Preparation method of biomass hard carbon material, biomass hard carbon material and secondary battery
By mixing biomass materials with cellulose dissolving agent, removing cellulose and pre-oxidizing carbonization treatment, hard carbon materials with high specific capacity and energy density are prepared, which solves the problem of insufficient performance of hard carbon materials in the prior art. in high-performance sodium ion batteries.
Patent Information
- Application Number
- CN202410983026.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
AI Technical Summary
In the prior art, the specific capacity and energy density of biomass hard carbon materials are relatively low, which limits the performance of sodium ion batteries.
By mixing the biomass material with a cellulose dissolving agent, removing cellulose, pre-oxidizing and carbonizing treatment, a hard carbon material with rich closed-cell structure is prepared to increase its specific capacity and energy density.
It improves the specific capacity and energy density of hard carbon materials, reduces production costs, simplifies the process flow, enhances electrochemical performance, and is suitable for high-performance sodium ion battery negative electrode materials.
Smart Images

Figure CN118929622A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field related to secondary batteries, and more specifically, relates to a method for preparing a biomass hard carbon material, a biomass hard carbon material and a secondary battery. Background Art
[0002] Sodium-ion batteries have been considered as one of the effective alternatives to lithium-ion batteries due to the abundance of sodium. However, their large-scale application is limited by problems such as low power density and energy density. The preparation of high-performance sodium-ion batteries mainly depends on negative electrode materials. Graphite-based negative electrode materials are widely used in sodium-ion battery negative electrode materials, such as artificial graphite and natural graphite. Other types of negative electrode materials such as lithium titanate, soft carbon, and hard carbon are also the main negative electrode materials for sodium-ion batteries. Among them, hard carbon refers to carbon that is difficult to graphitize. It is a pyrolytic carbon obtained by pyrolysis of polymers, petrochemical products, biomass, etc. Hard carbon is a representative negative electrode candidate material. Although the sodium storage mechanism of hard carbon is controversial, there is no doubt that the platform capacity is the main source of sodium storage capacity, and the platform capacity is highly correlated with the pore structure, so adjusting the pore structure is the top priority in the development of high-performance hard carbon materials.
[0003] In the prior art, the main production process for obtaining porous hard carbon materials using biomass raw materials is direct pyrolysis and carbonization. The hard carbon materials processed by the prior preparation process have low specific capacity and energy density. Summary of the invention
[0004] In response to the above defects or improvement needs of the prior art, the present invention provides a method for preparing a biomass hard carbon material, a biomass hard carbon material and a secondary battery, which solves the problem of low specific capacity and energy density of hard carbon materials processed by existing preparation processes. The prepared hard carbon has lower charge transfer resistance and higher ion diffusion rate, and the half-cell specific capacity is high.
[0005] To achieve the above object, according to a first aspect of the present invention, a method for preparing a biomass hard carbon material is provided, comprising:
[0006] S1, drying and dehydrating the biomass material, and crushing it into biomass powder;
[0007] S2, mixing the biomass powder with a cellulose dissolving agent to remove cellulose from the biomass powder to form a biomass slurry;
[0008] S3, removing the cellulose dissolving agent in the biomass slurry to obtain biomass secondary powder;
[0009] S4, pre-oxidizing the biomass secondary powder in an air atmosphere to stabilize the structure, and obtaining pre-oxidized powder;
[0010] S5, carbonizing the pre-oxidized powder to obtain a biomass hard carbon material.
[0011] According to a second aspect of the present invention, there is provided a biomass hard carbon material, which is prepared by any of the above-mentioned methods for preparing a biomass hard carbon material.
[0012] According to a third aspect of the present invention, there is provided a secondary battery, comprising an electrode plate, wherein the electrode plate comprises a current collector and the above-mentioned biomass hard carbon material, wherein the biomass hard carbon material is coated on the current collector.
[0013] In general, compared with the prior art, the above technical solutions conceived by the present invention mainly have the following beneficial effects:
[0014] 1. A cellulose dissolving agent is used to dissolve the cellulose in the biomass in a directional manner. By dissolving the cellulose in the material, the biomass structure can be reorganized to increase the disorder of the material; by removing cellulose from the biomass to expose the free radicals in lignin and hemicellulose, the abundance of closed pores in the hard carbon material after pyrolysis and carbonization can be regulated, so that the hard carbon material has a rich closed-pore structure; at the same time, exposing a large number of free radicals during the pyrolysis and carbonization process can improve the efficiency of small molecules and acute free radical reactions, thereby increasing the efficiency of the pyrolysis process, and ultimately achieving the effect of increasing the closed-pore ratio and exposing active sites after carbonization; so that the prepared biomass hard carbon material negative electrode has a higher specific capacity and energy density;
[0015] 2. At the same time, in the process of dissolving cellulose in biomass by cellulose dissolving agent, a small amount of heteroatoms in the dissolving agent can be incorporated into the biomass precursor, i.e., biomass. When the biomass hard carbon material is used in sodium ion batteries, it is helpful to assist the adsorption of sodium ions and further increase the specific capacity;
[0016] 3. The provided dissolution method can increase the dissolution efficiency in biomass materials, increase the amount of cellulose dissolved, and help increase the disorder of the material, and expose free radicals to a greater extent, so that the prepared hard carbon material has a rich closed-pore structure and improves the specific capacity;
[0017] 4. By rotary evaporating the biomass slurry and connecting the tail end with a condensing device, the cellulose dissolving agent can be recovered, which greatly reduces the production cost;
[0018] 5. The method for preparing biomass hard carbon materials shortens the firing time of the traditional hard carbon material preparation process, optimizes the electrochemical properties of the material, reduces the production cost, and increases the specific capacity of the half-cell; the process has commercial value because of its simple method, low cost, and the drugs used to treat biomass materials can be recycled and reused;
[0019] 6. The designed preparation method can be applied to a variety of biomass, is simple to operate, and has the potential for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a comparison diagram of different dissolution methods of Example 1 and Comparative Example 1;
[0021] Figure 2 It is a comparison diagram of different dissolution methods of Example 2 and Comparative Example 2;
[0022] Figure 3 It is a comparison diagram of different dissolution methods of Example 3 and Comparative Example 3;
[0023] Figure 4 The SEM images of Examples 4-6 and Comparative Examples 4-6 are shown;
[0024] Figure 5 TEM images of Examples 4-6 and Comparative Examples 4-6;
[0025] Figure 6 The XRD diagram of the powder after dissolution and evaporation of Example 4-6 and Comparative Example 4-6;
[0026] Figure 7 It is the EIS graph of Examples 4-6 and Comparative Example 4;
[0027] Figure 8 The cycle performance diagram of Examples 4-6 and Comparative Examples 4-6 at 0.001-2.5V, 1C;
[0028] Fig. 9 The cycle performance diagrams of Example 7 and Comparative Examples 9 and 10 at 0.001-2.5V, 1C;
[0029] Fig.10 The cycle performance diagram of Example 8 and Comparative Examples 11 and 12 at 0.001-2.5V, 1C;
[0030] Fig.11 The cycle performance diagrams of Example 9 and Comparative Examples 13 and 14 at 0.001-2.5V, 1C;
[0031] Fig.12 The cycle performance diagram of Example 10 and Comparative Examples 15 and 16 at 0.001-2.5V, 1C;
[0032] Fig.13 The cycle performance diagrams of Example 4 and Comparative Examples 17 and 18 at 0.001-2.5V, 1C;
[0033] Fig.14 The cycle performance diagrams of Example 4 and Comparative Examples 19 and 20 at 0.001-2.5V, 1C;
[0034] Fig.15 The cycle performance diagram of Example 4 and Comparative Example 21 at 0.001-2.5V, 1C;
[0035] Fig.16 The cycle performance diagram of Example 5 and Comparative Example 22 at 0.001-2.5V, 1C;
[0036] Fig.17 The cycle performance diagram of Example 6 and Comparative Example 23 at 0.001-2.5V, 1C;
[0037] Fig.18 The cycle performance diagram of Example 7 and Comparative Example 24 at 0.001-2.5V, 1C;
[0038] Fig.19 The cycle performance diagram of Example 8 and Comparative Example 25 at 0.001-2.5V, 1C;
[0039] Fig. 20 The cycle performance diagram of Example 9 and Comparative Example 26 at 0.001-2.5V, 1C;
[0040] Fig.21 The cycle performance diagram of Example 10 and Comparative Example 27 at 0.001-2.5V, 1C;
[0041] Fig. 22 The cycle performance diagram of Example 4 and Comparative Examples 7 and 8 at 0.001-2.5V, 1C. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0043] This embodiment 1 provides a method for preparing a biomass hard carbon material, the preparation method comprising:
[0044] S1, drying and dehydrating the biomass material, and crushing it into biomass powder;
[0045] S2, mixing the biomass powder with a cellulose dissolving agent to remove cellulose from the biomass powder to form a biomass slurry;
[0046] S3, removing the cellulose dissolving agent in the biomass slurry to obtain biomass secondary powder;
[0047] S4, pre-oxidizing the biomass secondary powder in an air atmosphere to stabilize the structure, and obtaining pre-oxidized powder; the pre-oxidation is to heat the biomass secondary powder in an air atmosphere to stabilize the structure formed in the above steps;
[0048] S5, carbonizing the pre-oxidized powder to obtain a biomass hard carbon material.
[0049] This embodiment takes into account that among the various precursors for preparing hard carbon, lignocellulosic biomass has an innate cross-linked structure, which originates from the bonding of structural biomacromolecules such as cellulose, hemicellulose and lignin, and this structure enables the biomass to be precisely modified at the molecular level to adjust the closed-pore structure in the hard carbon. On this basis, by adjusting the ratio of crystalline (cellulose) to amorphous (hemicellulose / lignin) components in the precursor, it is found that cellulose with high crystallinity tends to be converted into long graphite layers, while the amorphous part plays a role in preventing excessive graphitization of the carbon layer. Based on this, this embodiment proposes a method for preparing a hard carbon material by modifying a hard carbon precursor to adjust the closed-pore structure, starting from the mechanism of closed-pore formation at the molecular level.
[0050] The preparation method adopts a cellulose dissolving agent to directionally dissolve cellulose in biomass. By dissolving the cellulose in the material, the biomass structure can be reorganized to increase the disorder of the material; by removing cellulose from the biomass to expose free radicals in lignin and hemicellulose, the abundance of closed pores in the hard carbon material after pyrolysis and carbonization can be regulated, so that the hard carbon material has a rich closed-pore structure; at the same time, exposing a large number of free radicals during the pyrolysis and carbonization process can improve the efficiency of small molecules and acute free radical reactions, thereby increasing the efficiency of the pyrolysis process, and ultimately achieving the effect of increasing the closed-pore ratio and exposing active sites after carbonization; so that the prepared biomass hard carbon material negative electrode has a higher specific capacity and energy density.
[0051] At the same time, in the process of cellulose solvent dissolving cellulose in biomass, a small amount of heteroatoms in the solvent can be incorporated into the biomass precursor, i.e., biomass. When the biomass hard carbon material is used in sodium ion batteries, it is helpful to assist the adsorption of sodium ions and further increase the specific capacity.
[0052] This embodiment proposes a molecular structure design strategy for hard carbon materials. The free radical reaction in the biomass precursor can be enhanced by directional dissolution of cellulose, thereby forming an ideal abundance and structure of closed pores in the hard carbon material, thereby improving the performance of the hard carbon material.
[0053] S2 specifically includes: mixing the biomass powder with the cellulose dissolving agent, first heating and stirring, then stirring in an ice bath, and finally standing at room temperature. This embodiment proposes a new method for dissolving cellulose in biomass, specifically using a cellulose dissolving agent to stir and mix with the biomass powder under heating conditions. The heating and stirring can make the biomass powder and the dissolving agent fully and evenly mixed, and is conducive to the penetration of the dissolving agent into the molecules of the biomass powder, thereby facilitating a better removal effect of the cellulose on the surface and inside of the biomass; then this embodiment has found through research that as the temperature decreases, the solubility of the cellulose dissolving agent will increase, so it is proposed that stirring can be carried out under ice bath conditions, that is, lowering the temperature to below zero degrees for stirring, which is conducive to increasing the solubility of the dissolving agent and dissolving the cellulose more fully and completely; then standing at room temperature to restore the slurry to room temperature, that is, about 25°C.
[0054] The dissolution method provided in this embodiment can increase the dissolution efficiency in biomass materials, increase the amount of cellulose dissolved, which is beneficial to increasing the disorder of the material, and expose free radicals to a greater extent, so that the prepared hard carbon material has a rich closed-pore structure and improved specific capacity.
[0055] S3 specifically includes: performing rotary evaporation on the biomass slurry, and connecting a condensation device at the tail end to recover the cellulose dissolving agent. This embodiment proposes to recover the cellulose dissolving agent by rotary evaporation and connecting a condensation device at the tail end, which is beneficial to reducing production costs. The use of rotary evaporation is beneficial to the uniform dispersion of the cellulose dissolving agent, and thus to its full recovery.
[0056] The method for preparing biomass hard carbon materials provided in this embodiment shortens the firing time of the traditional hard carbon material preparation process, optimizes the electrochemical properties of the material, reduces the production cost, and improves the specific capacity of the half-cell; the process has commercial value because of its simplicity, low cost, and the chemicals used to treat biomass materials can be recycled and reused.
[0057] Furthermore, the range of the rotary evaporation speed R is 300rpm≤R≤600rpm; the range of the rotary evaporation temperature T is 80℃≤T≤120℃; the range of the rotary evaporation time t is 4h≤t≤24h; and the condensation system at the tail end is similar to a conventional distillation condensation system.
[0058] S5 specifically includes:
[0059] The pre-oxidized powder is firstly pre-carbonized in an inert atmosphere;
[0060] The pre-carbonized powder is naturally cooled to room temperature, immersed in acid solution for pickling, and then filtered and dried;
[0061] The powder obtained after filtration and drying is carbonized under an inert atmosphere, and then naturally cooled to room temperature to obtain a biomass hard carbon material;
[0062] The temperature of pre-carbonization is lower than the temperature of carbonization. Pre-oxidation, pre-carbonization and carbonization can be performed in a tube furnace. Pre-carbonization is beneficial to increase the carbon yield of the hard carbon material after carbonization; acid washing can remove trace metal elements in biomass, thereby improving the performance of the hard carbon material. The acid in the material after acid washing can be removed by filtration.
[0063] Specifically, the cellulose dissolving agent is at least one of tetrabutylammonium hydroxide solution, tetrabutylammonium fluoride solution and tetrabutylammonium sulfate solution; one of the above solutions can be used, or a mixture of two or three can be used to dissolve the cellulose.
[0064] And / or, the temperature range of heating and stirring in S2 is 30°C-50°C, and the time range of heating and stirring is 0.5h-6h; the temperature range of ice bath stirring is -5°C--25°C, and the time range of ice bath stirring is 1h-3h; the time range of standing at room temperature is 0.5h-2h. The temperature of ice bath stirring should be higher than the solidification point of the cellulose dissolving agent.
[0065] Furthermore, when the cellulose dissolving agent is a combination of two of the above solutions, the ratio of the two solutions is 2:3-7:3; when the cellulose dissolving agent is a combination of three of the above solutions, the ratio of tetrabutylammonium hydroxide solution, tetrabutylammonium fluoride solution and tetrabutylammonium sulfate solution is 7:7:6 or 3:3:4 or 2:2:1;
[0066] And / or, the mass fraction of the tetrabutylammonium hydroxide solution, the tetrabutylammonium fluoride solution and the tetrabutylammonium sulfate solution is 40%-70%.
[0067] Specifically, when the cellulose dissolving agent is a combination of tetrabutylammonium hydroxide solution and tetrabutylammonium sulfate solution, the mixing ratio of the tetrabutylammonium hydroxide solution and the tetrabutylammonium sulfate solution is 2:3-7:3; preferably, the mixing ratio of the tetrabutylammonium hydroxide solution and the tetrabutylammonium sulfate solution is 3:2.
[0068] When the cellulose dissolving agent is a combination of tetrabutylammonium hydroxide solution and tetrabutylammonium fluoride solution, the mixing ratio of the tetrabutylammonium hydroxide solution and the tetrabutylammonium fluoride solution is 2:3-7:3; preferably, the mixing ratio of the tetrabutylammonium hydroxide solution and the tetrabutylammonium fluoride solution is 1:1.
[0069] When the cellulose dissolving agent is a combination of tetrabutylammonium fluoride solution and tetrabutylammonium sulfate solution, the mixing ratio of the tetrabutylammonium fluoride solution and the tetrabutylammonium sulfate solution is 2:3-7:3; preferably, the mixing ratio of the tetrabutylammonium fluoride solution and the tetrabutylammonium sulfate solution is 3:2.
[0070] When the cellulose dissolving agent is a combination of tetrabutylammonium hydroxide solution, tetrabutylammonium fluoride solution and tetrabutylammonium sulfate solution, preferably, the mixing ratio of the tetrabutylammonium hydroxide solution, the tetrabutylammonium fluoride solution and the tetrabutylammonium sulfate solution is 7:7:6.
[0071] The pre-oxidation temperature range in S4 is 200°C-300°C, the pre-oxidation time range is 2h-6h, and the pre-oxidation sintering atmosphere is air;
[0072] After the pre-oxidation is completed, the atmosphere in the tube furnace is converted to an inert gas, and the inert gas is nitrogen or argon, and a pre-carbonization treatment is performed; the pre-carbonization temperature range in S5 is 500°C-900°C, and the pre-carbonization time range is 0.5h-6h. After the intermediate is cooled to room temperature after pre-carbonization, it is pickled, and the acid solution is at least one of sulfuric acid, nitric acid and hydrochloric acid, and the acid solution concentration M ranges from 0.5mol / L≤M≤4mol / L; the pickling time ranges from 0.1h-12h; the drying temperature range after filtration is 90℃-120℃, and the drying insulation time ranges from 8h-24h.
[0073] The inert atmosphere gas during the carbonization process is one of nitrogen and argon, the carbonization temperature range is 1000° C.-1600° C., and the carbonization time range is 1 h-12 h.
[0074] Furthermore, during the pre-oxidation, pre-carbonization and carbonization processes, the biomass powder is placed in a compacted state; that is, the biomass powder is compacted and placed in a container such as a crucible, and then placed inside a tubular furnace for corresponding operations.
[0075] The type of biomass material in S1 is at least one of hardwood, softwood, walnut shell, pistachio shell, pecan shell, almond shell, almond shell, hazelnut shell, pine nut shell, chestnut shell, ginkgo shell, macadamia shell, pili shell, peanut, sunflower seed, pumpkin seed and watermelon seed. The temperature range of drying the biomass material in S1 is 90℃-20℃; the range of heat preservation time, i.e. drying time, is 24h-72h.
[0076] The second embodiment provides a biomass hard carbon material, which is prepared by any of the above-mentioned methods for preparing a biomass hard carbon material.
[0077] The third embodiment provides a secondary battery, which includes an electrode plate, wherein the electrode plate includes a current collector and the above-mentioned biomass hard carbon material, and the biomass hard carbon material is coated on the current collector. The biomass hard carbon material is an active material layer coated on the current collector. Specifically, the current collector can be an aluminum current collector, which is not specifically limited.
[0078] The following are specific examples and comparative examples. For specific comparison information, please see Table 1 below:
[0079] Table 1 List of specific examples and comparative examples
[0080]
[0081]
[0082] Example 1
[0083] Disperse 5 g of cellulose powder in 15 mL of tetrabutylammonium hydroxide aqueous solution (40 wt%), stir at 40 °C for 3 hours, then transfer to an ice bath and stir for 2 hours, and ensure that the stirring environment is maintained at about -15 °C. After stirring, transfer to room temperature and let stand for 2 hours.
[0084] The solution prepared above was compared with a liquid dissolved at room temperature.
[0085] Example 2
[0086] Disperse 5 g of cellulose powder into 15 mL of tetrabutylammonium sulfate aqueous solution (40 wt%), stir at 40 °C for 3 hours, then transfer to an ice bath and stir for 2 hours, making sure that the stirring environment remains at about -15 °C. After stirring, transfer to room temperature and let stand for 2 hours.
[0087] The solution prepared above was compared with a liquid dissolved at room temperature.
[0088] Example 3
[0089] Disperse 5 g of cellulose powder into 15 mL of tetrabutylammonium fluoride aqueous solution (40 wt%), stir at 40 °C for 3 hours, then transfer to an ice bath and stir for 2 hours, and ensure that the stirring environment is maintained at about -15 °C. After the stirring is completed, transfer to room temperature and let stand for 2 hours.
[0090] The solution prepared above was compared with a liquid dissolved at room temperature.
[0091] Example 4
[0092] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0093] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0094] Example 5
[0095] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium sulfate aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0096] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0097] Example 6
[0098] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium fluoride aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0099] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0100] Example 7
[0101] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 3:2. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0102] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0103] Example 8
[0104] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%) and tetrabutylammonium fluoride aqueous solution (40wt%), with a mass ratio of 1:1. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0105] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0106] Example 9
[0107] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium fluoride aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 3:2. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0108] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0109] Example 10
[0110] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide (40wt%), tetrabutylammonium fluoride aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 7:7:6. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at around -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0111] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0112] Comparative Example 1
[0113] 5 g of cellulose powder was dispersed in 15 mL of tetrabutylammonium hydroxide aqueous solution (40 wt%) and stirred at room temperature for 7 h.
[0114] The solution prepared above was compared with the liquid prepared by the dissolution method of the present invention.
[0115] Comparative Example 2
[0116] 5 g of cellulose powder was dispersed in 15 mL of tetrabutylammonium sulfate aqueous solution (40 wt%) and stirred at room temperature for 7 h.
[0117] The solution prepared above was compared with the liquid prepared by the dissolution method of the present invention.
[0118] Comparative Example 3
[0119] 5 g of cellulose powder was dispersed in 15 mL of tetrabutylammonium fluoride aqueous solution (40 wt%) and stirred at room temperature for 7 h.
[0120] The solution prepared above was compared with the liquid prepared by the dissolution method of the present invention.
[0121] Comparative Example 4
[0122] The hardwood material was crushed and dried at 100°C for 48 hours to dehydrate. After dehydration, the hardwood powder was placed in a conventional corundum crucible and repeatedly shaken and continuously added with hardwood powder until the volume did not change. It was sent to a tubular furnace and kept at 1400°C for 6 hours under an argon atmosphere. After naturally cooling to room temperature, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried to obtain a hard carbon material.
[0123] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0124] Comparative Example 5
[0125] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of water and 10mL of acetic acid and 5g of sodium chlorite were added and stirred at 80°C for 8h to remove lignin. After stirring, it was transferred to room temperature and allowed to stand for 2h, then centrifuged until the centrifuged waste liquid was neutral, and then dried at 100°C. The dried sample was pre-oxidized at 250°C for 4 hours in an air atmosphere to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0126] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0127] Comparative Example 6
[0128] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of water and 10g of sodium hydroxide was added and stirred at 80°C for 8h to remove cellulose. After stirring, it was transferred to room temperature and allowed to stand for 2h, then centrifuged until the centrifuged waste liquid was neutral, and then dried at 100°C. The dried sample was pre-oxidized in an air atmosphere at 250°C for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0129] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0130] Comparative Example 7
[0131] The walnut shell material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0132] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0133] Comparative Example 8
[0134] The bamboo material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0135] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0136] Comparative Example 9
[0137] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 1:1. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0138] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0139] Comparative Example 10
[0140] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 7:3. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0141] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0142] Comparative Example 11
[0143] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%) and tetrabutylammonium fluoride aqueous solution (40wt%), with a mass ratio of 3:2. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0144] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0145] Comparative Example 12
[0146] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%) and tetrabutylammonium fluoride aqueous solution (40wt%), with a mass ratio of 2:3. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0147] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0148] Comparative Example 13
[0149] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium fluoride aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 1:1. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0150] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0151] Comparative Example 14
[0152] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium fluoride aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 7:3. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material is obtained.
[0153] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0154] Comparative Example 15
[0155] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), tetrabutylammonium fluoride aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 3:3:4. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at around -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0156] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0157] Comparative Example 16
[0158] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into a mixed solution of 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), tetrabutylammonium fluoride aqueous solution (40wt%) and tetrabutylammonium sulfate aqueous solution (40wt%), with a mass ratio of 2:2:1. Stir at 40°C for 3 hours, then transfer to an ice bath for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, perform rotary evaporation at 100°C, and collect the condensed liquid at the tail. After complete evaporation, pre-oxidize at 250°C in an air atmosphere for 4 hours to ensure structural stability, then replace the gas with argon and heat to 800°C for 3 hours. After completion, wait for it to naturally drop to room temperature. Then pour into a 2mol / L hydrochloric acid solution, stir for 6 hours, and filter and dry. The acid-washed intermediate was placed in a corundum crucible and carbonized at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0159] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0160] Comparative Example 17
[0161] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 700°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0162] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0163] Comparative Example 18
[0164] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 900°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0165] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0166] Comparative Example 19
[0167] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1200°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0168] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0169] Comparative Example 20
[0170] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed in 50mL of tetrabutylammonium hydroxide aqueous solution (40wt%), first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After stirring, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The acid-washed intermediate was placed in a corundum crucible and carbonized at high temperature at 1600°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0171] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0172] Comparative Example 21
[0173] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into 50mL of the solution recovered and purified in Example 4, first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After the stirring was completed, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0174] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0175] Comparative Example 22
[0176] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into 50mL of the solution recovered and purified in Example 5, first stirred at 40°C for 3 hours, then transferred to an ice bath for stirring for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After the stirring was completed, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The intermediate after pickling was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0177] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0178] Comparative Example 23
[0179] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into 50mL of the solution recovered and purified in Example 6, first stirred at 40°C for 3 hours, then transferred to an ice bath for 2 hours, and ensured that the stirring environment was maintained at about -15°C. After the stirring was completed, it was transferred to room temperature and left to stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The intermediate after pickling was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0180] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0181] Comparative Example 24
[0182] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into 50mL of the solution recovered and purified in Example 7. Stir at 40°C for 3 hours, then transfer to an ice bath and stir for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0183] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0184] Comparative Example 25
[0185] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into 50mL of the solution recovered and purified in Example 8. Stir at 40°C for 3 hours, then transfer to an ice bath and stir for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0186] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0187] Comparative Example 26
[0188] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into 50mL of the solution recovered and purified in Example 9. Stir at 40°C for 3 hours, then transfer to an ice bath and stir for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0189] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0190] Comparative Example 27
[0191] The hardwood material was crushed and dried at 100°C for 48 hours for dehydration. After dehydration, 5g of hardwood powder was dispersed into 50mL of the solution recovered and purified in Example 10. Stir at 40°C for 3 hours, then transfer to an ice bath and stir for 2 hours, and ensure that the stirring environment is maintained at about -15°C. After stirring, transfer to room temperature and let stand for 2 hours. Then, rotary evaporation was performed at 100°C, and the condensed liquid was collected at the tail. After complete evaporation, pre-oxidation was performed at 250°C in an air atmosphere for 4 hours to ensure structural stability, and then the gas was replaced with argon and heated to 800°C for 3 hours. After completion, it was necessary to wait for it to naturally drop to room temperature. Then, it was poured into a 2mol / L hydrochloric acid solution and stirred for 6 hours, and then filtered and dried. The pickled intermediate was placed in a corundum crucible and carbonized at high temperature at 1400°C in an argon atmosphere for 6 hours. After cooling to room temperature, a hard carbon material was obtained.
[0192] The hard carbon material prepared above was used as the negative electrode material of the sodium ion battery, coated on a commercial aluminum foil to prepare a negative electrode sheet, and finally assembled with metallic sodium into a half-cell, and electrochemical testing was performed.
[0193] Comparative results analysis: Figure 1 This is a comparison chart of the dissolution method used in the present invention and the conventional dissolution method. It can be found that more cellulose can be dissolved in the tetrabutylammonium hydroxide aqueous solution using the method of the present invention (left figure).
[0194] Figure 2 This is a comparison chart of the dissolution method used in the present invention and the conventional dissolution method. It can be found that more cellulose can be dissolved in the tetrabutylammonium sulfate aqueous solution using the method of the present invention (left figure).
[0195] Figure 3 This is a comparison chart of the dissolution method used in the present invention and the conventional dissolution method. It can be found that more cellulose can be dissolved in the tetrabutylammonium fluoride aqueous solution using the method of the present invention (left figure).
[0196] Figure 4 The SEM images of Example 4-6 and Comparative Example 4-6 show that the particle sizes of the prepared samples are basically the same, and the electrochemical performance is not affected by the particle size.
[0197] Figure 5 The TEM images of Examples 4-6 and Comparative Examples 4-6 show that the samples treated with tetrabutylammonium hydroxide, tetrabutylammonium sulfate or tetrabutylammonium fluoride do not have long graphene-like sheets, but maintain a highly disordered state with a large number of closed pores. The directly sintered materials have fewer closed pores and more long graphene-like sheets; the materials treated with sodium hydroxide or acetic acid have certain closed pores relative to the untreated materials, and fewer long-range ordered graphene-like sheets.
[0198] Figure 6The XRD diagrams are of the original biomass material, the powder after dissolution and evaporation of Examples 4-6, Comparative Examples 5 and Comparative Example 6. From the peak intensity, it can be seen that the treatment with tetrabutylammonium hydroxide, tetrabutylammonium sulfate or tetrabutylammonium fluoride is more effective in dissolving cellulose.
[0199] Figure 7 EIS graphs of Example 4-6 and Comparative Example 4. The hard carbon of Example 4-6 has lower charge transfer resistance and ion diffusion coefficient, and can achieve faster charge transfer and ion migration speed during the charge and discharge process.
[0200] Figure 8 The cycle performance diagrams of Examples 4-6 and Comparative Examples 4-6 at 0.001-2.5V, 1C. The capacity of Example 4 at 1C cycle is 343mAh / g; the capacity of Example 5 at 1C cycle is 337mAh / g; the capacity of Example 6 at 1C cycle is 340mAh / g; the capacity of Comparative Example 4 at 1C cycle is 295mAh / g; the capacity of Comparative Example 5 at 1C cycle is 309mAh / g; the capacity of Comparative Example 6 at 1C cycle is 314mAh / g; It can be seen that the surface treatment by dissolving agent greatly improves the specific capacity and stability of the hard carbon material.
[0201] Fig. 9 The cycle performance diagrams of Example 7 and Comparative Examples 9 and 10 at 0.001-2.5V, 1C are shown. The capacity of Example 7 at 1C cycle is 340mAh / g; the capacity of Comparative Example 9 at 1C cycle is 327.7mAh / g; the capacity of Comparative Example 10 at 1C cycle is 332.5mAh / g; it can be seen that when tetrabutylammonium hydroxide and tetrabutylammonium sulfate are mixed in a mass ratio of 3:2, the performance is the best.
[0202] Fig.10 The cycle performance diagrams of Example 8 and Comparative Examples 11 and 12 at 0.001-2.5V, 1C are shown. The capacity of Example 8 at 1C cycle is 345mAh / g; the capacity of Comparative Example 11 at 1C cycle is 333mAh / g; the capacity of Comparative Example 12 at 1C cycle is 327mAh / g; it can be seen that when tetrabutylammonium hydroxide and tetrabutylammonium fluoride are mixed in a mass ratio of 1:1, the performance is the best.
[0203] Fig.11 The cycle performance diagrams of Example 9 and Comparative Examples 13 and 14 at 0.001-2.5V, 1C are shown. The capacity of Example 9 at 1C cycle is 342mAh / g; the capacity of Comparative Example 13 at 1C cycle is 330mAh / g; the capacity of Comparative Example 14 at 1C cycle is 335mAh / g; it can be seen that when tetrabutylammonium fluoride and tetrabutylammonium sulfate are mixed in a mass ratio of 3:2, the performance is the best.
[0204] Fig.12 The cycle performance diagrams of Example 10 and Comparative Examples 15 and 16 at 0.001-2.5V, 1C are shown. The capacity of Example 10 at 1C cycle is 348mAh / g; the capacity of Comparative Example 15 at 1C cycle is 326mAh / g; the capacity of Comparative Example 16 at 1C cycle is 332mAh / g; it can be seen that when tetrabutylammonium hydroxide, tetrabutylammonium fluoride and tetrabutylammonium sulfate are mixed in a mass ratio of 7:7:6, the performance is the best.
[0205] Fig.13 The cycle performance diagrams of Example 4 and Comparative Examples 17 and 18 at 0.001-2.5V, 1C are shown. The capacity of Example 4 at 1C cycle is 343mAh / g; the capacity of Comparative Example 17 at 1C cycle is 308mAh / g; the capacity of Comparative Example 18 at 1C cycle is 314mAh / g, proving that the best pre-carbonization temperature is 800°C.
[0206] Fig.14 The cycle performance diagrams of Example 4 and Comparative Examples 19 and 20 at 0.001-2.5V, 1C are shown. The capacity of Example 4 at 1C cycle is 343mAh / g; the capacity of Comparative Example 19 at 1C cycle is 313mAh / g; the capacity of Comparative Example 20 at 1C cycle is 329mAh / g, proving that the best carbonization temperature is 1400°C.
[0207] Fig.15 The cycle performance diagrams of Example 4 and Comparative Example 21 at 0.001-2.5V, 1C are shown. The capacity of Example 4 at 1C cycle is 343mAh / g; the capacity of Comparative Example 21 at 1C cycle is 341mAh / g, proving that the recovered and purified drugs can still effectively dissolve cellulose in biomass.
[0208] Fig.16 The cycle performance diagrams of Example 5 and Comparative Example 22 at 0.001-2.5V, 1C are shown. The capacity of Example 5 at 1C cycle is 337mAh / g; the capacity of Comparative Example 22 at 1C cycle is 339mAh / g, proving that the recovered and purified drugs can still effectively dissolve cellulose in biomass.
[0209] Fig.17 The cycle performance diagrams of Example 6 and Comparative Example 23 at 0.001-2.5V, 1C are shown. The capacity of Example 6 at 1C cycle is 340mAh / g; the capacity of Comparative Example 23 at 1C cycle is 340mAh / g, proving that the recovered and purified drugs can still effectively dissolve cellulose in biomass.
[0210] Fig.18The cycle performance diagrams of Example 7 and Comparative Example 24 at 0.001-2.5V, 1C are shown. The capacity of Example 7 at 1C cycle is 340mAh / g; the capacity of Comparative Example 24 at 1C cycle is 339mAh / g, proving that the recycled and purified mixed chemicals can still effectively dissolve cellulose in biomass.
[0211] Fig.19 The cycle performance diagrams of Example 8 and Comparative Example 25 at 0.001-2.5V, 1C are shown. The capacity of Example 8 at 1C cycle is 345mAh / g; the capacity of Comparative Example 25 at 1C cycle is 346mAh / g, proving that the recycled and purified mixed chemicals can still effectively dissolve cellulose in biomass.
[0212] Fig. 20 The cycle performance diagrams of Example 9 and Comparative Example 26 at 0.001-2.5V, 1C are shown. The capacity of Example 9 at 1C cycle is 342mAh / g; the capacity of Comparative Example 26 at 1C cycle is 343mAh / g, proving that the recycled and purified mixed chemicals can still effectively dissolve cellulose in biomass.
[0213] Fig.21 The cycle performance diagrams of Example 10 and Comparative Example 27 at 0.001-2.5V, 1C are shown. The capacity of Example 10 at 1C cycle is 348mAh / g; the capacity of Comparative Example 27 at 1C cycle is 348mAh / g, proving that the recycled and purified mixed chemicals can still effectively dissolve cellulose in biomass.
[0214] Fig. 22 The cycle performance diagrams of Example 4 and Comparative Examples 7 and 8 at 0.001-2.5V, 1C are shown. The capacity of Example 4 at 1C cycle is 343mAh / g; the capacity of Comparative Example 7 at 1C cycle is 340mAh / g; the capacity of Comparative Example 8 at 1C cycle is 347mAh / g, which proves that this method is also applicable to other biomass materials.
[0215] The preparation method provided by the present invention has a higher energy density than traditional graphite negative electrode materials through surface modification of oxygen functional groups, can store more charge, and provide a longer service life. It shows good cycle stability during the charge and discharge process, can withstand a large number of charge and discharge cycles with almost no capacity decay, and prolongs the life of the secondary battery. In addition, it will not cause serious thermal runaway reactions in practical applications, has good thermal stability and safety, and reduces the risk of fire.
[0216] The hard carbon negative electrode designed by the present invention has a higher specific capacity and energy density, and can store more charge and energy; this means that the sodium ion battery can provide a longer working time and a higher energy output with a relatively small volume and weight.
[0217] The hard carbon negative electrode designed in the present invention has excellent cycle stability and life performance, and can withstand long-term charge and discharge cycles without obvious capacity decay or structural damage, which enables the sodium ion battery to maintain stable performance during long-term use.
[0218] The hard carbon designed in the present invention has a lower charge transfer resistance and a higher ion diffusion coefficient, and can achieve faster charge transfer and ion migration speed during the charge and discharge process, so that the sodium ion battery can be quickly charged and discharged to meet the demand for high power output.
[0219] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a biomass hard carbon material, characterized in that: include: S1, drying and dehydrating the biomass material, and crushing it into biomass powder; S2, mixing the biomass powder with a cellulose dissolving agent to remove cellulose from the biomass powder to form a biomass slurry; S3, removing the cellulose dissolving agent in the biomass slurry to obtain biomass secondary powder; S4, pre-oxidizing the biomass secondary powder in an air atmosphere to stabilize the structure, and obtaining pre-oxidized powder; S5, carbonizing the pre-oxidized powder to obtain a biomass hard carbon material.
2. The method for preparing a biomass hard carbon material according to claim 1, characterized in that: S2 specifically includes: mixing the biomass powder with the cellulose dissolving agent, first heating and stirring, then stirring in an ice bath, and finally standing at room temperature.
3. The method for preparing a biomass hard carbon material according to claim 1, characterized in that: S3 specifically includes: performing rotary evaporation on the biomass slurry, and connecting a condensation device at the tail end to recover the cellulose dissolving agent.
4. The method for preparing a biomass hard carbon material according to claim 1, characterized in that: S5 specifically includes: The pre-oxidized powder is firstly pre-carbonized in an inert atmosphere; The pre-carbonized powder is naturally cooled to room temperature, immersed in acid solution for pickling, and then filtered and dried; The powder obtained after filtration and drying is carbonized under an inert atmosphere, and then naturally cooled to room temperature to obtain a biomass hard carbon material; The pre-carbonization temperature is lower than the carbonization temperature.
5. The method for preparing a biomass hard carbon material according to claim 2, characterized in that: The cellulose dissolving agent is at least one of a tetrabutylammonium hydroxide solution, a tetrabutylammonium fluoride solution and a tetrabutylammonium sulfate solution; And / or, the temperature range of heating and stirring in S2 is 30°C-50°C, and the time range of heating and stirring is 0.5h-6h; the temperature range of ice bath stirring is -5°C--25°C, and the time range of ice bath stirring is 1h-3h; the time range of standing at room temperature is 0.5h-2h.
6. The method for preparing a biomass hard carbon material according to claim 5, characterized in that: When the cellulose dissolving agent is a combination of two of the above solutions, the ratio of the two solutions is 2:3-7:3; when the cellulose dissolving agent is a combination of three of the above solutions, the ratio of tetrabutylammonium hydroxide solution, tetrabutylammonium fluoride solution and tetrabutylammonium sulfate solution is 7:7:6 or 3:3:4 or 2:2:1; And / or, the mass fraction of the tetrabutylammonium hydroxide solution, the tetrabutylammonium fluoride solution and the tetrabutylammonium sulfate solution is 40%-70%.
7. The method for preparing a biomass hard carbon material according to claim 4, characterized in that: The pre-oxidation temperature range in S4 is 200°C-300°C, and the pre-oxidation time range is 2h-6h; The temperature range of pre-carbonization in S5 is 500°C-900°C, and the time range of pre-carbonization is 0.5h-6h; The temperature range of carbonization is 1000°C-1600°C, and the time range of carbonization is 1h-12h.
8. The method for preparing a biomass hard carbon material according to claim 1, characterized in that: The type of biomass material described in S1 is at least one of hardwood, softwood, walnut shells, pistachio shells, pecan shells, almond shells, almond shells, hazelnut shells, pine nut shells, chestnut shells, ginkgo shells, macadamia shells, pili shells, peanuts, sunflower seeds, pumpkin seeds and watermelon seeds.
9. A biomass hard carbon material, characterized in that: The biomass hard carbon material is prepared by the method for preparing the biomass hard carbon material according to any one of claims 1 to 8.
10. A secondary battery, characterized in that: It comprises an electrode plate, wherein the electrode plate comprises a current collector and the biomass hard carbon material according to claim 9, wherein the biomass hard carbon material is coated on the current collector.
Citation Information
Patent Citations
Preparation method of sodium lithium battery cathode material as well as product and application thereof
CN106816576A
Method for preparing battery negative electrode material by utilizing enzymatic hydrolysis lignin-based epoxy resin
CN112408359A
Sodium-ion battery biomass hard carbon modified composite negative electrode material, preparation method and application
CN117996030A
Positive electrode material, lithium ion secondary battery using the same, and method of manufacturing positive electrode material
JP2013077425A
Method for digesting a biomass comprising lignin together with cellulose and / or hemicellulose
US20110201096A1
Cited By
Hard carbon material prepared from atmosphere-modulated hard carbon closed pore and pseudo graphite domain as well as preparation method and application of hard carbon material
CN119528116A
A hard carbon material prepared by atmosphere-adjusted hard carbon closed pores and pseudo-graphite domains and a preparation method and application thereof
CN119528116B
Biomass hard carbon and preparation method and application thereof
CN120664525B
Preparation of lignin-based monatomic hard carbon material, hard carbon material and secondary battery
CN121757845A