Near-infrared high-reflection PVC (polyvinyl chloride) material and preparation method thereof
Through the modification of IR pigments, the incompatibility problem between alkaline IR pigments and plasticizers in PVC materials is solved, and the near-infrared reflectivity and stability are improved, which meets the construction membrane structure, tent tents and military materials. The requirements for efficient heat insulation and cooling performance.
Patent Information
- Application Number
- CN202411159563.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-22
AI Technical Summary
PVC materials have insufficient reflectivity in the near-infrared band, and there is incompatibility problem with alkaline IR pigments with commonly used phenylas plasticizers, which limits the performance of the material and the smoothness of the preparation process.
By modifying the BASF Sicopal Black L0095 IR pigment with dioctyl phthalate and EO/PO block polyether, the modified IR pigment works synergistically with other components in the PVC system to improve the uniform dispersion of the pigment and bonding forces, optimize the formulation design to improve reflectivity.
It significantly improves the reflectivity of PVC materials in the near infrared band, stably reaches or exceeds 40%, meets the needs of efficient heat insulation and cooling performance, and improves the stability and flame retardant performance of the material.
Smart Images

Figure BDA0005006048220000011 
Figure BDA0005006048220000021 
Figure BDA0005006048220000051
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of PVC coatings, and in particular to a near-infrared high-reflective PVC material and a preparation method thereof. Background Art
[0002] Due to its versatility, PVC coating materials have been widely used in diverse fields such as architectural membrane structures, tents and even military materials. However, as society's awareness of environmental protection and energy conservation continues to deepen, higher thermal protection standards have been proposed for the application of PVC materials in specific fields, especially its role as a thermal insulation barrier. This demand is intended to enhance the reflection ability of PVC materials to infrared radiation, especially the energy-intensive near-infrared band (700-2500 nanometers), by significantly improving the reflectivity to a higher level, such as from the current less than 10% to about 40%, thereby achieving significant thermal insulation and cooling effects.
[0003] The innovative research and development of infrared reflective PVC materials usually integrates key components such as PVC paste resin, plasticizer and IR pigment. However, in the actual production process, a significant technical challenge emerges: there is an incompatibility problem between alkaline IR pigments and commonly used orthophthalic plasticizers. This incompatibility not only limits the full performance of the material, but also constitutes a considerable obstacle to the smooth progress of the entire preparation process. Therefore, while pursuing high-efficiency infrared reflective performance, how to solve this compatibility problem has become a key technical problem that needs to be overcome in the research and development and application of infrared reflective PVC materials. Summary of the invention
[0004] To solve the above problems, the present application provides a near-infrared high-reflection PVC material and a preparation method thereof, aiming to effectively improve the incompatibility between alkaline IR pigments and ortho-phthalic plasticizers by optimizing the formula design, and at the same time to improve the reflective performance of PVC materials in the near-infrared band, ensuring that the reflectivity can stably reach or exceed 40%, so as to meet the needs of high-efficiency heat insulation and cooling performance in the fields of building membrane structures, tents and military materials.
[0005] In the first aspect, the present application provides a near-infrared high-reflection PVC material adopts the following technical solution: A near-infrared high-reflection PVC material, characterized in that it comprises a base fabric layer and a PVC coating coated on both sides of the base fabric layer, wherein the raw materials for preparing the PVC coating include the following components in parts by weight: The IR pigment is BASF Sicopal Black L0095 modified with dioctyl phthalate and EO / PO block polyether.
[0006] By adopting the above technical scheme: BASF Sicopal Black L0095 IR pigment is treated with dioctyl phthalate and EO / PO block polyether (such as The modification of 500L1) effectively solves the common incompatibility problem between alkaline IR pigments and orthophthalic plasticizers. This modification not only promotes the uniform dispersion of pigments in the PVC system, but also enhances the binding force between pigments and substrates, thereby improving the overall stability and durability of the material; The optimized formula design, especially the introduction of modified IR pigments, has significantly improved the reflective performance of PVC materials in the near-infrared band. By precisely controlling the proportion of each component and the modification process, it is ensured that the reflectivity of the material can stably reach or exceed 40%. This is especially important for application scenarios that require efficient thermal insulation and cooling performance, such as building membrane structures, tents and military materials.
[0007] Analyze the possible reasons: As a common plasticizer, dioctyl phthalate (DOP) has a molecular structure similar to that of phthalate plasticizers such as diisononyl phthalate (DINP). Modification of IR pigments with DOP may help form a film on the surface of the pigment that is compatible with the plasticizer in the PVC system, thereby reducing the interfacial tension between the pigment and the plasticizer and improving the dispersibility and compatibility of the pigment in PVC. EO / PO block polyether (such as 500L1) As a surfactant or compatibilizer, its unique molecular structure can interact well with the pigment and other components in the PVC system. This modification may enhance the wettability of the pigment particle surface, promote the uniform dispersion of the pigment in the PVC matrix, reduce the agglomeration of the pigment particles, and improve the binding force between the pigment and the PVC substrate; The optimized formula design accurately controls the weight proportions of PVC paste resin, plasticizer, stabilizer, IR pigment, flame retardant and other additives, so that the components can work synergistically with each other to achieve the best performance balance.
[0008] Preferably, the modified preparation raw material of IR pigment comprises, by weight percentage: BASF Sicopal Black L0095 90-95% Dioctyl phthalate 4.5-9.0% EO / PO block polyether 0.5-1% And prepared by the following preparation method: Clean the mixing container and first add the predetermined amount of BASF Sicopal Black L0095 pigment and stir gently to ensure that the pigment is evenly spread on the bottom of the container; Then, dioctyl phthalate is gradually added, and low-speed stirring is performed while adding to avoid excessive dust or local agglomeration; after the pigment and plasticizer are preliminarily mixed, the EO / PO block polyether is slowly added to the mixing container, and ultrasonic high-speed stirring is performed to fully mix them; During or after the mixing process, take samples for infrared reflection performance testing to ensure that the requirements are met.
[0009] By adopting the above technical solution: not only the incompatibility problem between the pigment and the plasticizer is solved, but also the near-infrared reflection performance of the pigment is significantly improved, laying a solid foundation for the preparation of high-performance near-infrared high-reflection PVC materials.
[0010] Preferably, the EO / PO block polyether is 500L1.
[0011] By adopting the above technical solution: As a kind of EO / PO block polyether, 500L1 can effectively interact with PVC resin and other additives to promote the uniform dispersion of pigments in the PVC system, thereby avoiding the agglomeration and precipitation of pigment particles and improving the stability and dispersibility of the pigments. In addition, it can also enhance the interfacial bonding force between the pigment and the PVC substrate. It can form a thin film on the surface of the pigment particles, improve the interaction between the pigment and the PVC resin, make the pigment more firmly attached to the PVC substrate, and improve the adhesion and durability of the coating.
[0012] Preferably, the flame retardant is at least one of triphenyl phosphate and triisopropylphenyl phosphate.
[0013] By adopting the above technical solution: triphenyl phosphate and triisopropylphenyl phosphate can decompose at high temperature to produce phosphoric acid and other phosphorus-containing compounds, which can catalyze the carbonization process of PVC materials to form a dense carbonized layer covering the surface of the material. This carbonized layer can not only effectively isolate oxygen and heat, but also prevent the escape of combustible gases, thereby significantly improving the flame retardant properties of the PVC material; These two flame retardants have good compatibility with PVC resin and can be evenly dispersed in PVC materials, reducing the agglomeration and precipitation of flame retardant particles, ensuring the stable existence and continuous effect of flame retardants in the material, and further improving the flame retardant effect of the material; At the same time, compared with other types of flame retardants, triphenyl phosphate and triisopropylphenyl phosphate have less effect on the physical properties and processing properties of PVC materials. They will not significantly reduce the strength, toughness or processing fluidity of the material, so they can maintain the original excellent properties of PVC materials.
[0014] Preferably, the other additives include one or more of a binder, an anti-UV agent, and titanium dioxide.
[0015] By adopting the above technical solution: the comprehensive properties of PVC materials such as adhesion, weather resistance and aesthetics can be significantly improved. The addition of these additives enables PVC materials to have better practicality and market competitiveness while maintaining excellent near-infrared reflection performance.
[0016] In a second aspect, the present application provides a method for preparing a near-infrared high-reflection PVC material using the following technical solution: A method for preparing a near-infrared high-reflection PVC material, the preparation steps comprising: S1, preparation of base fabric layer: selecting polyester fiber as material, and knitting the base fabric layer through a biaxial warp knitting machine; S2, material coating: PVC paste resin, diisononyl phthalate, stabilizer, modified IR pigment, flame retardant and other additives are mixed in a certain proportion, and stirred evenly at an appropriate temperature to prepare a PVC coating slurry, and the prepared PVC coating slurry is evenly coated on both sides of the base fabric layer prepared in step S1 by dipping; S3, curing: the base fabric layer coated with the PVC coating is sent to a curing furnace for curing. After the curing is completed, the material is subjected to post-processing operations such as cutting and trimming.
[0017] By adopting the above technical solution, the prepared near-infrared high-reflection PVC material not only has excellent near-infrared reflection performance, but also has good physical properties, weather resistance and aesthetics. This material has a wide range of application prospects in the fields of tents, building membrane structures, military protection, etc., and can meet the needs of different fields for high-performance and high-safety materials.
[0018] Preferably, the porosity of the base fabric layer in step S1 is 10-12%.
[0019] By adopting the above technical solution: it is beneficial for the PVC coating slurry to better penetrate into the fiber gaps of the base fabric layer to form a more solid bond. This enhanced adhesion can not only improve the durability of the coating, but also prevent the coating from peeling off or cracking during use.
[0020] Preferably, the viscosity of the PVC coating slurry in step S2 is 4000-4500 mPa·s.
[0021] By adopting the above technical solution: the viscosity of 4000-4500mPa·s ensures that the PVC coating slurry can be evenly and smoothly covered on the base fabric layer during the coating process, avoiding the problem of too thick, too thin or uneven coating, which helps to improve the uniformity and aesthetics of the coating, while ensuring the thickness and performance of the coating.
[0022] Preferably, in step S3, the curing temperature is 160-180° C. and the curing time is 1-2 hours.
[0023] By adopting the above technical solution: under this curing condition, the PVC coating can form a dense and uniform structure with excellent physical properties, weather resistance and chemical stability. At the same time, since the pigments and other additives are fully dispersed and fixed during the curing process, the near-infrared reflection performance of the coating can also be well maintained and improved.
[0024] In summary, the present application includes at least one beneficial technical effect: 1. This application is to treat BASF Sicopal Black L0095 IR pigment with dioctyl phthalate and EO / PO block polyether (such as The modified treatment of 500L1) solves the incompatibility problem between pigment and plasticizer, promotes the uniform dispersion of pigment in PVC system, and significantly improves the near-infrared reflection performance of the material. The optimized formula design ensures that the reflectivity of the material can stably reach or exceed 40%, which is particularly important for application scenarios that require efficient heat insulation and cooling performance (such as architectural membrane structures, tents and military materials, etc.); 2. In addition to excellent near-infrared reflection performance, this application also significantly improves the adhesion, weather resistance and aesthetics of PVC materials by adding adhesives, anti-UV agents, titanium dioxide and other additives. The introduction of flame retardants (such as triphenyl phosphate and triisopropylphenyl phosphate) significantly improves the flame retardant properties of the material and ensures the safety of the material during use. These comprehensive performance improvements enable the PVC material to maintain high performance while also having better practicality and market competitiveness; 3. The preparation method provided in the present application ensures the uniformity, adhesion and durability of the coating by precisely controlling the porosity of the base fabric layer (10-12%), the viscosity of the PVC coating slurry (4000-4500 mPa·s), and the curing temperature and time (160-180°C, 1-2h). The optimization of these process parameters not only improves the production efficiency, but also ensures the quality and stability of the final product. At the same time, the process flow of dip coating and high-temperature curing enables the PVC coating to be firmly attached to the base fabric layer to form a composite material with excellent performance. DETAILED DESCRIPTION
[0025] The present application is further described in detail below in conjunction with the examples. Except for the special instructions below, the raw materials used in the present application are all common commercially available materials.
[0026] Preparation Example 1-2 An IR pigment, its preparation raw materials and corresponding dosage (kg) are shown in the following table.
[0027] Among them, EO / PO block polyether is 500L1; And prepared by the following preparation method: In a clean, dry mixing container, first add the predetermined amount of BASF Sicopal Black L0095 pigment and stir gently to ensure that the pigment is evenly spread on the bottom of the container. Then, gradually add dioctyl phthalate while stirring at a low speed to avoid excessive dust or local agglomeration. After the pigment and plasticizer are preliminarily mixed, slowly add the EO / PO block polyether into the mixing container. Since the amount of EO / PO block polyether added is small, special attention should be paid to its dispersion uniformity. Ultrasonic dispersion is used to fully mix the mixture for testing and adjustment. During or after the mixing process, samples are taken for performance testing of infrared reflectance to ensure that the quality meets the requirements.
[0028] Preparation Example 3 An IR pigment, the preparation method of which is the same as that of Preparation Example 1, except that HTK-6096 is used in equal amounts to replace 500L1.
[0029] Preparation Example 4 An IR pigment, the preparation method of which is the same as that of Preparation Example 1, except that KJ-1800 superdispersant is used in equal amounts to replace 500L1.
[0030] Example 1 A near-infrared high-reflection PVC material, its preparation raw materials and corresponding usage (kg) are shown in the following table.
[0031] Among them, other additives are composed of adhesives and anti-UV agents. The adhesive is Beep 6119, UV inhibitor UV-360; And it is prepared by the following preparation method: S1. Preparation of base fabric layer: Select polyester fiber as material, and knit the base fabric layer by a biaxial warp knitting machine, wherein the porosity of the base fabric layer is 10%; S2, material coating: PVC paste resin, diisononyl phthalate, stabilizer, IR pigment prepared in Preparation Example 1, flame retardant and other additives are mixed in a certain proportion, and stirred evenly at an appropriate temperature to prepare a PVC coating slurry, the viscosity of the PVC coating slurry is 4200 mPa·s, and the prepared PVC coating slurry is evenly coated on both sides of the base fabric layer prepared in step S1 by dipping, and the coating thickness of the upper and lower sides is 3 mm; S3, curing: the base fabric layer coated with the PVC coating is sent to a curing furnace for curing at 160° C. for 1.5 hours. After the curing is completed, the material is subjected to post-processing operations such as cutting and trimming.
[0032] Embodiment 2-6 A near-infrared high-reflection PVC material, the preparation method and raw materials used are the same as those in Example 1, the only difference is that the amount of each component raw material in the preparation raw material of the PVC coating is different, the specific situation is shown in the following table; Embodiment 7-9 A near-infrared high-reflection PVC material, the preparation method of which is the same as that of Example 1, the only difference being that the source of the IR pigment used in the preparation raw materials of the PVC coating is different, as shown in the following table for details: Group Source of IR pigments used Example 7 Prepared from Preparation Example 2 Example 8 Prepared from Preparation Example 3 Example 9 Prepared by Preparation Example 4 Example 10 A near-infrared high-reflection PVC material, the preparation method of which is the same as that of Example 1, except that other IR pigment BASF Sicotan Brown K2711 is additionally added to the PVC coating when the color matching is changed. The specific situation is shown in the following table: Embodiment 11 A near-infrared high-reflection PVC material, the preparation method of which is the same as that of Example 1, except that other common pigments BASF Sicotan Brown K2711 are additionally added to the PVC coating when changing the color matching, and the specific situation is shown in the following table: Comparative Example 1 A near-infrared high-reflection PVC material, the preparation method of which is the same as that of Example 1, except that the IR pigment used in the preparation raw materials of the PVC coating is not modified.
[0033] Performance Testing 1.Near infrared reflection test: The materials prepared in the embodiments and comparative examples were cut into 5 square samples of 3×3 cm in the same area, and the reflectivity in the range of 700-2500 nm was measured using a TEMP 2000A portable infrared emissivity / reflectivity meter, and the test results were averaged.
[0034] The performance test results are shown in the following table: By analyzing the data in the above table, it can be seen that the near-infrared high-reflection PVC materials prepared in Examples 1-6 can reach a reflectivity of more than 40% in the near-infrared wavelength range of 700-2500nm. It can be seen from Examples 2-3 that as the amount of diisononyl phthalate increases, the reflectivity also increases. However, from the data performance of Example 4, it can be seen that the more the amount, the better. It can be seen from Examples 5-6 that the reflectivity of the prepared material samples in the wavelength range of 700-2500nm increases with further increasing the content of IR pigments. As for the near-infrared high-reflection PVC materials prepared in Examples 7-9, except for Example 9, the reflectivity in the near-infrared range of 700-2500nm reached 40%, especially Example 7, which reached 49%, which can be used as a preferred example. In Example 9, the raw materials for the preparation of the modified IR pigment used KJ-1800 superdispersant to replace 500L1, its reflectivity is only 38%; 500L1 is an EO / PO block polyether dispersant, while KJ-1800 is a super dispersant. There may be differences between 500L1 and KJ-1800 in chemical structure, intermolecular forces, etc., which affect the dispersion uniformity and stability of IR pigments in the PVC system, and thus affect the reflective properties of the material; In addition to dispersibility, the interaction between modified IR pigments and PVC substrates is also an important factor affecting reflective performance. Different modifiers may change the properties of the pigment surface, thereby affecting its binding force and compatibility with the PVC substrate. KJ-1800 superdispersant may not be as 500L1 does not effectively enhance the bonding between the pigment and the PVC substrate, causing some pigments to fall off or migrate during processing or use, reducing the reflectivity.
[0035] In Examples 10 and 11, in order to change the color of the prepared near-infrared high-reflection PVC material, pigments of other colors are often mixed. In Example 10, the same infrared-reflecting IR pigment is used, while in Example 11, ordinary pigments are used for mixing and preparation. From the test results, the reflectivity of the near-infrared high-reflection PVC material in Example 11 is only 14%. It can be seen that the infrared-reflecting IR pigment will lose its infrared reflection function after being mixed with ordinary pigments, so the color matching must all use infrared-reflecting IR pigments; In comparative experiment 1, we used an unmodified IR pigment as one of the raw materials for preparing near-infrared high-reflection PVC material. The experimental results showed that the reflectivity of the near-infrared high-reflection PVC material prepared in this way was only 22%, which was significantly lower than expected, and verified the obvious incompatibility problem between infrared reflective IR pigments and ortho-phthalic plasticizers.
[0036] 2. Flame retardancy test: In the flame retardancy test, the test was carried out according to GB / T 5455-1997 standard.
[0037] The specific test results are shown in the table below.
[0038] Through the data analysis of the above table, it can be seen that the near-infrared high-reflection PVC materials prepared in Examples 1 to 11 and Comparative Example 1 all showed excellent performance in the flame retardant performance test and successfully reached the B1 flame retardant grade standard.
[0039] The above are all modifications without creative contribution or solutions that obviously constitute technical inspiration that can be made to the present embodiment as needed by technical personnel in this field after reading this specification, but they should be protected by patent law as long as they are within the scope of the claims of this application.
Claims
1. A near-infrared high-reflection PVC material, characterized in that: It comprises a base fabric layer and a PVC coating coated on both sides of the base fabric layer, wherein the raw materials for preparing the PVC coating include the following components in parts by weight: PVC paste resin 95 parts 45-65 parts of diisononyl phthalate 1-2 parts of stabilizer IR pigment 25-40 parts Flame retardant 3-4 parts 1-2 parts of other additives; The IR pigment is BASF Sicopal Black L0095 modified with dioctyl phthalate and EO / PO block polyether.
2. The near-infrared high-reflection PVC material according to claim 1, characterized in that: The modified preparation raw materials of the IR pigment include, by weight percentage: BASF Sicopal Black L0095 90-95% Dioctyl phthalate 4.5-9.0% EO / PO block polyether 0.5-1% And prepared by the following preparation method: Clean the mixing container and first add the predetermined amount of BASF Sicopal Black L0095 pigment and stir gently to ensure that the pigment is evenly spread on the bottom of the container; Then gradually add dioctyl phthalate, stirring at a low speed to avoid excessive dust or local agglomeration; After the pigment and plasticizer are preliminarily mixed evenly, the EO / PO block polyether is slowly added into the mixing container and stirred at high speed by ultrasonication to make them fully mixed; During or after the mixing process, take samples for infrared reflection performance testing to ensure that the requirements are met.
3. The near-infrared high-reflection PVC material according to claim 1 or 2, characterized in that: The EO / PO block polyether is FTRT®500L1.
4. The near-infrared high-reflection PVC material according to claim 1, characterized in that: The flame retardant is at least one of triphenyl phosphate and triisopropylphenyl phosphate.
5. The near-infrared high-reflection PVC material according to claim 1, characterized in that: The other additives include one or more of a binder, an anti-UV agent, and titanium dioxide.
6. A method for preparing a near-infrared high-reflection PVC material, characterized in that: The preparation steps include: S1, preparation of base fabric layer: selecting polyester fiber as material, and knitting the base fabric layer through a biaxial warp knitting machine; S2, material coating: PVC paste resin, diisononyl phthalate, stabilizer, modified IR pigment, flame retardant and other additives are mixed in a certain proportion, and stirred evenly at an appropriate temperature to prepare a PVC coating slurry, and the prepared PVC coating slurry is evenly coated on both sides of the base fabric layer prepared in step S1 by dipping; S3, curing: the base fabric layer coated with the PVC coating is sent to a curing furnace for curing. After the curing is completed, the material is subjected to post-processing operations such as cutting and trimming.
7. The method for preparing the near-infrared high-reflection PVC material according to claim 6, characterized in that: The porosity of the base fabric layer in step S1 is 10-12%.
8. The method for preparing the near-infrared high-reflection PVC material according to claim 6, characterized in that: The viscosity of the PVC coating slurry in step S2 is 4000-4500 mPa·s.
9. The method for preparing the near-infrared high-reflection PVC material according to claim 6, characterized in that: In step S3, the curing temperature is 160-180° C. and the curing time is 1-2 hours.
Citation Information
Patent Citations
Infrared-reflective paint and infrared-reflective resin composition
CN102575128A
Infrared reflective material and membrane prepared therefrom
CN103408863A
Heat reflection artificial leather
CN107237163A
Infrared fluorescent coatings
CN108699362A
Infrared reflective PVC artificial leather
CN112626877A
Cited By
Preparation process and preparation device of high-elasticity fireproof flame-retardant fabric
CN119465662A
Silane-crosslinked halogen-free low-smoke flame-retardant polyolefin electronic wire material, preparation method and application
CN120118418A
Near-infrared highly-reflective PVC material and preparation method therefor
WO2026040395A1