Anti-saponification and anti-demulsification high-entropy alloy and preparation method thereof

By using high-entropy alloys in deep-water oil and gas fields, combined with ball milling and induction smelting processes and pulsed magnetic field treatment, the problem of oil well scaling is solved, the strength and corrosion resistance of the alloy are improved, and the efficiency and safety of oil and gas mining are significantly improved.

CN118910466APending Publication Date: 2024-11-08NANJING CHAOXUSCIENCE&TECH DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411009527.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the development of deep-water oil and gas fields, fluctuations in temperature, pressure, pH and dissolved oxygen factors in the oil well and surrounding environment cause fouling of the inner and outer walls of the oil well oil pipes, affecting the efficiency of oil and gas extraction, increasing equipment corrosion and safety risks, and the existing anti-saponification and emulsion decomposition measures are limited in effect. .

Method used

Using a high-entropy alloy that is anti-saponified and demulsified, containing elements such as Ni, Zn, W, Ti, Sn, Pb and Au, alloy rods are prepared through ball milling and induction smelting processes, and pulsed magnetic fields are added during cooling to optimize Microstructure and properties of alloys.

Benefits of technology

It improves the strength and plasticity of the alloy, enhances the resistance to high temperature and corrosion, significantly reduces the risk of tubing scale and equipment damage, and improves the production efficiency and safety of oil and gas fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004963913070000121
    Figure BDA0004963913070000121
  • Figure BDA0004963913070000131
    Figure BDA0004963913070000131
  • Figure BDA0004963913070000132
    Figure BDA0004963913070000132
Patent Text Reader

Abstract

The invention belongs to the technical field of alloy materials, and particularly relates to a saponification and demulsification prevention high-entropy alloy and a preparation method thereof. The invention discloses an anti-saponification and anti-demulsification high-entropy alloy which comprises the following raw materials in percentage by weight: 5-10% of Ni, 5-25% of Zn, 1-5% of W, 1-8% of Ti, 0.1-5% of Sn, 0.05-1% of Pb, 0.01-0.05% of Au and the balance of copper and other inevitable impurities, and the content of the impurities is not higher than 0.01%. The alloy material disclosed by the invention has extremely high strength and plasticity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy materials, and in particular relates to a high entropy alloy resistant to saponification and demulsification and a preparation method thereof. Background Art

[0002] With the continuous development of deep-sea technology and the growing demand for energy, the development of deepwater oil and gas fields has become an important field in today's petroleum industry. However, in the process of developing deepwater oil and gas fields, the complexity of oil wells and the surrounding environment makes it easy for scaling to form on the inner and outer walls of oil well tubing, which has become an important factor restricting the efficient and safe production of oil fields. In deepwater environments, factors such as temperature, pressure, pH and dissolved oxygen in the oil wells and the surrounding environment will continue to change. The fluctuations of these factors not only affect the efficiency of oil and gas production, but also directly lead to the frequent scaling of the inner and outer walls of oil well tubing. Scaling will not only reduce the production capacity of oil wells and increase the difficulty of production, but also cause serious corrosion and damage to equipment, and may even cause major safety accidents. The severity of the scaling problem in oil fields cannot be ignored. It not only increases the development cost of oil and gas fields, including equipment maintenance, replacement and shutdown costs, but may also lead to a reduction in oil field production efficiency, seriously affecting the economic benefits of oil fields.

[0003] Therefore, it is particularly important to take targeted anti-saponification and demulsification measures to address scaling problems during the development of deepwater oil and gas fields. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems existing in the prior art and provide a method for preparing a high entropy alloy that is resistant to saponification and demulsification.

[0005] The purpose of the present invention and the solution to the technical problem are achieved by adopting the following technical solutions.

[0006] One aspect of the present invention provides a high entropy alloy that resists saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 5-10%, Zn 5-25%, W 1-5%, Ti 1-8%, Sn 0.1-5%, Pb0.05-1%, Au 0.01-0.05%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0007] Another aspect of the present invention provides a method for preparing a high entropy alloy that resists saponification and demulsification, the method comprising the following steps:

[0008] S1: weighing the raw material components according to their proportions, then mixing and ball-milling the raw materials to obtain mixed metal powder;

[0009] S2: drying the mixed metal powder and pouring it into a smelting furnace for smelting. After smelting, pouring it into a mold for forming to obtain an alloy rod;

[0010] S3: taking out the obtained alloy rod and cooling it, wherein a pulsed magnetic field is applied during the cooling process to obtain an alloy rod.

[0011] In a preferred embodiment of the present invention, the purity of the metal raw material in step S1 is ≥ 99.9%.

[0012] In a preferred embodiment of the present invention, the ball milling conditions in step S1 are: ball-to-material ratio is 1:(0.1-0.3), rotation speed is 200-400 rpm, and time is 20-40 h.

[0013] In a preferred embodiment of the present invention, the smelting furnace in step S2 is an induction smelting furnace.

[0014] In a preferred embodiment of the present invention, the induction melting furnace conditions are: operating voltage is 350-450V, and current is 1900A-2000A.

[0015] In a preferred embodiment of the present invention, the smelting conditions in step S2 are: temperature 350-3500°C, time 40-80 min, stirring, argon gas flow rate 8-12 m 3 .

[0016] In a preferred embodiment of the present invention, the heating process of the smelting temperature is: first, the temperature is increased to 400-500°C at a heating rate of 5-15°C / min, and then kept warm for 10-20 minutes; then, the temperature is increased to 1400-1500°C at a heating rate of 10-15°C / min, and then kept warm for 10-20 minutes; finally, the temperature is increased to 3000-3500°C at a heating rate of 10-15°C / min, and then kept warm for 20-40 minutes.

[0017] In a preferred embodiment of the present invention, the mold diameter in step S2 is 100-120 cm, and the mold height is 300-360 cm.

[0018] In a preferred embodiment of the present invention, the pulse magnetic field conditions in step S3 are: intensity of 20-30 mT, frequency of 20-40 Hz, and duty cycle of 30-50%.

[0019] By means of the above technical solution, the present invention has at least the following advantages:

[0020] 1. The alloy of the present invention has copper and zinc as main components, and the strength of the alloy can be improved by adding a small amount of metal elements such as lead, gold, tungsten, etc. The most important advantage of tungsten is that it has good high temperature strength and good corrosion resistance to molten alkali metals and vapors. However, it also has the disadvantages of high plastic-brittle transition temperature and difficulty in plastic processing at room temperature. Lead and gold have high plasticity in addition to high stability, so the shortcomings of tungsten can be overcome by adding lead and gold, so that the obtained alloy has high strength and good plasticity.

[0021] 2. In the process of drying the metal powder, the present invention adopts a spray drying method combined with two stages of inert gas to prepare each metal raw material into a porous powder, and then melts and heats it in an induction melting furnace with uniform temperature, less burn loss, uniform metal composition and high quality. In addition, the present invention applies a pulsed magnetic field during the cooling of the metal rod, which can reduce the pinning effect and thus reduce the defects inside the alloy. The pulsed magnetic field conditions of the present invention are the best optimized conditions obtained after multiple rounds of screening, and the application of this condition can significantly improve the performance of the alloy.

[0022] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION

[0023] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Unless otherwise specified, the percentage content involved in the present invention refers to mass percentage for solid-liquid mixing and solid-solid mixing, and refers to volume percentage for liquid-liquid mixing.

[0025] Unless otherwise specified, the percentage concentrations referred to in the present invention all refer to final concentrations, which refer to the percentage of the added component in the system after the addition of the component.

[0026] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.

[0027] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods.

[0028] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0029] Embodiment 1:

[0030] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0031] The preparation method of the high entropy alloy comprises the following steps:

[0032] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0033] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0034] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0035] Embodiment 2:

[0036] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 10%, Zn 25%, W 5%, Ti 1%, Sn 0.1%, Pb 1%, Au 0.05%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0037] The preparation method of the high entropy alloy comprises the following steps:

[0038] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 20 hours at a ball-to-material ratio of 1:0.1 and a rotation speed of 400 rpm to obtain mixed metal powder.

[0039] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 450V and 1900A: first, heat it to 500℃ at a heating rate of 15℃ / min and keep it warm for 10min, then heat it to 1500℃ at a heating rate of 15℃ / min and keep it warm for 10min, and finally heat it to 3500℃ at a heating rate of 15℃ / min and keep it warm for 20min. The argon gas flow rate is 8m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0040] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 20 mT, the frequency is 40 Hz, and the duty cycle is 30%, to obtain an alloy rod.

[0041] Embodiment 3:

[0042] The present embodiment provides a high entropy alloy that resists saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 5%, Zn 5%, W 1%, Ti 8%, Sn 5%, Pb 0.05%, Au 0.01%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0043] The preparation method of the high entropy alloy comprises the following steps:

[0044] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 40 hours at a ball-to-material ratio of 1:0.3 and a rotation speed of 200 rpm to obtain mixed metal powder.

[0045] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 350V and 2000A: first, heat it to 400℃ at a heating rate of 5℃ / min and keep it warm for 10-20min, then heat it to 1400℃ at a heating rate of 10℃ / min and keep it warm for 20min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 40min. The argon gas flow rate is 12m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0046] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 30 mT, the frequency is 20 Hz, and the duty cycle is 50%, to obtain an alloy rod.

[0047] Embodiment 4:

[0048] The present embodiment provides a high entropy alloy that resists saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 6%, Zn 10%, W 4%, Ti 7%, Sn 0.5%, Pb 0.1%, Au 0.02%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0049] The preparation method of the high entropy alloy comprises the following steps:

[0050] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0051] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0052] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0053] Embodiment 6:

[0054] The present embodiment provides a high entropy alloy that resists saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 9%, Zn 20%, W 2%, Ti 2%, Sn 4%, Pb 0.9%, Au 0.04%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0055] The preparation method of the high entropy alloy comprises the following steps:

[0056] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0057] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0058] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0059] Embodiment 7:

[0060] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0061] The preparation method of the high entropy alloy comprises the following steps:

[0062] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0063] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0064] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 28 mT, the frequency is 35 Hz, and the duty cycle is 45%, to obtain an alloy rod.

[0065] Embodiment 8:

[0066] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0067] The preparation method of the high entropy alloy comprises the following steps:

[0068] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0069] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0070] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 22 mT, the frequency is 25 Hz, and the duty cycle is 35%, to obtain an alloy rod.

[0071] Comparative Example 1:

[0072] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0073] The preparation method of the high entropy alloy comprises the following steps:

[0074] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0075] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0076] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 15 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0077] Comparative Example 2:

[0078] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0079] The preparation method of the high entropy alloy comprises the following steps:

[0080] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0081] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0082] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 35 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0083] Comparative Example 3:

[0084] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0085] The preparation method of the high entropy alloy comprises the following steps:

[0086] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0087] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0088] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 15 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0089] Comparative Example 4:

[0090] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0091] The preparation method of the high entropy alloy comprises the following steps:

[0092] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0093] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0094] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 45 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0095] Comparative Example 5:

[0096] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0097] The preparation method of the high entropy alloy comprises the following steps:

[0098] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0099] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0100] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 25%, to obtain an alloy rod.

[0101] Comparative Example 6:

[0102] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0103] The preparation method of the high entropy alloy comprises the following steps:

[0104] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0105] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0106] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 55%, to obtain an alloy rod.

[0107] Comparative Example 7:

[0108] The present embodiment provides a high entropy alloy that is resistant to saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, Ti 4.5%, Sn 2.5%, Pb 0.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0109] The preparation method of the high entropy alloy comprises the following steps:

[0110] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0111] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0112] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0113] Comparative Example 8:

[0114] The present embodiment provides a high entropy alloy that resists saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Pb 0.5%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0115] The preparation method of the high entropy alloy comprises the following steps:

[0116] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0117] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0118] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0119] Comparative Example 9:

[0120] The present embodiment provides a high entropy alloy that resists saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, Au 0.03%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0121] The preparation method of the high entropy alloy comprises the following steps:

[0122] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0123] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0124] S3: The alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 40% to obtain an alloy rod.

[0125] Comparative Example 10:

[0126] The present embodiment provides a high entropy alloy that resists saponification and demulsification. The raw material composition and content of the alloy are, by weight percentage, Ni 7.5%, Zn 15%, W 3%, Ti 4.5%, Sn 2.5%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

[0127] The preparation method of the high entropy alloy comprises the following steps:

[0128] S1: Weigh the raw material components according to their proportions, then mix the raw materials and ball mill them for 30 hours at a ball-to-material ratio of 1:0.2 and a rotation speed of 300 rpm to obtain mixed metal powder.

[0129] S2: After drying the mixed metal powder, pour it into the melting furnace and smelt it at 400V and 1950A: first, heat it to 450℃ at a heating rate of 10℃ / min and keep it warm for 15min, then heat it to 1450℃ at a heating rate of 10℃ / min and keep it warm for 15min, and finally heat it to 3500℃ at a heating rate of 10℃ / min and keep it warm for 30min. The argon gas flow rate is 10m 3 After smelting, it is poured into a mold with a diameter of 120 cm and a height of 360 cm to form an alloy rod.

[0130] S3: The obtained alloy rod is taken out and cooled, wherein a pulse magnetic field is applied during the cooling process: the intensity is 25 mT, the frequency is 30 Hz, and the duty cycle is 40%, to obtain an alloy rod.

[0131] Test 1: Alloy Strength Comparison

[0132] The mechanical properties of the alloys of Examples 1-8 and Comparative Examples 1-11 were tested, and the statistical results are shown in Table 1.

[0133] Table 1 Mechanical properties of different alloys

[0134]

[0135]

[0136] It can be seen from the results in Table 1 that the comprehensive performance of compressive strength, yield strength and hardness of the alloy rods of Examples 1-8 of the present invention is significantly better than that of the alloy materials of Comparative Examples 1-10.

[0137] Test 2: Viscosity reduction and demulsification performance testing of different alloys

[0138] The viscosity reduction and demulsification performance testing of the alloys of Example 1 and Comparative Examples 1-11 refers to the contents disclosed in the patent application filed by the same applicant on April 29, 2024, with application number 2024105334040, which is incorporated herein by reference.

[0139] The test results are shown in Table 2.

[0140] Table 2 Viscosity reduction and demulsification rate

[0141]

[0142]

[0143] Note: “--” in the table means no significant changes were detected.

[0144] It can be seen from the results in Table 2 that, compared with the group without alloy device, the alloys of Example 1 of the present invention and Comparative Examples 1-11 can reduce the viscosity of heavy oil to a certain extent, but compared with Comparative Examples 1-11, the viscosity reduction and demulsification effect of the alloy of Example 1 of the present invention is more obvious.

[0145] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A high entropy alloy that resists saponification and demulsification, characterized in that: Calculated by weight percentage, the raw material composition and content of the alloy are Ni 5-10%, Zn 5-25%, W 1-5%, Ti 1-8%, Sn 0.1-5%, Pb 0.05-1%, Au0.01-0.05%, and the remainder of copper and other inevitable impurities, and the impurity content is not higher than 0.01%.

2. A method for preparing a high entropy alloy resistant to saponification and demulsification according to claim 1, characterized in that: The method comprises the following steps: S1: weighing the raw material components according to their proportions, then mixing and ball-milling the raw materials to obtain mixed metal powder; S2: drying the mixed metal powder and pouring it into a smelting furnace for smelting. After smelting, pouring it into a mold for forming to obtain an alloy rod; S3: taking out the obtained alloy rod and cooling it, wherein a pulsed magnetic field is applied during the cooling process to obtain an alloy rod.

3. The method according to claim 2, characterized in that The purity of the metal raw material in step S1 is ≥ 99.9%.

4. The method according to claim 2, characterized in that: The ball milling conditions in step S1 are: ball to material ratio is 1:(0.1-0.3), rotation speed is 200-400 rpm, and time is 20-40 h.

5. The method according to claim 2, characterized in that: The smelting furnace in step S2 is an induction smelting furnace.

6. The method according to claim 5, characterized in that The induction melting furnace conditions are: operating voltage is 350-450V, and current is 1900A-2000A.

7. The method according to claim 2, characterized in that The smelting conditions in step S2 are: temperature 350-3500°C, time 40-80 min, stirring, argon gas flow rate 8-12 m 3 .

8. The method according to claim 7, characterized in that The heating process of the smelting temperature is: firstly, the temperature is increased to 400-500°C at a heating rate of 5-15°C / min and then kept warm for 10-20 minutes, then the temperature is increased to 1400-1500°C at a heating rate of 10-15°C / min and then kept warm for 10-20 minutes, and finally, the temperature is increased to 3000-3500°C at a heating rate of 10-15°C / min and then kept warm for 20-40 minutes.

9. The method according to claim 2, characterized in that: In step S2, the mold diameter is 100-120 cm, and the mold height is 300-360 cm.

10. The method according to claim 2, characterized in that The pulse magnetic field conditions in step S3 are: intensity of 20-30 mT, frequency of 20-40 Hz, and duty cycle of 30-50%.