Preparation process of high-water-absorption breathable tissue base paper material

Through the combination of needle wood pulp fiber, broadleaf wood pulp fiber, viscose fiber and polyester fiber, combined with additives and multi-layer composite technology, the problem of insufficient water absorption and breathability of traditional paper towels is solved, and the water absorption of paper is improved. Breathability and strength, suitable for a variety of usage scenarios.

CN118910925APending Publication Date: 2024-11-08ZHEJIANG ZHENGHUA PAPER CO LTD

Patent Information

Application Number
CN202410999270.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional tissues have limited water absorption speed and water absorption, poor breathability, and are low in wet and dry states, making them prone to rupture.

Method used

Using the combination of needle wood pulp fiber, broadleaf wood pulp fiber, viscose fiber and polyester fiber, it is used to add polyamide epoxy chloride resin, carboxymethyl cellulose, glycerol and other additives, beat treatment and multi-layer composite technology. Improves the water absorption and breathability of the paper, and enhances the strength of the paper through calendering and drying processes.

Benefits of technology

It achieves high water absorption and breathability of the paper, enhances the wet and dry strength and tear resistance of the paper, is suitable for sensitive skin and infants, and improves the softness and feel of the paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910925A_ABST
    Figure CN118910925A_ABST
Patent Text Reader

Abstract

The invention relates to the field of tissue preparation, and discloses a preparation process of a high-water-absorption breathable tissue base paper material, which comprises the following specific steps: S1, fiber raw material selection: selecting softwood pulp fibers as long fibers, selecting hardwood pulp fibers as short fibers, selecting viscose fibers as regenerated cellulose fibers, and selecting polyester fibers as synthetic fibers; s2, chemical auxiliary agent selection: polyamide epichlorohydrin resin (PAE) is selected as a wet strength agent, diethanol amine (DEA) is selected as a softening agent, carboxymethyl cellulose (CMC) or polyvinyl alcohol (PVA) is selected as a water absorbent, and glycerol is selected as a humectant; s4, forming; S5, dehydrating; S6, drying; S7, calendaring; by adding the water absorbent (CMC or PVA), the water absorption capacity of the paper is improved, more liquid can be rapidly absorbed, the paper has air permeability through fiber combination and process control, dryness and dryness can be easily kept, moisture retention is prevented, and therefore the effect of enhancing the water absorption capacity and air permeability of the tissue can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paper towel preparation, and in particular to a preparation process of a high water-absorbent and breathable paper towel base material. Background Art

[0002] In modern life, paper towels have become an indispensable item in people's daily life. Paper towels have a wide range of uses, including but not limited to personal hygiene, household cleaning, industrial wiping, etc. As people's quality of life improves, the performance requirements for paper towels are getting higher and higher, especially in terms of water absorbency, air permeability and strength.

[0003] Traditional paper towels are usually made of a single wood pulp fiber. Although the production process is simple and the cost is low, their performance is insufficient. The water absorption speed and amount of traditional paper towels are limited. They cannot absorb liquid quickly and easily, which easily leads to waste. The fiber structure of traditional paper towels is tight and the air permeability is poor. They are easy to feel damp and uncomfortable when used. Traditional paper towels have low strength in dry and wet states and are easy to break, especially when used in a wet state. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a process for preparing a highly water-absorbent and breathable paper towel base material, which solves the problems of limited water absorption speed and water absorption amount and poor air permeability of traditional paper towels.

[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: A preparation process of a highly water-absorbent and breathable tissue base paper material, comprising the following specific steps:

[0006] S1: Fiber raw material selection: long fiber should choose coniferous wood pulp fiber, short fiber should choose hardwood pulp fiber, regenerated cellulose fiber should choose viscose fiber, and synthetic fiber should choose polyester fiber;

[0007] S2: Selection of chemical additives: wet strength agent: polyamide epichlorohydrin resin PAE, softener: diethanolamine DEA, water absorbent: carboxymethyl cellulose CMC or polyvinyl alcohol PVA, humectant: glycerol;

[0008] S3: pulp preparation, the selected fiber raw materials are pulped by a pulping machine, and during the pulping process, wet strength agent, softener, water absorbent and moisturizer are gradually added;

[0009] S4: Forming, diluting the slurry to an appropriate concentration and evenly distributing it on the forming wire through a paper machine;

[0010] S5: Dehydration, using a vacuum suction box to remove part of the water in the pulp, and then using a press to further remove the water in the paper sheet;

[0011] S6: Drying: Use a multi-cylinder dryer to dry the paper, gradually increase the temperature, and use hot air drying equipment to further remove moisture from the paper;

[0012] S7: calendering, calendering the dried paper through a calender, controlling the calendering temperature and pressure;

[0013] S8: Winding, rolling the processed paper into a roll.

[0014] Preferably, in step S1, coniferous wood pulp fibers account for 50%-70% of the total fiber weight, hardwood pulp fibers account for 20%-30% of the total fiber weight, viscose fibers account for 5%-10% of the total fiber weight, and polyester fibers account for 5%-10% of the total fiber weight.

[0015] Preferably, in step S2, polyamide epichlorohydrin resin (PAE) accounts for 0.5%-1% of the fiber weight, diethanolamine (DEA) accounts for 0.2%-0.5% of the fiber weight, carboxymethyl cellulose (CMC) or polyvinyl alcohol (PVA) accounts for 0.5%-1% of the fiber weight, and glycerol accounts for 0.2%-0.5% of the fiber weight.

[0016] Preferably, in the step S3, the pulping concentration is 3%-5%, and the pulping time is 30-60 minutes, in the step S4, the pulp dilution concentration is 0.5%-1%, in the step S5, the vacuum degree of vacuum dehydration is maintained at 30-50kPa, and the pressing pressure is set to 50-70kN / m, in the step S6, the initial drying temperature of the multi-cylinder drying is 90°C, the final drying temperature is 120°C, and hot air drying is used in combination to ensure that the final moisture content is 5%-8%, and in the step S7, the calendering temperature is set to 80-100°C, and the calendering pressure is set to 50-70kN / m.

[0017] Preferably, after step S5, a paper towel surface treatment is added, a coating liquid is selected as polyvinyl alcohol (PVA) or polyacrylate, a coating machine is used to evenly coat the coating liquid on the paper surface, the coated paper is dried by a drying device, a sizing liquid is prepared using starch and carboxymethyl cellulose (CMC), the sizing liquid is evenly applied to the paper surface by a sizing device, and the sizing paper is dried by a drying device.

[0018] Preferably, the polyvinyl alcohol (PVA) is 2%-5%, the polyacrylate is 1%-3%, the water is 92%-97%, the coating speed of the coating machine is 30-60 m / min, and the coating amount is 5-10 g / m 2 , starch is 3%-7%, carboxymethyl cellulose CMC is 0.5%-1.5%, water is 91.5%-96.5%, the sizing equipment sizing speed is 20-50m / min, and the sizing amount is 3-7g / m 2.

[0019] Preferably, after the S3 step or when the paper towel surface is treated, fragrance or functional additives are added, lavender essential oil or lemon essence is selected, and the fragrance is evenly added to the pulp or coated on the surface of the paper, and aloe extract or vitamin E additive is selected, and the functional additive is evenly added to the pulp or coated on the surface of the paper.

[0020] Preferably, the lavender essential oil is 0.1%-0.3%, the lemon essence is 0.1%-0.3%, the added amount of lavender essential oil or lemon essence is 0.2%-0.6%, the aloe extract is 0.2%-0.5%, the vitamin E is 0.1%-0.3%, and the added amount of aloe extract or vitamin E is 0.2%-0.5%.

[0021] Preferably, after the step S8, a multi-layer composite technology is added, and highly absorbent ingredients - polyvinyl alcohol PVA and carboxymethyl cellulose CMC are added to the inner layer fiber formula, and softeners and reinforcing agents, diethanolamine DEA and polyester fibers are added to the outer layer fiber formula, and the inner layer and the outer layer are combined together through a composite process.

[0022] Preferably, the polyvinyl alcohol (PVA) is 0.5%-1.0%, the carboxymethyl cellulose (CMC) is 0.5%-1.0%, and the wood pulp fiber is 98%-99%.

[0023] The present invention provides a preparation process of a highly water-absorbent and breathable tissue base paper material, which has the following beneficial effects:

[0024] 1. The present invention improves the water absorption capacity of paper by adding a water absorbent (CMC or PVA), which can quickly absorb more liquid. The fiber combination and process control make the paper have higher air permeability, which helps to keep dry and prevent moisture retention, thereby achieving the effect of enhancing the water absorption capacity and air permeability of the paper towel.

[0025] 2. The present invention improves the overall strength of the paper, especially the strength in dry and wet states, through the outer layer material in the multi-layer structure, such as polyester fiber. The sizing treatment in the surface treatment increases the tear resistance and tensile strength of the paper, further improving the durability of the paper, thereby achieving the effect of making the paper towel not easy to break during use.

[0026] 3. The present invention uses functional additives, such as aloe vera extract or vitamin E, to give the paper towel skin care and moisturizing functions, thereby achieving an effect suitable for people with sensitive skin and infants.

[0027] 4. The present invention uses a softener (such as DEA) and a coating process in the surface treatment to make the paper surface smoother and softer, making it more comfortable to use, thereby achieving the effect of increasing the softness and improving the feel of the paper towel. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a flow chart of the preparation process of the highly water-absorbent and breathable tissue base paper material. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] Please refer to the attached Figure 1 The embodiment of the present invention provides a preparation process of a highly water-absorbent and breathable tissue base paper material, comprising the following specific steps:

[0032] S1: Fiber raw material selection: long fiber should choose coniferous wood pulp fiber, short fiber should choose hardwood pulp fiber, regenerated cellulose fiber should choose viscose fiber, and synthetic fiber should choose polyester fiber;

[0033] S2: Selection of chemical additives: wet strength agent: polyamide epichlorohydrin resin PAE, softener: diethanolamine DEA, water absorbent: carboxymethyl cellulose CMC or polyvinyl alcohol PVA, humectant: glycerol;

[0034] S3: Slurry preparation, the selected fiber raw materials are pulped through a pulping machine to ensure the fiber is refined and properly cut. During the pulping process, wet strength agent, softener, water absorbent and moisturizer are gradually added to ensure that the additives are evenly distributed in the slurry;

[0035] S4: Forming, diluting the slurry to an appropriate concentration and evenly distributing it on the forming wire through a paper machine;

[0036] S5: Dehydration, remove part of the water in the pulp through a vacuum suction box, maintain a moderate vacuum degree, and then use a press to further remove the water in the paper to ensure the initial drying of the paper;

[0037] S6: Drying: Use a multi-cylinder dryer to dry the paper, gradually increase the temperature to avoid shrinkage and deformation of the paper, and use hot air drying equipment to further remove moisture from the paper to ensure that the final moisture content is controlled within an appropriate range;

[0038] S7: calendering, calendering the dried paper through a calender, controlling the calendering temperature and pressure;

[0039] S8: Winding, rolling the processed paper into a roll.

[0040] In step S1, the coniferous wood pulp fiber accounts for 60% of the total fiber weight, the hardwood pulp fiber accounts for 25% of the total fiber weight, the viscose fiber accounts for 10% of the total fiber weight, and the polyester fiber accounts for 5% of the total fiber weight.

[0041] In step S2, polyamide epichlorohydrin resin PAE accounts for 0.8% of the fiber weight, diethanolamine DEA accounts for 0.3% of the fiber weight, carboxymethyl cellulose CMC or polyvinyl alcohol PVA accounts for 0.8% of the fiber weight, and glycerol accounts for 0.3% of the fiber weight.

[0042] In step S3, the pulping concentration is 4% and the pulping time is 45 minutes. In step S4, the pulp dilution concentration is 0.8%. In step S5, the vacuum degree of vacuum dehydration is maintained at 40 kPa and the pressing pressure is set to 60 kN / m. In step S6, the initial drying temperature of multi-cylinder drying is 90°C and the final drying temperature is 120°C. Hot air drying is used in combination to ensure that the final moisture content is 6%. In step S7, the calendering temperature is set to 90°C and the calendering pressure is set to 60 kN / m.

[0043] After step S5, the surface treatment of the paper towel is added, the coating liquid is selected as polyvinyl alcohol PVA or polyacrylate, the coating liquid is evenly coated on the surface of the paper by a coating machine, the coated paper is dried by a drying device, a sizing liquid is prepared using starch and carboxymethyl cellulose CMC, the sizing liquid is evenly applied on the surface of the paper by a sizing device, and the sizing paper is dried by a drying device.

[0044] Polyvinyl alcohol PVA is 2%-5%, polyacrylate is 1%-3%, water is 92%-97%, the coating speed of the coating machine is 30-60m / min, and the coating amount is 5-10g / m 2 , starch is 3%-7%, carboxymethyl cellulose CMC is 0.5%-1.5%, water is 91.5%-96.5%, the sizing equipment sizing speed is 20-50m / min, and the sizing amount is 3-7g / m 2 ;

[0045] Specifically, the above addition amounts are all mass fractions.

[0046] After step S3 or when the paper towel surface is treated, fragrance or functional additives are added. Lavender essential oil or lemon essence is selected and the fragrance is evenly added to the pulp or applied on the surface of the paper. Aloe extract or vitamin E additive is selected and the functional additive is evenly added to the pulp or applied on the surface of the paper.

[0047] Lavender essential oil is 0.1% - 0.3%, lemon essence is 0.1% - 0.3%, the added amount of lavender essential oil or lemon essence is 0.2% - 0.6%, aloe extract is 0.2% - 0.5%, vitamin E is 0.1% - 0.3%, and the added amount of aloe extract or vitamin E is 0.2% - 0.5%;

[0048] Specifically, the above addition amounts are all mass fractions.

[0049] After step S8, multi-layer composite technology is added. Highly absorbent ingredients - polyvinyl alcohol (PVA) and carboxymethyl cellulose (CMC) are added to the inner fiber formula. Softeners and reinforcing agents - diethanolamine (DEA) and polyester fiber are added to the outer fiber formula. The inner and outer layers are combined together through a composite process.

[0050] Polyvinyl alcohol PVA is 0.5%-1.0%, carboxymethyl cellulose CMC is 0.5%-1.0%, and wood pulp fiber is 98%-99%;

[0051] Specifically, the above addition amounts are all mass fractions.

[0052] Embodiment 2:

[0053] Please refer to the attached Figure 1 The embodiment of the present invention provides a preparation process of a highly water-absorbent and breathable tissue base paper material, comprising the following specific steps:

[0054] S1: Fiber raw material selection: long fiber should choose coniferous wood pulp fiber, short fiber should choose hardwood pulp fiber, regenerated cellulose fiber should choose viscose fiber, and synthetic fiber should choose polyester fiber;

[0055] S2: Selection of chemical additives: wet strength agent: polyamide epichlorohydrin resin PAE, softener: diethanolamine DEA, water absorbent: carboxymethyl cellulose CMC or polyvinyl alcohol PVA, humectant: glycerol;

[0056] S3: Slurry preparation, the selected fiber raw materials are pulped through a pulping machine to ensure the fiber is refined and properly cut. During the pulping process, wet strength agent, softener, water absorbent and moisturizer are gradually added to ensure that the additives are evenly distributed in the slurry;

[0057] S4: Forming, diluting the slurry to an appropriate concentration and evenly distributing it on the forming wire through a paper machine;

[0058] S5: Dehydration, remove part of the water in the pulp through a vacuum suction box, maintain a moderate vacuum degree, and then use a press to further remove the water in the paper to ensure the initial drying of the paper;

[0059] S6: Drying: Use a multi-cylinder dryer to dry the paper, gradually increase the temperature to avoid shrinkage and deformation of the paper, and use hot air drying equipment to further remove moisture from the paper to ensure that the final moisture content is controlled within an appropriate range;

[0060] S7: calendering, calendering the dried paper through a calender, controlling the calendering temperature and pressure;

[0061] S8: Winding, rolling the processed paper into a roll.

[0062] In step S1, the coniferous wood pulp fiber accounts for 55% of the total fiber weight, the hardwood pulp fiber accounts for 30% of the total fiber weight, the viscose fiber accounts for 10% of the total fiber weight, and the polyester fiber accounts for 5% of the total fiber weight.

[0063] In step S2, polyamide epichlorohydrin resin PAE accounts for 0.7% of the fiber weight, diethanolamine DEA accounts for 0.4% of the fiber weight, carboxymethyl cellulose CMC or polyvinyl alcohol PVA accounts for 0.7% of the fiber weight, and glycerol accounts for 0.4% of the fiber weight.

[0064] In step S3, the pulping concentration is 3.5% and the pulping time is 50 minutes. In step S4, the pulp dilution concentration is 0.7%. In step S5, the vacuum degree of vacuum dehydration is maintained at 35 kPa and the pressing pressure is set to 65 kN / m. In step S6, the initial drying temperature of multi-cylinder drying is 95°C and the final drying temperature is 115°C. Hot air drying is used in combination to ensure that the final moisture content is 7%. In step S7, the calendering temperature is set to 85°C and the calendering pressure is set to 65 kN / m.

[0065] After step S5, the surface treatment of the paper towel is added, the coating liquid is selected as polyvinyl alcohol PVA or polyacrylate, the coating liquid is evenly coated on the surface of the paper by a coating machine, the coated paper is dried by a drying device, a sizing liquid is prepared using starch and carboxymethyl cellulose CMC, the sizing liquid is evenly applied on the surface of the paper by a sizing device, and the sizing paper is dried by a drying device.

[0066] Polyvinyl alcohol PVA is 2%-5%, polyacrylate is 1%-3%, water is 92%-97%, the coating speed of the coating machine is 30-60m / min, and the coating amount is 5-10g / m 2 , starch is 3%-7%, carboxymethyl cellulose CMC is 0.5%-1.5%, water is 91.5%-96.5%, the sizing equipment sizing speed is 20-50m / min, and the sizing amount is 3-7g / m 2 ;

[0067] Specifically, the above addition amounts are all mass fractions.

[0068] After step S3 or when the paper towel surface is treated, fragrance or functional additives are added. Lavender essential oil or lemon essence is selected and the fragrance is evenly added to the pulp or applied on the surface of the paper. Aloe extract or vitamin E additive is selected and the functional additive is evenly added to the pulp or applied on the surface of the paper.

[0069] Lavender essential oil is 0.1% - 0.3%, lemon essence is 0.1% - 0.3%, the added amount of lavender essential oil or lemon essence is 0.2% - 0.6%, aloe extract is 0.2% - 0.5%, vitamin E is 0.1% - 0.3%, and the added amount of aloe extract or vitamin E is 0.2% - 0.5%;

[0070] Specifically, the above addition amounts are all mass fractions.

[0071] After step S8, multi-layer composite technology is added. Highly absorbent ingredients - polyvinyl alcohol (PVA) and carboxymethyl cellulose (CMC) are added to the inner fiber formula. Softeners and reinforcing agents - diethanolamine (DEA) and polyester fiber are added to the outer fiber formula. The inner and outer layers are combined together through a composite process.

[0072] Polyvinyl alcohol PVA is 0.5%-1.0%, carboxymethyl cellulose CMC is 0.5%-1.0%, and wood pulp fiber is 98%-99%;

[0073] Specifically, the above addition amounts are all mass fractions.

[0074] Embodiment three:

[0075] Please refer to the attached Figure 1 The embodiment of the present invention provides a preparation process of a highly water-absorbent and breathable tissue base paper material, comprising the following specific steps:

[0076] S1: Fiber raw material selection: long fiber should choose coniferous wood pulp fiber, short fiber should choose hardwood pulp fiber, regenerated cellulose fiber should choose viscose fiber, and synthetic fiber should choose polyester fiber;

[0077] S2: Selection of chemical additives: wet strength agent: polyamide epichlorohydrin resin PAE, softener: diethanolamine DEA, water absorbent: carboxymethyl cellulose CMC or polyvinyl alcohol PVA, humectant: glycerol;

[0078] S3: Slurry preparation, the selected fiber raw materials are pulped through a pulping machine to ensure the fiber is refined and properly cut. During the pulping process, wet strength agent, softener, water absorbent and moisturizer are gradually added to ensure that the additives are evenly distributed in the slurry;

[0079] S4: Forming, diluting the slurry to an appropriate concentration and evenly distributing it on the forming wire through a paper machine;

[0080] S5: Dehydration, remove part of the water in the pulp through a vacuum suction box, maintain a moderate vacuum degree, and then use a press to further remove the water in the paper to ensure the initial drying of the paper;

[0081] S6: Drying: Use a multi-cylinder dryer to dry the paper, gradually increase the temperature to avoid shrinkage and deformation of the paper, and use hot air drying equipment to further remove moisture from the paper to ensure that the final moisture content is controlled within an appropriate range;

[0082] S7: calendering, calendering the dried paper through a calender, controlling the calendering temperature and pressure;

[0083] S8: Winding, rolling the processed paper into a roll.

[0084] In step S1, the coniferous wood pulp fiber accounts for 50% of the total fiber weight, the hardwood pulp fiber accounts for 35% of the total fiber weight, the viscose fiber accounts for 10% of the total fiber weight, and the polyester fiber accounts for 5% of the total fiber weight.

[0085] In step S2, polyamide epichlorohydrin resin PAE accounts for 0.9% of the fiber weight, diethanolamine DEA accounts for 0.2% of the fiber weight, carboxymethyl cellulose CMC or polyvinyl alcohol PVA accounts for 0.9% of the fiber weight, and glycerol accounts for 0.2% of the fiber weight.

[0086] In step S3, the pulping concentration is 4.5% and the pulping time is 40 minutes. In step S4, the pulp dilution concentration is 0.9%. In step S5, the vacuum degree of vacuum dehydration is maintained at 45 kPa and the pressing pressure is set to 55 kN / m. In step S6, the initial drying temperature of multi-cylinder drying is 85°C and the final drying temperature is 125°C. Hot air drying is used in combination to ensure that the final moisture content is 5%. In step S7, the calendering temperature is set to 80°C and the calendering pressure is set to 55 kN / m.

[0087] After step S5, the surface treatment of the paper towel is added, the coating liquid is selected as polyvinyl alcohol PVA or polyacrylate, the coating liquid is evenly coated on the surface of the paper by a coating machine, the coated paper is dried by a drying device, a sizing liquid is prepared using starch and carboxymethyl cellulose CMC, the sizing liquid is evenly applied on the surface of the paper by a sizing device, and the sizing paper is dried by a drying device.

[0088] Polyvinyl alcohol PVA is 2%-5%, polyacrylate is 1%-3%, water is 92%-97%, the coating speed of the coating machine is 30-60m / min, and the coating amount is 5-10g / m 2, starch is 3%-7%, carboxymethyl cellulose CMC is 0.5%-1.5%, water is 91.5%-96.5%, the sizing equipment sizing speed is 20-50m / min, and the sizing amount is 3-7g / m 2 ;

[0089] Specifically, the above addition amounts are all mass fractions.

[0090] After step S3 or when the paper towel surface is treated, fragrance or functional additives are added. Lavender essential oil or lemon essence is selected and the fragrance is evenly added to the pulp or applied on the surface of the paper. Aloe extract or vitamin E additive is selected and the functional additive is evenly added to the pulp or applied on the surface of the paper.

[0091] Lavender essential oil is 0.1% - 0.3%, lemon essence is 0.1% - 0.3%, the added amount of lavender essential oil or lemon essence is 0.2% - 0.6%, aloe extract is 0.2% - 0.5%, vitamin E is 0.1% - 0.3%, and the added amount of aloe extract or vitamin E is 0.2% - 0.5%;

[0092] Specifically, the above addition amounts are all mass fractions.

[0093] After step S8, multi-layer composite technology is added. Highly absorbent ingredients - polyvinyl alcohol (PVA) and carboxymethyl cellulose (CMC) are added to the inner fiber formula. Softeners and reinforcing agents - diethanolamine (DEA) and polyester fiber are added to the outer fiber formula. The inner and outer layers are combined together through a composite process.

[0094] Polyvinyl alcohol PVA is 0.5%-1.0%, carboxymethyl cellulose CMC is 0.5%-1.0%, and wood pulp fiber is 98%-99%;

[0095] Specifically, the above addition amounts are all mass fractions.

[0096] Embodiment 4:

[0097] Please refer to the attached Figure 1 The embodiment of the present invention provides a preparation process of a highly water-absorbent and breathable tissue base paper material, comprising the following specific steps:

[0098] S1: Fiber raw material selection: long fiber should choose coniferous wood pulp fiber, short fiber should choose hardwood pulp fiber, regenerated cellulose fiber should choose viscose fiber, and synthetic fiber should choose polyester fiber;

[0099] S2: Selection of chemical additives: wet strength agent: polyamide epichlorohydrin resin PAE, softener: diethanolamine DEA, water absorbent: carboxymethyl cellulose CMC or polyvinyl alcohol PVA, humectant: glycerol;

[0100] S3: Slurry preparation, the selected fiber raw materials are pulped through a pulping machine to ensure the fiber is refined and properly cut. During the pulping process, wet strength agent, softener, water absorbent and moisturizer are gradually added to ensure that the additives are evenly distributed in the slurry;

[0101] S4: Forming, diluting the slurry to an appropriate concentration and evenly distributing it on the forming wire through a paper machine;

[0102] S5: Dehydration, remove part of the water in the pulp through a vacuum suction box, maintain a moderate vacuum degree, and then use a press to further remove the water in the paper to ensure the initial drying of the paper;

[0103] S6: Drying: Use a multi-cylinder dryer to dry the paper, gradually increase the temperature to avoid shrinkage and deformation of the paper, and use hot air drying equipment to further remove moisture from the paper to ensure that the final moisture content is controlled within an appropriate range;

[0104] S7: calendering, calendering the dried paper through a calender, controlling the calendering temperature and pressure;

[0105] S8: Winding, rolling the processed paper into a roll.

[0106] In step S1, the coniferous wood pulp fiber accounts for 65% of the total fiber weight, the hardwood pulp fiber accounts for 20% of the total fiber weight, the viscose fiber accounts for 10% of the total fiber weight, and the polyester fiber accounts for 5% of the total fiber weight.

[0107] In step S2, polyamide epichlorohydrin resin PAE accounts for 1% of the fiber weight, diethanolamine DEA accounts for 0.4% of the fiber weight, carboxymethyl cellulose CMC or polyvinyl alcohol PVA accounts for 1% of the fiber weight, and glycerol accounts for 0.3% of the fiber weight.

[0108] In step S3, the pulping concentration is 4.5%, and the pulping time is 35 minutes. In step S4, the pulp dilution concentration is 0.7%. In step S5, the vacuum degree of vacuum dehydration is maintained at 40 kPa, and the pressing pressure is set to 70 kN / m. In step S6, the initial drying temperature of multi-cylinder drying is 90°C, and the final drying temperature is 130°C. Hot air drying is used in combination to ensure that the final moisture content is 6%. In step S7, the calendering temperature is set to 95°C, and the calendering pressure is set to 60 kN / m.

[0109] After step S5, the surface treatment of the paper towel is added, the coating liquid is selected as polyvinyl alcohol PVA or polyacrylate, the coating liquid is evenly coated on the surface of the paper by a coating machine, the coated paper is dried by a drying device, a sizing liquid is prepared using starch and carboxymethyl cellulose CMC, the sizing liquid is evenly applied on the surface of the paper by a sizing device, and the sizing paper is dried by a drying device.

[0110] Polyvinyl alcohol PVA is 2%-5%, polyacrylate is 1%-3%, water is 92%-97%, the coating speed of the coating machine is 30-60m / min, and the coating amount is 5-10g / m 2 , starch is 3%-7%, carboxymethyl cellulose CMC is 0.5%-1.5%, water is 91.5%-96.5%, the sizing equipment sizing speed is 20-50m / min, and the sizing amount is 3-7g / m 2 ;

[0111] Specifically, the above addition amounts are all mass fractions.

[0112] After step S3 or when the paper towel surface is treated, fragrance or functional additives are added. Lavender essential oil or lemon essence is selected and the fragrance is evenly added to the pulp or applied on the surface of the paper. Aloe extract or vitamin E additive is selected and the functional additive is evenly added to the pulp or applied on the surface of the paper.

[0113] Lavender essential oil is 0.1% - 0.3%, lemon essence is 0.1% - 0.3%, the added amount of lavender essential oil or lemon essence is 0.2% - 0.6%, aloe extract is 0.2% - 0.5%, vitamin E is 0.1% - 0.3%, and the added amount of aloe extract or vitamin E is 0.2% - 0.5%;

[0114] Specifically, the above addition amounts are all mass fractions.

[0115] After step S8, multi-layer composite technology is added. Highly absorbent ingredients - polyvinyl alcohol (PVA) and carboxymethyl cellulose (CMC) are added to the inner fiber formula. Softeners and reinforcing agents - diethanolamine (DEA) and polyester fiber are added to the outer fiber formula. The inner and outer layers are combined together through a composite process.

[0116] Polyvinyl alcohol PVA is 0.5%-1.0%, carboxymethyl cellulose CMC is 0.5%-1.0%, and wood pulp fiber is 98%-99%;

[0117] Specifically, the above addition amounts are all mass fractions.

[0118] Table 1: Properties of high absorbent and breathable tissue paper materials

[0119]

[0120] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing a highly water-absorbent and breathable tissue base paper material, characterized in that: The specific steps include: S1: Fiber raw material selection: long fiber should choose coniferous wood pulp fiber, short fiber should choose hardwood pulp fiber, regenerated cellulose fiber should choose viscose fiber, and synthetic fiber should choose polyester fiber; S2: Selection of chemical additives: wet strength agent: polyamide epichlorohydrin resin PAE, softener: diethanolamine DEA, water absorbent: carboxymethyl cellulose CMC or polyvinyl alcohol PVA, humectant: glycerol; S3: pulp preparation, the selected fiber raw materials are pulped by a pulping machine, and during the pulping process, wet strength agent, softener, water absorbent and moisturizer are gradually added; S4: Forming, diluting the slurry to an appropriate concentration and evenly distributing it on the forming wire through a paper machine; S5: Dehydration, using a vacuum suction box to remove part of the water in the pulp, and then using a press to further remove the water in the paper sheet; S6: Drying: Use a multi-cylinder dryer to dry the paper, gradually increase the temperature, and use hot air drying equipment to further remove moisture from the paper; S7: calendering, calendering the dried paper through a calender, controlling the calendering temperature and pressure; S8: Winding, rolling the processed paper into a roll.

2. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 1, characterized in that: In the step S1, the coniferous wood pulp fibers account for 50%-70% of the total fiber weight, the hardwood pulp fibers account for 20%-30% of the total fiber weight, the viscose fibers account for 5%-10% of the total fiber weight, and the polyester fibers account for 5%-10% of the total fiber weight.

3. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 1, characterized in that: In the step S2, polyamide epichlorohydrin resin PAE accounts for 0.5%-1% of the fiber weight, diethanolamine DEA accounts for 0.2%-0.5% of the fiber weight, carboxymethyl cellulose CMC or polyvinyl alcohol PVA accounts for 0.5%-1% of the fiber weight, and glycerol accounts for 0.2%-0.5% of the fiber weight.

4. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 1, characterized in that: In the step S3, the pulping concentration is 3%-5%, and the pulping time is 30-60 minutes. In the step S4, the pulp dilution concentration is 0.5%-1%. In the step S5, the vacuum degree of vacuum dehydration is maintained at 30-50kPa, and the pressing pressure is set to 50-70kN / m. In the step S6, the initial drying temperature of multi-cylinder drying is 85℃-95℃, and the final drying temperature is 115℃-130℃. Hot air drying is used in combination to ensure that the final moisture content is 5%-8%. In the step S7, the calendering temperature is set to 80-100℃, and the calendering pressure is set to 50-70kN / m.

5. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 1, characterized in that: After step S5, the surface treatment of the paper towel is added, the coating liquid is selected as polyvinyl alcohol PVA or polyacrylate, the coating liquid is evenly coated on the surface of the paper by a coating machine, the coated paper is dried by a drying device, a sizing liquid is prepared using starch and carboxymethyl cellulose CMC, the sizing liquid is evenly applied on the surface of the paper by a sizing device, and the sizing paper is dried by a drying device.

6. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 5, characterized in that: The polyvinyl alcohol PVA is 2%-5%, the polyacrylate is 1%-3%, the water is 92%-97%, the coating speed of the coating machine is 30-60m / min, and the coating amount is 5-10g / m 2 , starch is 3%-7%, carboxymethyl cellulose CMC is 0.5%-1.5%, water is 91.5%-96.5%, the sizing equipment sizing speed is 20-50m / min, and the sizing amount is 3-7g / m 2 .

7. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 1, characterized in that: After the S3 step or when the paper towel surface is treated, fragrance or functional additives are added, lavender essential oil or lemon essence is selected, and the fragrance is evenly added to the pulp or coated on the surface of the paper, and aloe extract or vitamin E additive is selected, and the functional additive is evenly added to the pulp or coated on the surface of the paper.

8. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 7, characterized in that: The lavender essential oil is 0.1%-0.3%, the lemon essence is 0.1%-0.3%, the added amount of lavender essential oil or lemon essence is 0.2%-0.6%, the aloe extract is 0.2%-0.5%, the vitamin E is 0.1%-0.3%, and the added amount of aloe extract or vitamin E is 0.2%-0.5%.

9. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 1, characterized in that: After the step S8, a multi-layer composite technology is added, and highly absorbent ingredients such as polyvinyl alcohol (PVA) and carboxymethyl cellulose (CMC) are added to the inner layer fiber formula, and softeners and reinforcing agents such as diethanolamine (DEA) and polyester fiber are added to the outer layer fiber formula, and the inner layer and the outer layer are combined together through a composite process.

10. The process for preparing a highly water-absorbent and breathable tissue base paper material according to claim 9, characterized in that: The polyvinyl alcohol (PVA) accounts for 0.5%-1.0%, the carboxymethyl cellulose (CMC) accounts for 0.5%-1.0%, and the wood pulp fiber accounts for 98%-99%.

Citation Information

Patent Citations

  • Preparation method for composite processed absorbent paper by using cylinder mould machine

    CN108867149A

  • Soft easy-to-degrade and dispersible plant fiber cleansing tissue as well as preparation method and application of soft easy-to-degrade and dispersible plant fiber cleansing tissue

    CN114808525A

  • Sanitary paper

    JP2004124314A

Cited By

  • Dialyzing paper and preparation method thereof

    CN119754081A