Inorganic two-component binder as well as preparation method and application thereof

By using inorganic two-component binder composed of modified water glass and polyols, silane coupling agents, etc. in the inorganic sand core, combined with microsilicon powder and other additives, the strength and fluidity of the inorganic sand core are solved, and the problem of inorganic sand core is improved. The comprehensive performance of castings is achieved, and a more environmentally friendly and efficient casting process is achieved.

CN118926478APending Publication Date: 2024-11-12BEIHANG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410994609.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing inorganic sand cores have low strength, poor fluidity, poor collapse and insufficient hygroscopic properties, resulting in low casting production efficiency and environmental pollution problems.

Method used

Inorganic consisting of sodium silicate powder, (S)-2-hydroxylithium propionate, polypotassium metaphosphate, sodium tetraborate, polyol, silane coupling agent, surfactant, modified silicone oil, chelating agent and resin Two-component binder, which prepares modified water glass through hydrothermal reaction, and combines with microsilicon powder, epoxy resin powder, nanocellulose whisker powder, solid lubricant and powder crumb agent to form efficient bonding agent system.

Benefits of technology

It significantly improves the strength, fluidity, collapse and anti-hygroscopic properties of inorganic sand, improves the comprehensive performance of castings, reduces harm to the human body and the environment, and achieves a more environmentally friendly and efficient casting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926478A_ABST
    Figure CN118926478A_ABST
Patent Text Reader

Abstract

The invention relates to a mixed enhanced inorganic two-component binder as well as a preparation method and application thereof. The inorganic two-component binder comprises a liquid agent and a powder agent, wherein the liquid agent is prepared from the following components in parts by mass: 30 to 50 parts of sodium silicate powder, 0.1 to 2 parts of (S)-2-hydroxypropionate lithium, 0.1 to 2 parts of potassium polymetaphosphate, 0.25 to 2 parts of sodium tetraborate, 19 to 66 parts of deionized water, 0.1 to 5 parts of polyhydric alcohol and 0.5 to 5 parts of silane coupling agent. The formula of the powder comprises the following components in parts by mass: 100 parts of micro silicon powder, 1-2 parts of epoxy resin powder and 2-4 parts of nano cellulose whisker powder. The mixed enhanced inorganic two-component binder is obtained by exploring the material formulas of liquid and powder, the strength, fluidity, collapsibility and moisture absorption resistance of molding sand can be greatly improved, the comprehensive performance of inorganic molding sand is remarkably improved, and the mixed enhanced inorganic two-component binder has wide application prospects in the field of green and environment-friendly molding sand.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of casting technology, and in particular to a composite reinforced inorganic two-component binder and a preparation method and application thereof. The inorganic two-component binder has the advantages of high strength, good moisture resistance, good fluidity, high disintegration, etc. Background Art

[0002] As society's urgent demand for energy conservation and emission reduction and new energy vehicles continues to increase, the automotive industry's demand for large-size hollow thin-walled aluminum alloy castings such as aluminum alloy subframes and motor housings is also expanding. However, in the traditional sand core preparation process, toxic organic resin binders such as furan resins are usually used. These organic binders release a large amount of toxic gases and air pollutants during use, posing a serious threat to the health of operators and causing great damage to the environment.

[0003] In order to solve this problem, it is urgent to find new environmentally friendly inorganic materials to replace traditional organic resins. This will not only help improve the sustainability of casting binders, but also effectively reduce harm to human health and the environment. The introduction of new inorganic bonding materials will provide a more environmentally friendly and healthier option for the production of automotive aluminum alloy castings, and contribute to the sustainable development of the industry.

[0004] In recent years, new inorganic binders have been initially applied to the production of inorganic sand and sand cores. Unlike the traditional single-component water glass binder, the new inorganic binder adopts an inorganic two-component system consisting of a liquid and a powder. Usually, the liquid uses modified water glass, while the powder includes ingredients such as a curing agent, aggregates, and trace additives. Although the new inorganic binder surpasses the traditional organic binder in some aspects, there are still some problems, one of which is that the strength of the sand core is not satisfactory. This problem mainly stems from the fact that traditional organic binders use chemical reactions to form cross-linking hardening, while water glass binders usually use simple physical dehydration hardening. By adding special additives to water glass, its hardening mechanism can be changed from physical dehydration hardening to chemical cross-linking hardening, thereby improving the strength of the sand core. Therefore, in-depth research on the formula of adding additives is crucial to solving the problem of low strength of inorganic sand cores.

[0005] In addition, the preparation process of inorganic sand usually includes mixing the water glass binder and the raw sand in a certain order to form an inorganic sand mixture, and then combining the preparation process of the inorganic sand core to obtain the final sand core. However, in the preparation process of inorganic sand, the viscosity of the water glass binder will cause the fluidity of the inorganic sand mixture to decrease, resulting in problems such as sticking to the wall and being unable to completely fill the mold. In addition, the strength of the water glass sand is almost unchanged before and after casting, and the collapsibility is poor, which makes it difficult to clean the sand from the casting. At the same time, due to the water glass sand's easy water absorption, the sand core will fail during storage due to the water glass absorbing water, making the water glass sand's anti-hygroscopic performance poor.

[0006] Therefore, there is an urgent need to find a two-component inorganic binder to solve the current problems of inorganic sand in terms of curing speed, strength, fluidity, disintegration and anti-hygroscopicity, so as to improve the comprehensive performance of the sand core and ensure industrial production efficiency.

[0007] It should be noted that the information disclosed in this background technology section is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or suggestion in any form that the information constitutes the prior art known to those skilled in the art. Summary of the invention

[0008] In view of this, the purpose of the present invention is to provide an inorganic two-component binder and a preparation method and application thereof in view of the current status of the above-mentioned prior art, and to solve the technical problems of low strength, poor fluidity, poor disintegration and poor anti-hygroscopicity of the existing inorganic molding sand by exploring the material formula of the liquid and powder in the inorganic two-component binder.

[0009] To achieve the above object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a liquid of the above-mentioned inorganic two-component adhesive, which includes a matrix and a first composite agent, wherein the matrix includes the following components in parts by weight: 30 to 50 parts of sodium silicate powder, 0.1 to 2 parts of (S)-2-hydroxypropionic acid lithium, 0.1 to 2 parts of potassium polymetaphosphate, 0.25 to 2 parts of sodium tetraborate, and 19 to 66 parts of deionized water; the first composite agent includes a polyol and a silane coupling agent, wherein 0.1 to 5 parts of a polyol and 0.5 to 5 parts of a silane coupling agent are added to 100 parts of the matrix, mixed evenly, to obtain a liquid A, and the liquid A is used as the liquid of the inorganic two-component adhesive.

[0011] Furthermore, a second composite agent is added to the formula of the liquid, and the second composite agent includes a surfactant and a modified silicone oil; wherein, 0.01 to 1 part of a surfactant and 1 to 4 parts of modified silicone oil are added to 100 parts of the liquid A, and mixed evenly to obtain a liquid B, and the liquid B is used as the liquid of the inorganic two-component adhesive.

[0012] Furthermore, a third compounding agent is added to the formula of the liquid, and the third compounding agent includes a chelating agent and a resin; wherein, 1 to 8 parts of the chelating agent and 2 to 4 parts of the resin are added to 100 parts of the liquid A or 100 parts of the liquid B, and mixed evenly to obtain liquid C, and the liquid C is used as the liquid of the inorganic two-component adhesive.

[0013] In a second aspect, the present invention provides a powder of the above-mentioned inorganic two-component binder, wherein the formula of the powder comprises the following components in parts by mass: 100 parts of microsilica powder, 1 to 2 parts of epoxy resin powder and 2 to 4 parts of nanocellulose whisker powder.

[0014] Furthermore, the following components in parts by mass are added to the powder formula: 4 to 6 parts of solid lubricant.

[0015] Furthermore, the formula of the powder also contains the following components in parts by mass: 2 to 4 parts of a powder disintegrating agent.

[0016] In a third aspect, the present invention provides a method for preparing the liquid preparation of the first aspect, comprising the following steps:

[0017] S11 Preparation of modified water glass matrix: 30-50 parts of sodium silicate powder, 0.1-2 parts of (S)-2-hydroxypropionic acid lithium, 0.1-2 parts of potassium polymetaphosphate, 0.25-2 parts of sodium tetraborate and 19-66 parts of deionized water are mixed, and modified water glass is obtained through hydrothermal reaction.

[0018] S12: adding the first composite agent: adding 0.1-5 parts of polyol and 0.5-5 parts of silane coupling agent to 100 parts of the modified water glass prepared in step S11, mixing evenly to obtain liquid A, and using the liquid A as a liquid of the inorganic two-component adhesive.

[0019] Furthermore, in step S11, the reaction temperature of the hydrothermal reaction is 140-160° C., and the reaction time is 8-12 hours.

[0020] Furthermore, the step S11 specifically includes: adding 0.1 to 2 parts of lithium (S)-2-hydroxypropionate, 0.1 to 2 parts of potassium polymetaphosphate and 0.25 to 2 parts of sodium tetraborate to 19 to 66 parts of water, stirring until lithium polyacrylate, potassium polymetaphosphate and sodium tetraborate are dissolved; then adding 30 to 50 parts of sodium silicate, reacting until the sodium silicate is dissolved.

[0021] Furthermore, the above preparation method further comprises the following steps:

[0022] S13 adding a second composite agent: adding 0.01 to 1 part of a surfactant and 1 to 4 parts of silicone oil to 100 parts of the liquid A prepared in step S12, mixing evenly to obtain a liquid B, and using the liquid B as the liquid of the inorganic two-component adhesive.

[0023] Furthermore, the above preparation method further comprises the following steps:

[0024] S14: adding a third compounding agent: adding 1 to 8 parts of a chelating agent and 2 to 4 parts of a resin to 100 parts of the liquid A prepared in step (2) or the liquid B prepared in step (3), mixing them evenly to obtain a liquid C, and using the liquid C as the liquid of the hybrid enhanced inorganic two-component adhesive.

[0025] In a fourth aspect, the present invention provides a method for preparing the liquid preparation of the second aspect, comprising the following steps:

[0026] S21: After gradually adding 1 to 2 parts of epoxy resin powder and 2 to 4 parts of nanocellulose whisker powder into 100 parts of microsilica powder, use a stirring equipment to evenly stir the mixture to ensure that the various ingredients are fully dispersed and mixed to form powder A, and use powder A as the powder of the inorganic two-component adhesive.

[0027] Furthermore, the above preparation method further comprises the following steps:

[0028] S22: adding solid lubricant: gradually adding 4 to 6 parts of solid lubricant to the powder A prepared in step S21, mixing evenly to form powder B, and using the powder B as the powder of the inorganic two-component binder.

[0029] Furthermore, the above preparation method further comprises the following steps:

[0030] S23: adding powder disintegrating agent: adding 2 to 4 parts of powder disintegrating agent to the powder A prepared in step S21 or the powder B prepared in step S22, mixing evenly to form powder C, and using the powder C as the powder of the inorganic two-component binder.

[0031] In a fifth aspect, the present invention provides a method for preparing inorganic molding sand, comprising the following steps: adding raw sand into a sand mixer for mixing, adding the powder of the second aspect to the raw sand while mixing, and after mixing evenly, adding the liquid of the first aspect to obtain molding sand; wherein, 1 to 5 parts of the liquid and 0.1 to 5 parts of the powder are added to every 100 parts of raw sand.

[0032] The beneficial effects of the present invention are:

[0033] 1. The liquid of the inorganic two-component binder provided by the present invention effectively improves the strength of the sand core by changing the curing mechanism of the binder. At the same time, the surfactant and modified silicone oil added in the liquid can synergistically reduce the friction resistance between the gravel and the wall of the sand-shooting mold, thereby improving the fluidity of the inorganic sand. Further adding a chelating agent can form a high-functionality cross-linking site between water glass and sand particles, further improving the strength of the inorganic sand. The addition of resin in the liquid not only improves the mechanical properties of the binder after curing, but also enhances the anti-hygroscopic properties of the inorganic sand. The polyol is rich in terminal hydroxyl groups, and forms a high-functionality cross-linking site with water glass and sand particles, further improving the strength of the inorganic sand. Silane coupling agent is a compound with a dual reaction function, and the alkoxy group in its molecule is hydrolyzed to generate an active group silanol, which reacts with the surface of silica sand to form a continuous film, thereby improving the curing speed, strength and anti-hygroscopicity of the inorganic sand core.

[0034] 2. Solid lubricants are added to the powder of the two-component adhesive provided by the present invention, and the lubrication effect is achieved by means of its physical structure, further improving the fluidity of inorganic sand. Powder disintegrator, epoxy resin powder and nanocellulose whisker powder are also added to the powder, and the combined effect of the three leads to a decrease in the strength of the sand core after pouring, making sand cleaning easier and improving the user experience. At the same time, the addition of resin powder and nanocellulose whiskers strengthens the bonding network of the adhesive and significantly improves the bonding strength of the adhesive.

[0035] 3. The optimization of the formula of the above-mentioned liquid and powder enables the mixed enhanced inorganic two-component adhesive to significantly improve the comprehensive performance of inorganic sand, and has broad application prospects in the field of inorganic sand bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0037] Figure 1 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in each embodiment and comparative example provided in this application;

[0038] Figure 2-Figure 3 This is a test diagram of the anti-hygroscopicity of the long strip inorganic sand block samples prepared in each embodiment and comparative example provided in this application;

[0039] Figure 4 This is a graph showing the collapsibility of cylindrical inorganic sand block samples prepared in various embodiments and comparative examples provided in this application;

[0040] Figure 5 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Comparative Example 2 and Comparative Example 1 provided in this application;

[0041] Figure 6 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Comparative Examples 3, 4 and Comparative Example 2 provided in this application;

[0042] Figure 7 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Examples 1, 2 and Comparative Example 3 provided in the present application;

[0043] Figure 8 This is a test diagram of the moisture absorption resistance of the long strip inorganic sand block samples prepared in Examples 1, 2 and Comparative Example 3 provided in the present application;

[0044] Fig. 9 This is a graph showing the collapsibility of the cylindrical inorganic sand block samples prepared in Examples 1, 2 and Comparative Example 3 provided in the present application;

[0045] Fig.10 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Examples 5, 6 and Examples 1, 2 provided in this application;

[0046] Fig.11 This is a test diagram of the moisture absorption resistance of the long strip inorganic sand block samples prepared in Examples 5, 6 and Examples 1, 2 provided in this application;

[0047] Fig.12 This is a graph showing the collapsibility of the cylindrical inorganic sand block samples prepared in Examples 5, 6 and Examples 1, 2 provided in this application;

[0048] Fig.13 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Example 7 and Comparative Example 3 provided in the present application;

[0049] Fig.14 This is a test diagram of the anti-hygroscopicity of the long strip inorganic sand block samples prepared in Example 7 and Comparative Example 3 provided in the present application;

[0050] Fig.15 This is a graph showing the collapsibility of the cylindrical inorganic sand block samples prepared in Example 7 and Comparative Example 3 provided in the present application;

[0051] Fig.16 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Examples 8, 9 and Comparative Example 3 provided in the present application;

[0052] Fig.17 This is a graph showing the collapsibility of the cylindrical inorganic sand block samples prepared in Examples 12, 13 and Examples 8, 9 provided in the present application;

[0053] Fig.18This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Example 14 and Comparative Example 3 provided in the present application;

[0054] Fig.19 This is a graph showing the collapsibility of the cylindrical inorganic sand block samples prepared in Example 14 and Comparative Example 3 provided in the present application;

[0055] Fig. 20 This is a test diagram of the bending strength of the long strip inorganic sand block samples prepared in Example 15 and Comparative Example 3 provided in the present application;

[0056] Fig.21 This is a test diagram of the anti-hygroscopicity of the long strip inorganic sand block samples prepared in Example 15 and Comparative Example 3 provided in the present application;

[0057] Fig. 22 This is a graph showing the collapsibility of the cylindrical inorganic sand block samples prepared in Example 15 and Comparative Example 3 provided in the present application;

[0058] Fig.23 This is a schematic structural diagram of a strip-shaped inorganic sand block sample for testing the bending strength of a sand core used in each embodiment and comparative example of the present application;

[0059] Fig.24 This is a schematic structural diagram of a cylindrical inorganic sand block sample for testing the collapsibility of sand cores used in each embodiment and comparative example of the present application;

[0060] Fig.25 This is a schematic structural diagram of a curved inorganic sand sample used in the inorganic sand fluidity test used in each embodiment and comparative example of the present application. DETAILED DESCRIPTION

[0061] The following is a more detailed description of the technical features and advantages of the present application in combination with embodiments and comparative examples, so that the advantages and features of the present application can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0062] The embodiments of the present application provide an inorganic two-component binder modified with trace organic matter, comprising a liquid and a powder. By exploring and optimizing the material formula of the liquid and the powder, the inorganic two-component binder can solve the technical problems of low strength, poor fluidity, poor disintegration and poor anti-hygroscopicity of existing molding sand when used for sand mixing.

[0063] First, the embodiment of the present application provides a liquid formulation of the inorganic two-component binder, the liquid formulation includes a matrix and a first composite agent, wherein the matrix includes the following components by mass: 30 to 50 parts of sodium silicate powder, 0.1 to 2 parts of (S)-2-hydroxypropionic acid lithium, 0.1 to 2 parts of potassium polymetaphosphate, 0.25 to 2 parts of sodium tetraborate, and 19 to 66 parts of deionized water; the first composite agent includes a polyol and a silane coupling agent, 0.1 to 5 parts of a polyol and 0.5 to 5 parts of a silane coupling agent are added to 100 parts of the matrix, mixed evenly, and liquid A is obtained, and liquid A is used as the liquid of the inorganic two-component binder. In the formula of the above-mentioned liquid, by adding (S)-2-hydroxypropionic acid lithium, potassium polymetaphosphate, and sodium tetraborate to water glass (aqueous solution of sodium silicate) to modify the water glass, the curing mechanism of the binder can be effectively changed and the strength of the sand core can be improved. Unmodified water glass (aqueous solution of sodium silicate) has the disadvantages of slow curing speed, low bonding strength and weak anti-hygroscopic performance. The present embodiment can improve the curing speed, bonding strength and anti-hygroscopicity of water glass binder to a certain extent by modifying water glass and adjusting its parameters such as modulus, cation content and solid content, so that the modified water glass has better performance and wider application surface as a binder. And the polyol further added is rich in terminal hydroxyl groups, which can cross-link sites with high functionality between water glass and sand particles, thereby improving the strength of inorganic sand; the added silane coupling agent is a compound with double reaction function, and the alkoxy group in the molecule is hydrolyzed to generate active group silanol, which reacts with the surface of silica sand, and the surface performance is changed from hydrophilic to hydrophobic to different degrees, and can be spread into a continuous film on the surface of silica sand, forming a firm chemical bond (≡Si-OM, M is inorganic sand) between the interface of silica sand and the binder surface, thereby improving the strength and anti-hygroscopicity of the inorganic sand core.

[0064] In the formula, the polyol can preferably be one of ethylene glycol monobenzyl ether, aminoisooctanol, isopentylene glycol, sucrose alcohol, xylitol, propylene glycol monoisopropyl ether, propylene glycol diisopropyl ether and polyethylene glycol, or a mixture of several of them.

[0065] The silane coupling agent can preferably be one or a mixture of γ-(2,3-epoxypropyl)propyltrimethoxysilane, p-phenylvinyltrimethoxysilane, (3-epoxypropyl)trimethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxysilane and N-vinylbenzyl-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride.

[0066] In a preferred embodiment of the present application, a second compounding agent is further added to the formula of the liquid of the inorganic two-component binder, and the second compounding agent includes a surfactant and a modified silicone oil; wherein, 0.01 to 1 part of a surfactant and 1 to 4 parts of a modified silicone oil are added to 100 parts of the above-mentioned liquid A, and the mixture is evenly mixed to obtain a liquid B, and the liquid B is used as the liquid of the mixed enhanced inorganic two-component binder. In the formula of this embodiment, the addition of a surfactant can change the surface tension of the water glass liquid and the wetting properties for the molding sand and metal, effectively reduce the friction resistance between the gravel and the wall of the sand-shooting mold, and thus improve the fluidity of the molding sand mixture. The addition of modified silicone oil can change the surface tension of the water glass liquid and the wetting properties for the molding sand and metal, and can effectively reduce the friction resistance between the gravel and the wall of the sand-shooting mold, and thus improve the fluidity of the molding sand mixture. Surfactants and modified silicone oil are added to the modified water glass matrix, both of which can change the surface tension of the water glass liquid and its wetting properties for molding sand and metal, and can effectively reduce the friction resistance between the gravel and the wall of the sand shooting mold, thereby improving the fluidity of the molding sand mixture.

[0067] Among them, the surfactant is preferably an anionic surfactant or a nonionic surfactant. The reason for selecting anionic or nonionic surfactants is that cationic surfactants will react chemically with water glass, resulting in the production of white flocculent insolubles in the water glass, and will cause the water glass binder to lose its function, so anionic surfactants and nonionic surfactants that do not react with water glass are selected. Surfactants and modified silicone oil are added to the matrix of modified water glass, which can change the surface tension of the water glass liquid and the wetting properties for molding sand and metal, and can effectively reduce the friction resistance of gravel and the wall of the sand-shooting mold, thereby improving the fluidity of the inorganic sand mixture. The surfactant is more preferably an anionic surfactant; further preferably, the surfactant can be selected from one or a mixture of hydrogenated castor oil fatty acid, dehydrated castor oil fatty acid, tall oil fatty acid hexadecene salt, castor oil fatty acid and ammonium lauryl sulfate.

[0068] The modified silicone oil is preferably one or a mixture of amino-modified silicone oil, epoxy-modified silicone oil, polyether-modified silicone oil, carboxyl-modified silicone oil, alcohol-hydroxyl-modified silicone oil, phenol-modified silicone oil, mercapto-modified silicone oil, and polydiorganosiloxane-polyether block copolymer modified silicone oil.

[0069] In a preferred embodiment of the present application, a third compounding agent is further added to the formula of the liquid of the inorganic two-component adhesive, and the third compounding agent includes a chelating agent and a resin; wherein, 1 to 8 parts of a chelating agent and 2 to 4 parts of a resin are added to 100 parts of the above-mentioned liquid A or 100 parts of the above-mentioned liquid B, and mixed evenly to obtain a liquid C, and the liquid C is used as the liquid of the inorganic two-component adhesive. In the formula of this embodiment, the added chelating agent can form a high-functionality cross-linking site between water glass and sand particles, thereby improving the strength of the molding sand. The addition of the resin improves the mechanical properties of the inorganic sand after curing, and the addition of the resin can also improve the anti-hygroscopic properties of the inorganic sand. The single-component epoxy resin and the water-soluble phenolic resin also ensure that the inorganic adhesive will not be accidentally cured during storage and transportation.

[0070] The chelating agent may preferably be one or a mixture of sodium N,N-dicarboxylic acid amino-2-hydroxypropane sulfonate, sodium gluconate, polyaspartic acid, polyacrylic acid and acrylic acid-maleic anhydride copolymer.

[0071] The resin can preferably be a mixture of one or both of a medium temperature curing single component epoxy resin and a water-soluble phenolic resin. The reason for selecting the medium temperature curing single component epoxy resin is that it will not undergo a curing reaction at room temperature. While improving the bonding performance of the water glass binder, it can prevent the added epoxy resin from undergoing a curing reaction in a conventional size environment, thereby extending the shelf life. The water-soluble phenolic resin can be dissolved in the binder system to improve the bonding strength.

[0072] Secondly, the embodiment of the present application provides a powder formula of the inorganic two-component binder, including the following components by mass: 100 parts of microsilica powder, 1-2 parts of epoxy resin powder and 2-4 parts of nanocellulose whisker powder. In the powder formula, nanocellulose whiskers are a kind of micro-needle-shaped active cellulose material, and the active terminal hydroxyl groups on their surface will cross-link with the microsilica powder, water glass and inorganic sand surface, and at the same time strengthen the bonding network, thereby significantly improving the bonding strength of the binder.

[0073] The nanocellulose whisker powder may preferably be one or a mixture of cellulose nanowhiskers, sulfonated cellulose nanowhiskers and carboxylated cellulose nanowhiskers.

[0074] In a preferred embodiment of the present application, the powder formulation further includes the following components in parts by mass: 4 to 6 parts of solid lubricant. The addition of solid lubricant can reduce the friction between inorganic sands and improve the fluidity of inorganic sands after sand mixing.

[0075] The solid lubricant may preferably be one or a mixture of polytetrafluoroethylene, molybdenum disulfide and polyimide.

[0076] In a preferred embodiment of the present application, the formula of the powder may further include the following components in parts by mass: 2 to 4 parts of powder disintegrating agent. The powder disintegrating agent decomposes in the high temperature environment of casting, releases gases such as carbon dioxide and water vapor, destroys the bonding bridge of the sand core, causes the sand core to break after casting, thereby improving the disintegration of the sand core and making it easier to remove sand.

[0077] The powder disintegrator can preferably be one or a mixture of basic copper carbonate powder, manganese carbonate powder, zinc carbonate powder, sodium carbonate powder, corn starch and dextrin.

[0078] The embodiments of the present application further provide a method for preparing the above-mentioned hybrid reinforced inorganic two-component binder, comprising the following steps:

[0079] S1 Preparation of the liquid of the inorganic two-component binder

[0080] S11 Preparation of modified water glass matrix:

[0081] a. Prepare raw materials: prepare 30 to 50 parts of sodium silicate powder (as the main raw material of water glass), 0.1 to 2 parts of (S)-2-hydroxypropionic acid lithium (modifier), 0.1 to 2 parts of potassium polymetaphosphate (modifier), 0.25 to 2 parts of sodium tetraborate (modifier) ​​and 19 to 66 parts of deionized water (as solvent and reaction medium).

[0082] b. Mixing raw materials: Place sodium silicate powder, (S)-2-hydroxypropionic acid lithium, potassium polymetaphosphate, sodium tetraborate and deionized water in a reaction container in proportion to ensure that the components are evenly mixed.

[0083] c. Perform hydrothermal reaction: Place the mixture in a hydrothermal reaction device, set the reaction temperature to 140-160°C, and the reaction time to 8-12 hours. Hydrothermal reaction is a chemical reaction carried out under high temperature and high pressure conditions, which helps to promote the reaction and combination between the raw materials to form modified water glass.

[0084] S12: adding the first compounding agent: adding 0.1 to 5 parts of polyol and 0.5 to 5 parts of silane coupling agent to 100 parts of the modified water glass matrix prepared in step (1), wherein the addition of polyol helps to adjust the fluidity and viscosity of the binder, and the silane coupling agent is used to improve the bonding force between the binder and the filler. The components are mixed uniformly to obtain a liquid A, and the liquid A is used as the liquid of the inorganic two-component binder.

[0085] In a preferred embodiment of the present application, the preparation step of the liquid may further include:

[0086] S13 adding a second compounding agent: on the basis of 100 parts of the liquid A prepared in step S12, further adding 0.01 to 1 parts of a surfactant and 1 to 4 parts of a modified silicone oil. The surfactant and the modified silicone oil are dissolved or dispersed in the water glass matrix by stirring or mixing, and the liquid B is obtained by mixing evenly, and the liquid B is used as the liquid of the inorganic two-component adhesive. In this formula, the surfactant can improve the dispersibility and stability of the water glass, and the modified silicone oil can be used to improve the wettability and high temperature resistance of the adhesive.

[0087] In a more preferred embodiment of the present application, the preparation step of the liquid may further include:

[0088] S14: adding a third compounding agent: further adding 1 to 8 parts of a chelating agent and 2 to 4 parts of a resin to 100 parts of liquid A prepared in step S12 or 100 parts of liquid B prepared in step S13, and fully mixing and stirring to ensure that each component is evenly dispersed and fully reacted, to obtain liquid C, and use liquid C as the liquid of the inorganic two-component adhesive.

[0089] In summary, the formulation of the liquid agent in the embodiment of the present application can be selected from the following schemes:

[0090] Formula 1: modified water glass matrix (sodium silicate powder, (S)-2-hydroxypropionic acid lithium, potassium polymetaphosphate, sodium tetraborate, deionized water) + first compounding agent (polyol, silane coupling agent);

[0091] Formula 2: modified water glass matrix (sodium silicate powder, (S)-2-hydroxypropionic acid lithium, potassium polymetaphosphate, sodium tetraborate, deionized water) + first compounding agent (polyol, silane coupling agent) + second compounding agent (surfactant, modified silicone oil);

[0092] Formula 3: modified water glass matrix (sodium silicate powder, (S)-2-hydroxypropionic acid lithium, potassium polymetaphosphate, sodium tetraborate, deionized water) + first compounding agent (polyol, silane coupling agent) + third compounding agent (chelating agent, resin);

[0093] Formula 4: modified water glass matrix (sodium silicate powder, (S)-2-hydroxypropionic acid lithium, potassium polymetaphosphate, sodium tetraborate, deionized water) + first compounding agent (polyol, silane coupling agent) + second compounding agent (surfactant, modified silicone oil) + third compounding agent (chelating agent, resin). When preparing the liquid, the order of adding the above-mentioned formula components can be adjusted as needed.

[0094] S2 Preparation of the powder of the inorganic two-component binder

[0095] S21 prepare raw materials: prepare the required 100 parts of microsilica powder, 1 to 2 parts of epoxy resin powder and 2 to 4 parts of nanocellulose whisker powder.

[0096] S22 Mixed raw materials: After gradually adding 1 to 2 parts of epoxy resin powder and 2 to 4 parts of nano-cellulose whisker powder into the microsilica powder, use a stirring equipment to evenly stir the mixture to ensure that all ingredients are fully dispersed and mixed to form powder A, and use powder A as the powder of the inorganic two-component binder.

[0097] In a preferred embodiment of the present application, the preparation step of the powder may further include:

[0098] S23 adding solid lubricant: gradually adding 4 to 6 parts of solid lubricant to the powder A in step 2, mixing evenly to form powder B, and using the powder B as the powder of the inorganic two-component binder. In the powder formula, the solid lubricant has the function of reducing the friction coefficient of the binder and improving fluidity and processing performance.

[0099] In a more preferred embodiment of the present application, the preparation step of the powder may further include:

[0100] S24: Adding a powder disintegrating agent: Add 2 to 4 parts of the powder disintegrating agent to the powder A or powder B in step 2, mix them evenly to form a powder C, and use the powder C as the powder of the inorganic two-component binder. In the powder formula, the addition of the powder disintegrating agent helps to improve the disintegrating performance and fluidity of the binder.

[0101] In summary, the formula of the powder in the embodiment of the present application can be selected from the following schemes:

[0102] Formula 1: 100 parts of microsilica powder, 1-2 parts of epoxy resin powder, 2-4 parts of nanocellulose whisker powder;

[0103] Formula 2: 100 parts of microsilica powder, 1-2 parts of epoxy resin powder, 2-4 parts of nanocellulose whisker powder and 4-6 parts of solid lubricant;

[0104] Formula 3: 100 parts of microsilica powder, 1-2 parts of epoxy resin powder, 2-4 parts of nanocellulose whisker powder + 2-4 parts of powder disintegrator;

[0105] Formula 4: 100 parts of microsilica powder, 1-2 parts of epoxy resin powder and 2-4 parts of nanocellulose whisker powder + 4-6 parts of solid lubricant + 2-4 parts of powder disintegrator. When preparing the powder, the order of adding the above formula components can be adjusted as needed.

[0106] The liquid prepared in step S1 and the powder prepared in step S2 are stored separately for subsequent use in preparing molding sand. The recommended storage method is as follows:

[0107] 1. Choose a suitable storage container: Choose a clean, dry, well-sealed container, such as a plastic bucket, glass bottle or metal container. Make sure the surface of the container is clean and free of residue.

[0108] 2. Clearly label: Mark the container with important information such as the name, batch number, production date and expiration date of the liquid / powder. This helps to track and manage the use of the liquid / powder.

[0109] 3. Avoid direct sunlight: Place the storage container in a cool, dry place, away from direct sunlight and heat sources. Avoid prolonged exposure to high temperatures to prevent the quality of the liquid / powder from being affected.

[0110] 4. Regular inspection and maintenance: Regularly check the sealing and appearance of the storage container to ensure that there is no damage or leakage. If any problems are found, replace the container or repair the seal in time.

[0111] 5. Avoid cross contamination: Store different types or batches of liquids / powders separately to avoid cross contamination and chemical reactions and ensure their stability and performance.

[0112] 6. Strictly control humidity: Maintain a dry environment in the storage area. Use a dehumidifier or hygrometer to monitor the humidity level. Avoid moisture absorption by liquid / powder, which may cause performance degradation.

[0113] 7. Proper disposal of waste: When handling adhesive packaging and waste, they should be classified and properly disposed of in accordance with local environmental regulations to avoid pollution to the environment.

[0114] The above steps help to protect the quality and stability of the inorganic binder, extend its service life, and ensure that the binder can be used safely and effectively when needed.

[0115] The present application further provides a method for preparing inorganic molding sand using the above-mentioned inorganic two-component binder, comprising the following steps:

[0116] 1. Prepare sand mixing equipment: Prepare the sand mixer or other suitable mixing equipment and ensure that the equipment is clean and free of impurities.

[0117] 2. Add raw sand: put the raw sand to be processed into the sand mixing equipment.

[0118] 3. Add the powder of the inorganic two-component binder: gradually add the required amount of the powder prepared in step S2 to the raw sand. The powder can be added in batches or continuously to ensure that the binder and the raw sand particles are evenly mixed. The added amount is 0.1 to 5 parts of the powder per 100 parts by mass of the raw sand.

[0119] 4. Add the liquid of the inorganic two-component binder: gradually add the required amount of the liquid prepared in step S1 to the raw sand. This can be done by adding in batches or continuously to ensure that the binder is fully covered and evenly mixed with the raw sand particles. The amount of the liquid added is 1 to 5 parts per 100 parts by mass of the raw sand.

[0120] 5. Control the mixing time: When adding liquid agent, control the mixing time to ensure uniform mixing without over-solidification or loss of liquid agent activity. It is usually recommended that the mixing time after adding powder is 1 to 2 minutes, and the mixing time after adding liquid agent is 1 to 2 minutes, and the total mixing time is 2 to 4 minutes.

[0121] 6. Observe the mixing effect: By observing the particle state and color changes of the molding sand inside the sand mixing equipment, determine whether the mixing has reached the ideal state.

[0122] 7. Storage and use: Store the mixed inorganic sand in a dry, clean, sealed container to avoid moisture and impurity contamination for subsequent casting process use.

[0123] By executing the above steps, inorganic sand with stable quality and superior performance can be obtained, which is suitable for various casting processes and improves the quality and production efficiency of castings.

[0124] In order to verify the strength, fluidity, disintegration and anti-hygroscopicity of the prepared molding sand mixture, the prepared molding sand mixture was added to the new hot air-warm core box composite hardening process sample machine, and the molding sand block samples were obtained by hot air heating and molding. The number of obtained molding sand block samples and the degree of mold filling were used as the standard for testing the fluidity of the molding sand mixture, and the flexural strength of the molding sand block samples after being placed at room temperature for different times, the flexural strength after being placed at room temperature and high humidity for different times, and the compressive strength after high temperature storage were measured.

[0125] In the embodiments and comparative examples of the present application, several molding sand block samples in the shape of curved, strip and cylindrical shapes are prepared to facilitate testing of fluidity and testing in a bending test machine and a compression test machine. The shapes of the molding sand block samples used are curved and strip, to facilitate testing of fluidity and testing in a bending test machine. Fig. 22 , which is a schematic diagram of the structure of a strip-shaped sand block sample; please refer to Fig.23 , for the structural diagram of the cylindrical sand block specimen, please refer to Fig.24 , which is a schematic diagram of the structure of the curved molding sand block specimen.

[0126] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0127] The raw materials and reagents used in the following examples and comparative examples are all commercially available or homemade.

[0128] Comparative Example 1

[0129] 1) Preparation of water glass:

[0130] Add 57 g of sodium silicate to 93 g of water and stir until the sodium silicate is dissolved to obtain a mixture. The mixing temperature of the above mixing process is 25° C. and the stirring rate is 800 rpm. Add the mixed solution into a hydrothermal reactor and perform a hydrothermal reaction at 150° C. for 10 hours to obtain 150 g of a single-component water glass adhesive.

[0131] Comparative Example 2

[0132] 1) Preparation of water glass:

[0133] Add 57 g of sodium silicate to 93 g of water and stir until the sodium silicate is dissolved to obtain a mixture. The mixing temperature of the above mixing process is 25° C. and the stirring rate is 800 rpm. Add the mixed solution to a hydrothermal reactor and perform a hydrothermal reaction at 150° C. for 10 hours to obtain 150 g of water glass binder as a liquid of an inorganic two-component binder.

[0134] 2) Use microsilica powder as a powder of an inorganic two-component binder.

[0135] Comparative Example 3

[0136] 1) Preparation of modified water glass:

[0137] Add 0.3g of lithium (S)-2-hydroxypropionate and 0.15g of potassium oxonate to 93g of water, stir until the lithium (S)-2-hydroxypropionate and potassium oxonate are dissolved; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.45g of modified water glass binder as a liquid agent of an inorganic two-component binder.

[0138] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0139] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0140] Comparative Example 4

[0141] 1) Preparation of modified water glass:

[0142] Add 0.6g of lithium (S)-2-hydroxypropionate and 0.3g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionate and potassium oxonate; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.9g of modified water glass binder as a liquid agent of an inorganic two-component binder.

[0143] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0144] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0145] Example 1

[0146] 1) Preparation of modified water glass:

[0147] Add 0.3g of lithium (S)-2-hydroxypropionic acid and 0.15g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.45g of modified water glass binder.

[0148] 2) Preparation of liquid inorganic two-component adhesive:

[0149] 1 g of polyethylene glycol and 2 g of (3-glycidoxypropyl)trimethoxysilane were added to 100 g of the modified water glass prepared in step 1) to obtain 110 g of a liquid composite reinforced inorganic modified water glass binder. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0150] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0151] Example 2

[0152] 1) Preparation of modified water glass:

[0153] Add 1.5g of lithium (S)-2-hydroxypropionic acid and 0.5g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 152g of modified water glass binder.

[0154] 2) Preparation of liquid inorganic two-component adhesive:

[0155] 5 g of polyethylene glycol and 5 g of p-phenyltrimethoxysilane were added to 100 g of the modified water glass prepared in step 1) to obtain 110 g of a liquid composite reinforced inorganic modified water glass binder. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0156] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0157] Example 3

[0158] 1) Preparation of modified water glass:

[0159] Add 1g of lithium (S)-2-hydroxypropionate and 1g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionate and potassium oxonate; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 152g of modified water glass binder.

[0160] 2) Preparation of liquid inorganic two-component adhesive:

[0161] 1 g of aminoisooctanol and 4 g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane were added to 100 g of the modified water glass obtained in step 1), and then 0.4 g of castor oil fatty acid and 1 g of epoxy-modified silicone oil were added and mixed evenly to obtain 106.4 g of a liquid of an inorganic two-component adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0162] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0163] Example 4

[0164] 1) Preparation of modified water glass:

[0165] Add 0.3g of lithium (S)-2-hydroxypropionate and 0.3g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionate and potassium oxonate; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.6g of modified water glass binder.

[0166] 2) Preparation of liquid inorganic two-component adhesive:

[0167] 2 g of sucrose alcohol and 6 g of (3-glycidoxypropyl)trimethoxysilane were added to 100 g of the modified water glass obtained in step 1), and then 0.8 g of castor oil fatty acid and 4 g of epoxy-modified silicone oil were added and mixed evenly to obtain 112.8 g of a liquid inorganic two-component adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0168] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0169] Example 5

[0170] 1) Preparation of modified water glass:

[0171] Add 1g of lithium (S)-2-hydroxypropionic acid and 0.15g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 151.15g of modified water glass binder.

[0172] 2) Preparation of liquid inorganic two-component adhesive:

[0173] 4 g of propylene glycol monoisopropyl ether and 2 g of N-vinylbenzyl-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride were added to 100 g of the modified water glass obtained in step 1), and then 1 g of sodium gluconate and 2 g of a single-component medium-temperature curing epoxy resin were added after stirring, and mixed evenly to obtain 1096 g of a liquid of an inorganic two-component adhesive. The mixing temperature of the above mixing process was 25° C. and the stirring rate was 800 rpm.

[0174] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0175] Example 6

[0176] 1) Preparation of modified water glass:

[0177] Add 0.3g of lithium (S)-2-hydroxypropionate and 1g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionate and potassium oxonate; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 151.3g of modified water glass binder.

[0178] 2) Preparation of liquid inorganic two-component adhesive:

[0179] To 100 g of the modified water glass prepared in step 1), 3 g of propylene glycol diisopropyl ether and 3 g of (3-glycidoxypropyl) trimethoxysilane were added, and after stirring, 8 g of polyaspartic acid and 4 g of a one-component medium-temperature curing epoxy resin were added, and mixed evenly to obtain 118 g of a liquid of an inorganic two-component adhesive. The mixing temperature of the above mixing process was 25° C., and the stirring rate was 800 rpm.

[0180] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0181] Example 7

[0182] 1) Preparation of modified water glass:

[0183] Add 0.3g of lithium (S)-2-hydroxypropionate and 0.3g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionate and potassium oxonate; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.6g of modified water glass binder.

[0184] 2) Preparation of liquid inorganic two-component adhesive:

[0185] Add 1g of polyethylene glycol, 1g of xylitol and 4g of (3-glycidoxypropyl) trimethoxysilane to 100g of the modified water glass prepared in step 1), stir evenly, then add 0.5g of castor oil fatty acid and 1g of epoxy-modified silicone oil, stir evenly, then add 2g of acrylic acid-maleic anhydride copolymer and 2g of one-component medium-temperature curing epoxy resin, mix evenly, and obtain 111.5g of a liquid of an inorganic two-component adhesive. The mixing temperature of the above mixing process is 25°C and the stirring rate is 800rpm.

[0186] 3) Use microsilica powder as a powder of an inorganic two-component binder.

[0187] Example 8

[0188] 1) Preparation of modified water glass:

[0189] Add 0.5g of lithium (S)-2-hydroxypropionic acid and 0.15g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.65g of modified water glass binder.

[0190] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0191] 3) Preparation of powder of inorganic two-component binder:

[0192] 1 g of epoxy resin powder and 2 g of carboxylated cellulose nano whisker powder were added to 100 g of microsilica powder, and stirred until the powders were evenly dispersed to obtain 103 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0193] Example 9

[0194] 1) Preparation of modified water glass:

[0195] Add 0.3g of lithium (S)-2-hydroxypropionic acid and 0.15g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.45g of modified water glass binder.

[0196] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0197] 3) Preparation of powder of inorganic two-component binder:

[0198] 2 g of epoxy resin powder and 4 g of sulfonated cellulose nano whisker powder were added to 100 g of microsilica powder, and stirred until the powder was evenly dispersed to obtain 106 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0199] Example 10

[0200] 1) Preparation of modified water glass:

[0201] Add 0.3g of lithium (S)-2-hydroxypropionic acid and 0.1g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.4g of modified water glass binder.

[0202] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0203] 3) Preparation of powder of inorganic two-component binder:

[0204] 2 g of epoxy resin powder, 4 g of carboxylated cellulose nano whisker powder and 4 g of polytetrafluoroethylene were added to 100 g of microsilica powder, and stirred until the powder was evenly dispersed to obtain 110 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0205] Embodiment 11

[0206] 1) Preparation of modified water glass:

[0207] Add 0.3g of lithium (S)-2-hydroxypropionate and 1g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionate and potassium oxonate; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 151.3g of modified water glass binder.

[0208] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0209] 3) Preparation of powder of inorganic two-component binder:

[0210] 2 g of epoxy resin powder, 4 g of cellulose nano whisker powder and 6 g of molybdenum disulfide were added to 100 g of microsilica powder and stirred until the powder was evenly dispersed to obtain 112 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0211] Example 12

[0212] 1) Preparation of modified water glass:

[0213] Add 1g of lithium (S)-2-hydroxypropionate and 1g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionate and potassium oxonate; then add 57g of sodium silicate, stir until the sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 152g of modified water glass binder.

[0214] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0215] 3) Preparation of powder of inorganic two-component binder:

[0216] 2 g of epoxy resin powder, 6 g of carboxylated cellulose nano whisker powder and 2 g of zinc carbonate powder were added to 100 g of microsilica powder and stirred until the powder was evenly dispersed to obtain 110 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0217] Embodiment 13

[0218] 1) Preparation of modified water glass:

[0219] Add 0.5g of lithium (S)-2-hydroxypropionic acid and 1.5g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 152g of modified water glass binder.

[0220] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0221] 3) Preparation of powder of inorganic two-component binder:

[0222] 2 g of epoxy resin powder, 4 g of carboxylated cellulose nano whisker powder and 4 g of sodium carbonate powder were added to 100 g of microsilica powder and stirred until the powder was evenly dispersed to obtain 110 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0223] Embodiment 14

[0224] 1) Preparation of modified water glass:

[0225] Add 0.3g of lithium (S)-2-hydroxypropionic acid and 0.15g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.45g of modified water glass binder.

[0226] 2) Using the modified water glass in step 1) as a liquid agent of an inorganic two-component adhesive.

[0227] 3) Preparation of powder of inorganic two-component binder:

[0228] 2 g of epoxy resin powder, 4 g of carboxylated cellulose nano whisker powder, 4 g of polytetrafluoroethylene and 2 g of zinc carbonate powder were added to 100 g of microsilica powder and stirred until the powder was evenly dispersed to obtain 112 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0229] Embodiment 15

[0230] 1) Preparation of modified water glass:

[0231] Add 0.3g of lithium (S)-2-hydroxypropionic acid and 0.15g of potassium oxonate to 93g of water, stir until lithium (S)-2-hydroxypropionic acid and potassium oxonate; then add 57g of sodium silicate, stir until sodium silicate is dissolved, and obtain a mixed solution. The mixing temperature of the above mixing process is 25°C, and the stirring rate is 800rpm. Add the mixed solution to a hydrothermal reactor, and hydrothermally react at 150°C for 10h to obtain 150.45g of modified water glass binder.

[0232] 2) Preparation of liquid inorganic two-component adhesive:

[0233] To 100g of the modified water glass prepared in step 1), 1g of polyethylene glycol, 1g of propylene glycol monoisopropyl ether, 0.5g of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and 2g of (3-epoxypropoxypropyl)trimethoxysilane were added, and 0.4g of castor oil fatty acid and 1g of epoxy-modified silicone oil were added after stirring, and 1g of polyacrylic acid and 2g of single-component medium-temperature curing epoxy resin were added after stirring, and mixed evenly to obtain 108.9g of a liquid of a composite reinforced inorganic two-component adhesive. The mixing temperature of the above mixing process was 25°C and the stirring rate was 800rpm.

[0234] 3) Preparation of powder of inorganic two-component binder:

[0235] 2 g of epoxy resin powder, 4 g of carboxylated cellulose nano whisker powder, 4 g of polytetrafluoroethylene and 2 g of zinc carbonate powder were added to 100 g of microsilica powder and stirred until the powder was evenly dispersed to obtain 112 g of composite reinforced inorganic two-component binder powder. The stirring rate of the above mixing process was 800 rpm.

[0236] The binder prepared in each embodiment and comparative example is used to further prepare an inorganic sand mixture, and then the inorganic sand block sample is obtained by combining with the preparation process of the inorganic sand core. The performance test of the prepared inorganic sand block sample is carried out to examine the performance of the corresponding binder. The specific method is as follows:

[0237] Weigh 2.5kg of 50 / 100 mesh Dalin standard sand and put it into the sand mixer, weigh 50g of the single-component water glass binder prepared in Comparative Example 1, add the mixed enhanced inorganic binder to the standard sand while mixing the sand, and mix the sand for 1 minute to obtain inorganic sand. Put the mixed inorganic sand into the new hot air-warm core box composite hardening process sample machine, blow the inorganic sand from the sand storage tank into the mold with normal temperature air, the sand shooting time is 2s, and then, under the condition of the mold temperature of 180℃, continue to pass hot air into the mold for 40s (hot air temperature 120℃, pressure 4bar), so that the mixed enhanced water glass inorganic binder is cured to obtain strip inorganic sand blocks, cylindrical inorganic sand blocks and curved inorganic sand blocks, and the strip inorganic sand blocks are tested for bending strength, the cylindrical inorganic sand blocks are tested for disintegration, and the curved inorganic sand blocks are tested for fluidity.

[0238] Weigh 2.5 kg of 50 / 100 mesh Dalin standard sand and put it into a sand mixer, weigh 15 g of the powder of the inorganic two-component binder prepared in Comparative Example 2, add the powder to the standard sand while mixing the sand, and mix the sand for 1 minute. Then weigh 50 g of the water glass binder prepared in Comparative Example 2, add the liquid to the standard sand while mixing the sand, and mix the sand for 1 minute to obtain an inorganic sand mixture. The mixed sand is placed in a new hot air-warm core box composite hardening process sample machine, and the inorganic sand mixture is blown from the sand storage tank into the mold with air at room temperature. The sand shooting time is 2s, and then hot air is continuously introduced into the mold for 40s (hot air temperature 120°C, pressure 4bar) under the condition that the mold temperature is 180°C to solidify the binder to obtain a number of strip inorganic sand block samples, cylindrical inorganic sand block samples and curved inorganic sand block samples. The strip inorganic sand block samples are tested for bending strength, the cylindrical inorganic sand block samples are tested for disintegration, and the curved inorganic sand block samples are tested for fluidity. Repeat the above steps, replace the liquid and powder of the inorganic two-component binder prepared in the above comparative example 2 with the liquid and powder of the inorganic two-component binder prepared in comparative examples 3 to 4, respectively, to obtain the corresponding inorganic sand block samples.

[0239] Weigh 2.5 kg of 50 / 100 mesh Dalin standard sand and put it into a sand mixer, weigh 15 g of the powder of the inorganic two-component binder prepared in Example 1, add the powder to the standard sand while mixing the sand, and mix the sand for 1 minute. Then weigh 50 g of the liquid of the inorganic two-component binder prepared in Example 1, add the liquid to the standard sand while mixing the sand, and mix the sand for 1 minute to obtain an inorganic sand mixture. The mixed sand is placed in a new hot air-warm core box composite hardening process sample machine, and the inorganic sand mixture is blown from the sand storage tank into the mold with air at room temperature. The sand shooting time is 2s, and then hot air is continuously introduced into the mold for 40s (hot air temperature 120°C, pressure 4bar) under the condition that the mold temperature is 180°C to solidify the binder to obtain a number of strip inorganic sand block samples, cylindrical inorganic sand block samples and curved inorganic sand block samples. The strip inorganic sand block samples are tested for bending strength, the cylindrical inorganic sand block samples are tested for disintegrability, and the curved inorganic sand block samples are tested for fluidity. Repeat the above steps, replace the liquid and powder of the inorganic two-component binder prepared in the above Example 1 with the liquid and powder of the inorganic two-component binder prepared in Examples 2 to 17, respectively, to obtain the corresponding inorganic sand block samples.

[0240] Specifically, the bending strength of the strip inorganic sand block specimens was tested at 30 seconds and at 25° C., 20% RH humidity environment for 1 hour and 24 hours.

[0241] The bending strength of the inorganic sand strips was tested at 25° C. and 80% RH for 1 day, 3 days, 5 days and 7 days. The higher the bending strength, the better the moisture absorption resistance.

[0242] The compressive strength of the cylindrical inorganic sand block was tested by placing it at 25℃ for 1 hour, wrapping it with aluminum foil, and then placing it in a 710℃ resistance furnace for 5 minutes. The sand sample was taken out and cooled to room temperature. The lower the compressive strength of the cylindrical inorganic sand block, the better the collapsibility.

[0243] The curved inorganic sand block sample is used to test the fluidity of the inorganic sand mixture. If the fluidity of the inorganic sand mixture is not good, the sand will not be able to fill the entire curved mold. At the same time, if the fluidity of the inorganic sand mixture is not good, the air will make a hole in the middle of the sand, and the sand next to it cannot fall, and the compactness of the sand in the sand block sample is also low. Therefore, the higher the degree of filling of the curved mold and the higher the compactness of the sand in the sand block, the better the fluidity of the inorganic sand mixture. In the embodiment of the present application, the standard for assessing the fluidity of the inorganic sand is that if the inorganic sand fills the curved mold, it is a qualified curved sample, and if it is not filled, it is an unqualified curved sample. The qualified rate is calculated. The higher the qualified rate and the more total roots, the better the fluidity of the inorganic sand mixture.

[0244] In the above test, the new hot air-warm core box composite hardening process sample machine is an inorganic sample machine sold by Suzhou Ailid Intelligent Equipment Co., Ltd., model IWJ01. The standard sand used is a special foundry sand with certain particle size, dust content and humidity requirements. The standard sand can also be replaced by sand that meets the casting standards with other indicators.

[0245] The fluidity test results of each inorganic sand block sample are shown in Table 1, and the bending strength test results are shown in Figure 1 , Figure 2 The test results of moisture absorption resistance are shown in Figure 3 , Figure 4 The test results of collapsibility are shown in Figure 5 , Figure 6 shown.

[0246] Table 1 Sand block sample fluidity test results

[0247]

[0248]

[0249] like Figure 5 As shown, the difference between Comparative Example 2 and Comparative Example 1 is that microsilica powder is added to form a two-component binder. The experimental results show that after using the two-component binder, the cold strength of the sand core at 1h and 24h is significantly improved. This shows that the two-component binder can improve the bonding strength of inorganic sand compared to the single-component binder.

[0250] like Figure 6 As shown, the difference between Comparative Examples 3 and 4 and Comparative Example 2 is that the liquid binder is replaced by modified water glass. The experimental results show that after using modified water glass, the 30s hot strength and 1h and 24h cold strength of the sand core are significantly improved. This shows that modified water glass can improve the curing speed and bonding strength of inorganic sand.

[0251] like Figure 7 , Figure 8 , Fig. 9 As shown, compared with Example 3, the difference between Examples 1 and 2 is that polyols and silane coupling agents are added to the liquid of the inorganic two-component binder. The experimental results show that after adding polyols and silane coupling agents, the 30s hot strength, 1h and 24h cold strength and residual strength of the sand core after 7 days of storage have been significantly improved, and the residual strength has been significantly reduced. It shows that the addition of polyols and silane coupling agents can greatly improve the curing speed, bonding strength, moisture absorption resistance and collapse of inorganic sand.

[0252] As shown in Table 1, the difference between Examples 3 and 4 and Examples 1 and 2 is that surfactants and modified silicone oils are added to the liquid of the inorganic two-component binder. The experimental results show that after adding surfactants and modified silicone oils, the number and qualified rate of the prepared qualified curved specimens are significantly improved. This shows that the addition of surfactants and modified silicone oils can greatly improve the fluidity of inorganic sand, and the improved fluidity increases the sand shooting amount of the instrument, which is of great significance for the realization of mechanized sand shooting.

[0253] like Fig.10 , Fig.11 , Fig.12 As shown, compared with Examples 1 and 2, Examples 5 and 6 differ in that a chelating agent and a resin are added to the liquid of the inorganic two-component binder. The experimental results show that after adding the chelating agent and the resin, the 30s hot strength, 1h and 24h cold strength and the residual strength after 7 days of storage of the sand core are significantly improved, and the residual strength is significantly decreased. This shows that the addition of the chelating agent and the resin can greatly improve the curing speed, bonding strength, moisture absorption resistance and collapsibility of the inorganic sand.

[0254] As shown in Table 1, Fig.13 , Fig.14 , Fig.15 As shown, compared with Comparative Example 3, Example 7 is different in that polyols, silane coupling agents, surfactants, modified silicone oils, chelating agents and resins are added to the liquid of the inorganic two-component adhesive. The experimental results show that after adding surfactants and modified silicone oils, the number of qualified curved specimens prepared and the qualified rate have been significantly improved. It is shown that the addition of surfactants and modified silicone oils can greatly improve the fluidity of inorganic sand, and the improved fluidity increases the amount of sand shooting of the instrument, which is of great significance for the realization of mechanized sand shooting. After adding polyols, silane coupling agents, chelating agents and resins, the 30s hot strength of the sand core, the cold strength of 1h and 24h and the residual strength of storage for 7 days have been significantly improved, and the residual strength has been significantly reduced. It is shown that the coordinated addition of polyols, silane coupling agents, chelating agents and resins can greatly improve the curing speed, bonding strength, moisture absorption resistance and disintegration of inorganic sand.

[0255] like Fig.16 As shown, compared with Example 3, the difference between Examples 8 and 9 is that epoxy resin powder and nanocellulose whisker powder are added to the powder of the inorganic two-component binder. The experimental results show that after adding the chelating agent, the 30s hot strength and 1h and 24h cold strength of the sand core are significantly improved. This shows that the addition of the chelating agent can greatly improve the curing speed and bonding strength of the inorganic sand.

[0256] As shown in Table 1, the difference between Examples 10 and 11 and Examples 8 and 9 is that a solid lubricant is added to the powder of the inorganic two-component binder. The experimental results show that after adding the solid lubricant, the number and qualified rate of the prepared qualified curved specimens are significantly improved. This shows that the addition of solid lubricants can greatly improve the fluidity of inorganic sand, and the improved fluidity increases the sand shooting amount of the instrument, which is of great significance for the realization of mechanized sand shooting.

[0257] like Fig.17 As shown, the difference between Examples 12 and 13 and Comparative Example 3 is that a powder disintegrating agent is added to the powder of the inorganic two-component binder. The experimental results show that after adding the powder disintegrating agent, the residual strength of the sand core has been significantly reduced. This shows that the addition of the powder disintegrating agent can greatly improve the disintegration of the inorganic sand.

[0258] As shown in Table 1, Fig.18 , Fig.19 As shown, compared with Comparative Example 3, Example 14 differs in that epoxy resin powder, nanocellulose whisker powder, solid lubricant and powder disintegrator are added to the powder of the inorganic two-component binder. The experimental results show that after adding the solid lubricant, the number of qualified curved specimens prepared and the qualified rate are significantly improved. It is shown that the addition of solid lubricant can greatly improve the fluidity of inorganic sand, and the improved fluidity increases the sand shooting amount of the instrument, which is of great significance for realizing mechanized sand shooting. After adding epoxy resin powder, nanocellulose whisker powder and powder disintegrator, the 30s hot strength, 1h and 24h cold strength of the sand core are significantly improved, and the residual strength is significantly decreased. It is shown that the coordinated addition of epoxy resin powder, nanocellulose whisker powder and powder disintegrator can greatly improve the curing speed, bonding strength and disintegration of inorganic sand.

[0259] As shown in Table 1, Fig. 20 , Fig.21 , Fig. 22As shown, compared with Comparative Example 3, Example 15 differs in that polyols, silane coupling agents, surfactants, modified silicone oils, chelating agents and resins are added to the liquid of the inorganic two-component binder, and epoxy resin powder, nanocellulose whisker powder, solid lubricants and powder disintegrating agents are added to the powder of the inorganic two-component binder. The experimental results show that after adding surfactants, modified silicone oils and solid lubricants, the number and qualified rate of the prepared qualified curved specimens have been significantly improved. It is shown that the addition of solid lubricants can greatly improve the fluidity of inorganic sand, and the improved fluidity increases the amount of sand shooting of the instrument, which is of great significance for realizing mechanized sand shooting. After adding polyols, silane coupling agents, chelating agents, resins, epoxy resin powders, nanocellulose whisker powders and powder disintegrating agents, the 30s hot strength, 1h and 24h cold strength and residual strength after storage for 7 days of the sand core have been significantly improved, and the residual strength has been significantly reduced. It shows that the addition of polyols, silane coupling agents, chelating agents and resins can greatly improve the curing speed, bonding strength, moisture absorption resistance and disintegration of inorganic sand.

[0260] In summary, the composite reinforced inorganic two-component binder provided in the present application can greatly improve the curing speed, strength, fluidity, disintegration and anti-hygroscopicity of inorganic sand. It has broad application prospects in the field of inorganic sand and is of great significance for realizing mechanized sand shooting production and tailings recycling.

[0261] In addition, it should be noted that in Examples 1 to 15, the same weight of components is used to prepare liquid or powder. This is to facilitate performance comparison with comparative examples and other examples. In other embodiments of the present application, the applicant uses other weight ratios of each component to prepare liquid or powder, and obtains similar test results. Specifically, the basic formula of the liquid of the mixed enhanced inorganic water glass binder of the present application embodiment includes: 30 to 50 parts of sodium silicate powder, 0.1 to 2 parts of (S)-2-hydroxypropionic acid lithium, 0.1 to 2 parts of potassium polymetaphosphate, 0.25 to 2 parts of sodium tetraborate, 19 to 66 parts of deionized water, 0.1 to 5 parts of polyols, and 0.5 to 5 parts of silane coupling agents. The preferred formula is to further include: 0.01 to 1 parts of surfactants and 1 to 4 parts of modified silicone oils on the basis of the basic formula. Other preferred formulas are to further include: 1 to 8 parts of chelating agents and 2 to 4 parts of resins on the basis of the basic formula or the above preferred formula. The basic formula of the powder of the hybrid reinforced inorganic water glass binder of the embodiment of the present application includes: 100 parts of microsilica powder, 1-2 parts of epoxy resin powder and 2-4 parts of nanocellulose whisker powder. The preferred formula is based on the basic formula and further includes: 4-6 parts of solid lubricant. Other preferred formulas are based on the basic formula or the above preferred formula and further include: 2-4 parts of powder disintegrating agent. The components and content ranges of the above liquid / powder formulas have been verified by the applicant through a large number of performance test experiments.

[0262] The above descriptions are merely embodiments of the present application and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. An inorganic two-component adhesive, characterized in that: Including liquid and powder, including: The liquid agent includes a matrix and a first composite agent, wherein the matrix includes the following components in parts by weight: 30 to 50 parts of sodium silicate powder, 0.1 to 2 parts of (S)-2-hydroxypropionic acid lithium, 0.1 to 2 parts of potassium polymetaphosphate, 0.25 to 2 parts of sodium tetraborate, and 19 to 66 parts of deionized water; the first composite agent includes a polyol and a silane coupling agent, wherein 0.1 to 5 parts of the polyol and 0.5 to 5 parts of the silane coupling agent are added to 100 parts of the matrix, and the mixture is mixed uniformly to obtain a liquid agent A, and the liquid agent A is used as the liquid agent of the inorganic two-component adhesive; The powder comprises the following components in parts by mass: 100 parts of microsilica powder.

2. The inorganic two-component adhesive according to claim 1, characterized in that: A second composite agent is further added to the formula of the liquid, and the second composite agent includes a surfactant and a modified silicone oil; wherein, 0.01 to 1 part of a surfactant and 1 to 4 parts of modified silicone oil are added to 100 parts of the liquid A, and mixed evenly to obtain a liquid B, and the liquid B is used as the liquid of the inorganic two-component adhesive.

3. The inorganic two-component adhesive according to claim 1 or 2, characterized in that: A third compounding agent is further added to the formula of the liquid, and the third compounding agent includes a chelating agent and a resin; wherein, 1 to 8 parts of the chelating agent and 2 to 4 parts of the resin are added to 100 parts of the liquid A or 100 parts of the liquid B, and mixed evenly to obtain a liquid C, and the liquid C is used as the liquid of the inorganic two-component adhesive.

4. The inorganic two-component adhesive according to claim 1, characterized in that: The formula of the powder further comprises the following components in parts by mass: 1 to 2 parts of epoxy resin powder and 2 to 4 parts of nano-cellulose whisker powder.

5. The inorganic two-component adhesive according to claim 4, characterized in that: The formula of the powder further includes the following components in parts by weight: 4 to 6 parts of solid lubricant.

6. The inorganic two-component adhesive according to claim 4 or 5, characterized in that: The formula of the powder further includes the following components in parts by weight: 2 to 4 parts of a powder disintegrating agent.

7. The method for preparing the inorganic two-component adhesive according to claim 1, characterized in that: The following steps are involved: Preparation of S1 solution: S11: preparing a modified water glass matrix: mixing 30 to 50 parts of sodium silicate powder, 0.1 to 2 parts of (S)-2-hydroxypropionic acid lithium, 0.1 to 2 parts of potassium polymetaphosphate, 0.25 to 2 parts of sodium tetraborate and 19 to 66 parts of deionized water, and obtaining modified water glass through a hydrothermal reaction; S12: adding the first composite agent: adding 0.1 to 5 parts of polyol and 0.5 to 5 parts of silane coupling agent to 100 parts of the modified water glass prepared in step S1, mixing them evenly to obtain liquid A, and using the liquid A as the liquid of the inorganic two-component adhesive; S2 powder preparation.

8. The preparation method according to claim 7, characterized in that: The step S1 further comprises: S13 adding a second composite agent: adding 0.01 to 1 part of a surfactant and 1 to 4 parts of silicone oil to 100 parts of the liquid A prepared in step S12, mixing evenly to obtain a liquid B, and using the liquid B as the liquid of the inorganic two-component adhesive.

9. The preparation method according to claim 7 or 8, characterized in that: The step S1 further comprises: S14: adding a third compounding agent: adding 1 to 8 parts of a chelating agent and 2 to 4 parts of a resin to 100 parts of the liquid A prepared in step S12 or 100 parts of the liquid B prepared in step S13, mixing evenly to obtain a liquid C, and using the liquid C as the liquid of the inorganic two-component adhesive.

10. A method for preparing inorganic molding sand, characterized in that: The following steps are involved: Add raw sand into a sand mixer for sand mixing, add powder of inorganic two-component binder to the raw sand while mixing, and then add liquid of inorganic two-component binder after mixing evenly to obtain molding sand; wherein, the inorganic two-component binder is according to any one of claims 1 to 6; 1 to 5 parts of the liquid and 0.1 to 5 parts of the powder are added to every 100 parts of raw sand.

Citation Information

Cited By

  • Multifunctional binder for aluminum electrolysis as well as preparation method and application of multifunctional binder

    CN119931510A