is wrapped by the sidewall. It mainly buffers the internal stress of the tire, thereby extending the service life of the tire. Since the shoulder pad is located at a low heat dissipation rate and is at the thickest position of the tire, this component needs to have sufficient heat-oxidative aging resistance and rebound performance. At the same time, the shoulder pad is in a transitional position, so the thinnest thickness is generally as small as possible and cannot exceed 0.5mm.
[0003] Currently available shoulder pads generally use white carbon black and silane coupling agents as ingredients to obtain high rebound performance. However, the introduction of white carbon black increases the number of mixing stages during product preparation, and the semi-finished products shrink greatly during the preparation process, with poor dimensional stability. The thinnest thickness during storage may exceed 1mm, and edge breakage problems are prone to occur, requiring an extended production cycle. The production efficiency is much lower than that of conventional carbon black system shoulder pad products. Summary of the invention
[0004] Based on the defects of the prior art, the purpose of the present invention is to provide a rubber composition. The product uses a specific trans-polyoctene rubber as a compatibilizer in a rubber matrix, compounded with carbon black with specific iodine absorption values and oil absorption values, and introduces insoluble sulfur and sulfur donors. Under the synergistic effect of various components, not only can the ideal high resilience, mechanical properties and dimensional stability be achieved, but also good heat-oxidative aging resistance and excellent comprehensive performance can be achieved.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A rubber composition comprising the following raw materials in parts by weight:
[0007] 100 parts of natural rubber, 5-20 parts of trans-polyoctene rubber, 17-35 parts of carbon black A, 7-25 parts of carbon black B, 1.6-2.4 parts of insoluble sulfur, 0.45-1.35 parts of sulfur donor and 1-2 parts of accelerator;
[0008] The carbon black A has an iodine absorption value of 60 to 87 g / kg and a DBP oil absorption value of 67 to 107×10 -5 m 3 / kg;
[0009] The carbon black B has an iodine absorption value of 32 to 59 g / kg and a DBP oil absorption value of 85 to 127×10 -5 m 3 / kg.
[0010] The rubber composition of the present invention is different from existing products in that the formula system of white carbon black + silane coupling agent is not used to achieve high resilience performance. Instead, on the basis of natural rubber as a matrix, trans-polyoctene rubber is first used as a compatibilizer. This component can make the product have ideal high tensile strength and elasticity based on its crystallinity and high proportion of cyclic macromolecular structure during natural rubber processing. At the same time, two carbon black compounds with different iodine absorption values / oil absorption values are introduced as reinforcing fillers. At the same time, a certain proportion of insoluble sulfur and sulfur donor are compounded to provide the product with certain rigid strength and anti-flexibility, and at the same time, dimensional stability is significantly improved. The selection of these two specific carbon black compounds can also ensure that the mechanical properties of the product after thermal oxidative aging are maintained at a high level. If an inappropriate carbon black is selected or a single carbon black formula is used, the product may not be able to obtain ideal basic performance, dimensional stability and thermal oxidative aging resistance.
[0011] At the same time, the inventors have found through experiments that the special formula system is only suitable for natural rubber matrix resin. If it is replaced with an inappropriate rubber body such as styrene-butadiene rubber, the prepared product will not only have poor mechanical and elastic properties, but also relatively low performance retention after thermal oxidative aging, and the dimensional stability during processing cannot be guaranteed; on the other hand, trans-polyoctene rubber has a significant toughening effect. Excessive introduction will inevitably lead to an imbalance in the rigidity and toughness of the product, and the component has relatively weak resistance to thermal oxidative aging, which will lead to the deterioration of the product's resistance to thermal oxidative aging. Therefore, it is necessary to adjust its addition amount within a specific range.
[0012] Preferably, the Mooney viscosity of the natural rubber according to ASTM D1646 standard is ≥70MU.
[0013] Preferably, the relative molecular weight of the trans-polyoctene rubber is 120,000-150,000, and the melting point is 50-58°C.
[0014] More preferably, the trans-polyoctene rubber has a melt viscosity of 15 to 20 m / s at 190°C and 2.16 kg load according to ISO 1133. 3 / 10min.
[0015] Trans-polyoctene rubber is a composite structure formed by cyclic molecules entangled with linear rubber molecules. Therefore, after the introduction of natural rubber, it not only has good affinity, but also has high deformation resistance, which enables the product to achieve high resilience. At the same time, this component has high cross-linking activity and can achieve high degree and high uniformity of cross-linking without the introduction of additional cross-linking agents.
[0016] Preferably, the accelerator includes at least one of a thiazole accelerator, a sulfenamide accelerator, and a thiuram accelerator.
[0017] Preferably, the mass ratio of carbon black A to carbon black B is (1-3):1.
[0018] The inventors have discovered through experiments that carbon black with high iodine absorption value / oil absorption value and carbon black with low iodine absorption value / oil absorption value are not only related to the degree of bonding and uniformity when bonding with rubber, but also have an impact on the mechanical properties, dimensional stability and even heat-oxidative aging resistance of the product. When the carbon blacks of both types are maintained at the above-mentioned preferred levels, the product can not only achieve the best balance of rigidity and toughness, but also the mechanical properties such as tensile strength and elongation at break after heat-oxidative aging can be maintained at a higher level.
[0019] Preferably, the mass ratio of the insoluble sulfur to the sulfur donor is (2-3):1.
[0020] More preferably, the sulfur donor is dicaprolactam disulfide.
[0021] In the rubber composition of the present invention, insoluble sulfur and sulfur donor need to be used in combination, and when the total amount of sulfur remains unchanged (that is, the total amount of insoluble sulfur and sulfur donor remains unchanged), the change in the ratio of the two will affect the mechanical properties of the product, especially the tensile strength and the tensile strength retention rate after thermal oxidative aging. When the ratio of the two is preferably within the above range, the product can not only maintain a high intrinsic tensile strength, but also maintain the tensile strength retention rate at a higher level after thermal oxidative aging.
[0022] Preferably, the oil-filling amount of the insoluble sulfur is 15-33%.
[0023] The inventors found in their research that the performance of products prepared by using insoluble sulfur with different oil filling amounts and compounding with a sulfur donor is also different. In terms of tensile strength and flexural resistance, if the oil filling amount is too low, the performance of the product prepared using the insoluble sulfur as a raw material will be reduced.
[0024] Preferably, the raw materials for preparing the rubber composition further include a processing aid, and the processing aid includes 1-3 parts of stearic acid, 4-8 parts of zinc oxide, 1-4 parts of tackifying resin, 2-4 parts of antioxidant and 0.1-0.4 parts of anti-scorch agent.
[0025] More preferably, the antioxidant is a mixture of an amine antioxidant and a quinoline antioxidant.
[0026] More preferably, the antioxidant is a mixture of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline, and the mass ratio of the two is (0.5-1.5):1.
[0027] Another object of the present invention is to provide a method for preparing the rubber composition, comprising the following steps:
[0028] (1) natural rubber, trans-polyoctene rubber, stearic acid, zinc oxide, tackifying resin and antioxidant are mixed in an internal mixer and subjected to rolling for 10 to 30 seconds, followed by adding carbon black and rolling and mixing to 120 to 135° C., maintaining the temperature for 10 to 30 seconds, and rolling and mixing again to 155 to 165° C., extruding and sheeting to obtain a mixed rubber;
[0029] (2) kneading the first-stage rubber mixture in an internal mixer to 120-135° C., maintaining the temperature for 10-30 seconds, and kneading the first-stage rubber mixture again to 145-155° C., extruding and tableting to obtain a second-stage rubber mixture;
[0030] (3) The second-stage mixed rubber, insoluble sulfur, sulfur donor, accelerator and scorch retarder are mixed in an internal mixer and rolled for 30 to 60 seconds and then held for 10 to 30 seconds, followed by a second rolling for 30 to 60 seconds and a second rolling for 10 to 30 seconds, and finally rolled and mixed at 95 to 105° C., extruded and sheeted to obtain the rubber composition.
[0031] Preferably, the interval time between each mixing section is 3 to 24 hours.
[0032] The preparation method of the rubber composition of the present invention has simple operation steps, low requirements on equipment, and can realize large-scale batch production.
[0033] Another object of the present invention is to provide a tire shoulder pad, comprising the rubber composition of the present invention.
[0034] The rubber composition of the present invention has ideal performance in use, wherein in terms of performance in use, the tensile product (i.e., the product of tensile strength and elongation at break) can reach more than 14,000, the tear strength is as high as more than 67 kN / m, the mechanical properties are good, the elasticity is high (the rebound rate reaches more than 60%), the heat generation rate is low, the flexural resistance is good, the flexion times reach 100,000 times / level 3, the processing dimensional stability is good, and it has good resistance to thermal oxidative aging, and the retention rate of various performance indicators after thermal oxidative aging of the product is high.
[0035] The beneficial effect of the present invention is that the present invention provides a rubber composition, in which a specific trans-polyoctene rubber is used as a compatibilizer in a rubber matrix, carbon black with specific iodine absorption value and oil absorption value is compounded, and insoluble sulfur and sulfur donor are introduced at the same time. Under the synergistic effect of various components, not only the ideal high resilience, mechanical properties and dimensional stability can be achieved, but also the heat-oxidative aging resistance is good and the comprehensive performance is excellent. DETAILED DESCRIPTION
[0036] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0037] Example 1
[0038] An embodiment of the rubber composition of the present invention, a method for preparing the rubber composition, comprises the following steps:
[0039] (1) mixing rubber, trans-polyoctene rubber, stearic acid, zinc oxide, tackifying resin and antioxidant in an internal mixer and subjecting to rolling for 20 seconds, then adding carbon black and subjecting to rolling and mixing at 130° C., maintaining the temperature for 20 seconds, and subjecting to rolling and mixing again at 160° C., and extruding and sheeting with a twin-screw extruder to obtain a first-stage mixed rubber;
[0040] (2) After an interval of 3 hours, the first-stage mixed rubber was kneaded in an internal mixer to 130°C, maintained at this temperature for 20 seconds, and kneaded again to 150°C, and extruded and sheeted using a twin-screw extruder to obtain a second-stage mixed rubber;
[0041] (3) After an interval of 3 hours, the second-stage mixed rubber, insoluble sulfur, sulfur donor, accelerator and scorch retarder are mixed in an internal mixer and rolled for 40 seconds and then held for 20 seconds, followed by a second rolling for 40 seconds and a second rolling for 20 seconds, and finally rolled and mixed to 100° C., and extruded and sheeted by a twin-screw extruder to obtain the rubber composition.
[0042] The added materials and their weight portions are shown in Table 1.
[0043] Embodiments 2 to 11
[0044] An embodiment of the rubber composition of the present invention is different from Embodiment 1 only in the added materials and weight portions, as shown in Table 1.
[0045] Comparative Examples 1 to 13
[0046] A rubber composition, which differs from Example 1 only in the added materials and weight portions, as shown in Table 2.
[0047] The materials used in each embodiment and comparative example are as follows:
[0048] Rubber-1: natural rubber, STR20, Sri Trang Rubber Co., Ltd., Thailand;
[0049] Rubber-2: styrene-butadiene rubber, SBR1502, Sinopec Qilu Petrochemical Company;
[0050] Rubber-3: butadiene rubber, BR9000, Sinopec Qilu Petrochemical Company;
[0051] Trans-polyoctene rubber: VESTENAMER 8012, relative molecular weight 140000, melting point 54°C, melt viscosity at 190°C and 2.16kg load is 16m 3 / 10min, Evonik Industries AG, Germany;
[0052] Carbon black-1: N326, Cabot Corporation, USA, iodine absorption value is 82±5g / kg, DBP oil absorption value is 72±5×10 -5 m 3 / kg;
[0053] Carbon black-2: N330, Cabot Corporation, USA, iodine absorption value 82±5g / kg, DBP oil absorption value 102±5×10 -5 m 3 / kg;
[0054] Carbon black-3: N339, Cabot Corporation, USA, iodine absorption value 90±5g / kg, DBP oil absorption value 120±5×10 -5 m 3 / kg;
[0055] Carbon black-4: N375, Cabot Corporation, USA, iodine absorption value 90±5g / kg, DBP oil absorption value 114±5×10 -5 m 3 / kg;
[0056] Carbon black-5: N650, Cabot Corporation, USA, iodine absorption value 36±4g / kg, DBP oil absorption value 122±5×10 -5 m 3 / kg;
[0057] Carbon black-6: N660, Cabot Corporation, USA, iodine absorption value 36±4g / kg, DBP oil absorption value 90±5×10 -5 m 3 / kg;
[0058] Carbon black-7: N683, Cabot Corporation, USA, iodine absorption value 35±4g / kg, DBP oil absorption value 133±5×10 -5 m 3 / kg;
[0059] Carbon black-8: N774, Cabot Corporation, USA, iodine absorption value 29±4g / kg, DBP oil absorption value 72±5×10 -5 m3 / kg;
[0060] Zinc oxide: Zinc oxide (indirect process), Dalian Zinc Oxide Plant;
[0061] Stearic acid: Octadecanoic acid, Malaysian natural oil chemical;
[0062] Tackifying resin: SL1801, Huaqi (China) Chemical Co., Ltd.;
[0063] Antioxidant-1: N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (6PPD), Shengao Chemical Technology Co., Ltd.;
[0064] Antioxidant-2: 2,2,4-trimethyl-1,2-dihydroquinoline, Shengao Chemical Technology Co., Ltd.
[0065] Insoluble sulfur-1: HS OT10 (oil filling 10%), Puyang Weilin Chemical Co., Ltd.;
[0066] Insoluble sulfur-2: HS OT20 (oil filling 20%), Puyang Weilin Chemical Co., Ltd.;
[0067] Insoluble sulfur-3: HS OT33 (oil filling 33%), Puyang Weilin Chemical Co., Ltd.
[0068] Sulfur donor: dicaprolactam disulfide (sulfur content 22%), Puyang Weilin Chemical Co., Ltd.
[0069] Accelerator: N-cyclohexyl-2-benzothiazolesulfenamide, Puyang Weilin Chemical Co., Ltd.;
[0070] Anti-scorching agent: N-cyclohexylthiophthalimide, Puyang Weilin Chemical Co., Ltd.
[0071] Table 1
[0072]
[0073]
[0074] Table 2
[0075]
[0076]
[0077]
[0078] Effect Example 1
[0079] In order to verify the performance of the rubber composition of the present invention, the products obtained from the embodiments and comparative examples were subjected to the following tests:
[0080] (1) At 100°C, the hysteresis loss tanδ (100 cpm, 7%) of each unvulcanized product was tested using a rubber processing analyzer (RPA). The larger the value, the smaller the outlet expansion effect of the product during the extrusion production process and the better the processing dimensional stability;
[0081] (2) Each product was vulcanized (150°C, 60 min) and then tested as follows:
[0082] (2.1) Tensile properties test: refer to GB / T 528-2009, type 1;
[0083] (2.2) Elongation at break test: refer to GB / T 528-2009, type 1;
[0084] (2.3) Tear strength test: refer to GB / T 529-2008, right angle;
[0085] (2.4) Rebound test: refer to GB / T 1681-2009;
[0086] (2.5) Flexion test: refer to GB / T 13934-2006, Demosia type;
[0087] (2.6) Compression fatigue heat generation test: refer to GB / T 1687.3-2016, 55°C, stroke 4.45mm, prestress 1.0MPa;
[0088] (3) The products of step (2) were subjected to aging treatment according to GB / T 3512-2014, with the aging conditions being 100° C. and 48 h, and then performance tests were performed using the same test method as step (2), and the retention rate of each test result was calculated.
[0089] The test results are shown in Tables 3 to 5, where tensile product = tensile strength × elongation at break. When calculating, the tensile strength is based on the value in MPa, and the elongation at break is based on the value in %.
[0090] Table 3
[0091]
[0092]
[0093] Table 4
[0094]
[0095] Table 5
[0096]
[0097]
[0098] It can be clearly seen from the results that the rubber composition of the present invention has excellent processing performance, use performance and heat-oxidative aging resistance. During the processing, tanδ (100°C) is maintained above 0.73, the outlet expansion effect is small, and the dimensional stability is good; in the initial state, the tensile strength of the rubber composition can reach above 24MPa, the elongation at break can reach above 610%, and the tear strength is above 67kN / m, indicating that the product has a strong ability to withstand damage; the product has a high rebound rate, reaching 63% and above; the compression temperature rise value can be controlled within 21°C, and the heat generation rate is low; the flexural resistance is good, and the flexion times can reach at least 100,000 times / 3 levels. After the heat-oxidative aging treatment, the tensile strength retention rate can reach above 70%, the elongation at break retention rate can reach above 60%, and the tear strength retention rate can reach above 45%.
[0099] In contrast, the main rubber used in the formulation of the products of Comparative Examples 1 and 2 is not pure natural rubber. Not only can the damage resistance, tear resistance and flexural resistance not be guaranteed, but also the product performance retention rate after thermal oxidation aging is reduced compared with the product of Example 2 used as a single control. According to Examples 1 to 4 and Comparative Examples 3 and 4, it can be seen that when the product of the present invention does not introduce trans-polyoctene rubber, the product has a low tanδ (100°C) value, poor processing dimensional stability, and low initial elongation at break and tear strength, fewer flexion times, and a high heat generation rate; with the introduction of trans-polyoctene rubber, the elongation at break, tear strength and flexural resistance of the product gradually improve, the tanδ (100°C) value increases, the processing dimensional stability improves, and the performance retention rate of the product after thermal oxidative aging is also improved to a certain extent, but when the trans-polyoctene rubber increases, the flexural resistance of the product reaches a peak and then begins to decline, and the tensile strength of the product also decreases, and when the amount of this component introduced is too much, as shown in Comparative Example 4, not only the tensile strength and flexural resistance of the product are poor, but also the performance retention rate after thermal oxidative aging is lower than that of the product in Example 4.
[0100] On the other hand, in the selection of carbon black, as shown in Example 2, Examples 5 to 6 and Comparative Examples 5 to 8, it can be seen that the type of carbon black in the rubber composition of the present invention is very critical, and the iodine absorption value and oil absorption value of the two carbon blacks need to be maintained within a certain range. If an inappropriate type is selected, various intrinsic properties represented by the number of flexion times may be performed at a low level, and the product's tanδ (100°C) may also be small, as shown in Comparative Example 6, and the processing dimensional stability is poor; on the other hand, as shown in Comparative Example 5, the retention rate of the tear strength of the product after thermal oxidative aging is only 43%, which is much lower than that of the parallel comparison example product, indicating that improper selection of carbon black may also affect the product's thermal oxidative aging resistance.
[0101] According to Example 2, Examples 7-8 and Comparative Examples 9-10, it can be seen that after selecting the type of carbon black, the selection of the addition amount of the two will also affect the performance of the product, especially the flex resistance. When the content of high iodine absorption value carbon black is low, the flexion times of the product are low. As the proportion of its addition amount increases, the flexion times increase to the highest 140,000 times / level 3, but after further increase, the flexion times of the product will decrease again. Inappropriate carbon black ratio will also make it impossible to guarantee the tear strength and tensile strength of the product. In terms of heat-oxidative aging resistance and heat generation rate, if the selection is inappropriate, the product will also remain at a low level.
[0102] According to Example 2, Examples 9-10 and Comparative Examples 11-12, it can be seen that when the total amount of sulfur is certain, the ratio of insoluble sulfur and sulfur donor will also affect the performance of the product. When the proportion of insoluble sulfur is small, the various properties of the product including mechanical properties, resilience, heat generation rate and flexibility resistance are at a low level, and the thermal oxygen aging resistance is also poor. As its proportion increases, the various properties of the product are improved, but after reaching a certain level, the thermal oxygen aging performance of the product will drop sharply. As shown in Comparative Example 11, the retention rate of each property is at a low level.
[0103] It can be seen from Example 2, Example 11 and Comparative Example 13 that, when the total amount of sulfur is constant, the oil filling amount of insoluble sulfur affects the performance of the product. The oil filling amount is only 10%, which is not conducive to the dispersion of insoluble sulfur, resulting in a significant decrease in the tensile strength and elongation at break of the product at a relatively low level. The product of Comparative Example 13 cannot achieve the desired effect.
[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the present invention.
Claims
1. A rubber composition, characterized in that: The preparation comprises the following raw materials in parts by weight: 100 parts of natural rubber, 5-20 parts of trans-polyoctene rubber, 17-35 parts of carbon black A, 7-25 parts of carbon black B, 1.6-2.4 parts of insoluble sulfur, 0.45-1.35 parts of sulfur donor and 1-2 parts of accelerator; The carbon black A has an iodine absorption value of 60 to 87 g / kg and a DBP oil absorption value of 67 to 107×10 -5 m 3 / kg; The carbon black B has an iodine absorption value of 32 to 59 g / kg and a DBP oil absorption value of 85 to 127×10 -5 m 3 / kg.
2. The rubber composition according to claim 1, characterized in that: The relative molecular weight of the trans-polyoctene rubber is 120,000-150,000, and the melting point is 50-58°C.
3. The rubber composition according to claim 1, characterized in that: The trans-polyoctene rubber has a melt viscosity of 15 to 20 m / s at 190°C and a load of 2.16 kg according to ISO 1133. 3 / 10min.
4. The rubber composition according to claim 1, characterized in that: The accelerator includes at least one of a thiazole accelerator, a sulfenamide accelerator, and a thiuram accelerator.
5. The rubber composition according to claim 1, characterized in that: The mass ratio of the carbon black A to the carbon black B is (1-3):
1.
6. The rubber composition according to claim 1, characterized in that: The mass ratio of the insoluble sulfur to the sulfur donor is (2-3):
1.
7. The rubber composition according to claim 1, characterized in that: The sulfur donor is dicaprolactam disulfide; the oil filling amount of the insoluble sulfur is 15-33%.
8. The rubber composition according to claim 1, characterized in that: The raw materials for preparing the rubber composition also include processing aids, which include 1 to 3 parts of stearic acid, 4 to 8 parts of zinc oxide, 1 to 4 parts of tackifying resin, 2 to 4 parts of antioxidant and 0.1 to 0.4 parts of anti-scorch agent.
9. The method for preparing the rubber composition according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) natural rubber, trans-polyoctene rubber, stearic acid, zinc oxide, tackifying resin and antioxidant are mixed in an internal mixer and subjected to rolling for 10 to 30 seconds, followed by adding carbon black and rolling and mixing to 120 to 135° C., maintaining the temperature for 10 to 30 seconds, and rolling and mixing again to 155 to 165° C., extruding and sheeting to obtain a mixed rubber; (2) kneading the first-stage rubber mixture in an internal mixer to 120-135° C., maintaining the temperature for 10-30 seconds, and kneading the first-stage rubber mixture again to 145-155° C., extruding and tableting to obtain a second-stage rubber mixture; (3) The second-stage mixed rubber, insoluble sulfur, sulfur donor, accelerator and scorch retarder are mixed in an internal mixer and rolled for 30 to 60 seconds and then held for 10 to 30 seconds, followed by a second rolling for 30 to 60 seconds and a second rolling for 10 to 30 seconds, and finally rolled and mixed at 95 to 105° C., extruded and sheeted to obtain the rubber composition.
10. A tire shoulder pad, characterized in that: The rubber composition comprises the rubber composition according to any one of claims 1 to 8.
Citation Information
Cited By
Composite carbon black for cable shielding material and preparation method thereof
CN121160122A
Composite carbon black for cable shielding material and preparation method thereof
CN121160122B