Thermal insulation slurry as well as preparation method and application thereof
By using the combination of organic insulation particles and inorganic gelling materials in the external insulation system of building exterior walls, a fire-resistant differential bin structure is formed, which solves the problems of flammability and high thermal conductivity of existing materials, and achieves good insulation performance and durability reduces production costs and improves the safety and environmental protection of the system.
Patent Information
- Application Number
- CN202411427117.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
AI Technical Summary
The existing insulation materials have problems such as cracking, flammability, cavity and material shedding in the external insulation system of building exterior walls, which affects their durability and safety. Inorganic materials have a large thermal conductivity and limited insulation performance.
A thermal insulation slurry, including organic thermal insulation particles, inorganic gelling materials and water, forms a fire-resistant differential silo structure through reasonable proportions and component ratios, improves thermal insulation and fire resistance, and ensures the material through dry mixing and stirring technology. Even mixing and bonding.
It realizes good adhesion, compressive strength and crack resistance of the external insulation system of building exterior walls, reduces the thermal conductivity, improves the durability and fire resistance of the material, extends the service life of the system, and uses environmentally friendly materials and resources Reuse reduces production costs.
Smart Images

Figure CN118930161A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal insulation materials, and particularly relates to a thermal insulation slurry and a preparation method and application thereof. Background Art
[0002] The external insulation system of building exterior walls is currently the most widely used energy-saving measure for building exterior wall enclosure structures. However, in actual use, the insulation system will have problems such as cracking, flammability, cavities and material shedding. In particular, doubts about its durability and safety have affected its promotion and use. The performance of the insulation material itself is the main reason for the cracking and shedding of the external insulation system of the building exterior wall. Existing insulation materials can be divided into organic insulation materials and inorganic insulation materials according to the material properties. Organic insulation materials have the advantages of low density, light weight, low thermal conductivity, and excellent thermal insulation performance, but they have low fire resistance, poor flame retardant properties, and are easy to burn, which makes the fire accidents of building exterior walls frequent, causing huge casualties and property losses. This major defect limits the application scope of this type of material in the construction market. Inorganic insulation materials have the advantages of good fire resistance, excellent stability, and anti-aging, but they have a large thermal conductivity and limited thermal insulation performance.
[0003] At present, there is an urgent need for thermal insulation materials with good thermal insulation performance, weather resistance and fire resistance. Summary of the invention
[0004] In view of this, the present invention provides a thermal insulation slurry and a preparation method and application thereof. The thermal insulation slurry provided by the present invention has good thermal insulation performance, weather resistance and fire resistance as a thermal insulation material for building exterior walls, improves the safety of use of the external thermal insulation system of the building exterior wall and extends the validity period of the external thermal insulation system of the building exterior wall.
[0005] In order to solve the above technical problems, the present invention provides a thermal insulation slurry, comprising organic thermal insulation particles, an inorganic gelling material and water; the mass ratio of the inorganic gelling material to the volume of the organic thermal insulation particles is 3.8-4.4 kg:30-35 L, and the mass ratio of the inorganic gelling material to water is 3.8-4.4:4-5; The organic heat-insulating particles include the following components in parts by volume, where the volume is the bulk volume: 10-73 parts of polyurethane particles; 30-60 parts of polystyrene particles; The inorganic gelling material comprises the following components in parts by weight: 36~62 parts of cement; Fly ash 23-39 parts; 5-15 parts of talcum powder; 2~8 parts of redispersible latex powder; 1.8~2.2 parts of resin powder; Polyvinyl alcohol 0.3-0.5 parts; Hydroxypropyl methylcellulose 0.8-1.2 parts; 0.4~0.6 parts of silicone water repellent; 0.4~0.6 parts of polypropylene fiber.
[0006] Preferably, the polyurethane particles include polyurethane foam particles and recyclable polyurethane granules; the mass ratio of the polyurethane foam particles to the recyclable polyurethane granules is 20-40:20-33.
[0007] Preferably, the average particle size of the polyurethane foam particles is 3-10 mm, and the bulk density is 45-100 kg / m 3 , thermal conductivity is 0.032~0.038W / (m·K); The average particle size of the recyclable polyurethane pellets is ≤10mm, and the bulk density is 40-50kg / m 3 .
[0008] Preferably, the average particle size of the polystyrene particles is ≤5 mm, and the bulk density is 15-25 kg / m 3 , the thermal conductivity is 0.024~0.041W / (m·K).
[0009] Preferably, the mass ratio of the inorganic gelling material to the volume of the organic thermal insulation particles is 4.2 kg:30-35 L, and the mass ratio of the inorganic gelling material to water is 4.2:4-5.
[0010] The present invention also provides a method for preparing the thermal insulation slurry described in the above technical solution, comprising the following steps: The organic thermal insulation particles, the inorganic gelling material and water are mixed to obtain the thermal insulation slurry.
[0011] Preferably, the mixing comprises the following steps: The cement, fly ash, talcum powder, redispersible latex powder, resin rubber powder, polyvinyl alcohol, hydroxypropyl methylcellulose, silicone water repellent and polypropylene fiber are dry-mixed to obtain a dry mix; The dry mixed material and a portion of water are first mixed, and then polyurethane particles, polystyrene particles and the remaining portion of water are added for a second mixing to obtain the thermal insulation slurry.
[0012] Preferably, the dry mixing is carried out under stirring conditions, and the stirring time is greater than or equal to 8 minutes.
[0013] Preferably, the first mixing and the second mixing are performed under stirring conditions, and the first mixing stirring time and the second mixing stirring time are independently 3 to 5 minutes.
[0014] The present invention also provides the use of the thermal insulation slurry described in the above technical solution or the thermal insulation slurry prepared by the preparation method described in the above technical solution as a thermal insulation material for building exterior walls.
[0015] The invention provides a thermal insulation slurry, comprising organic thermal insulation particles, an inorganic gelling material and water; the mass ratio of the inorganic gelling material to the organic thermal insulation particles is 3.8-4.4 kg:30-35 L, and the mass ratio of the inorganic gelling material to water is 3.8-4.4:4-5; the organic thermal insulation particles comprise the following components in parts by volume, where the volume is the stacking volume: 10-73 parts of polyurethane particles and 30-60 parts of polyphenyl particles; the inorganic gelling material comprises the following components in parts by mass: 36-62 parts of cement, 23-39 parts of fly ash, 5-15 parts of talc, 2-8 parts of redispersible latex powder, 1.8-2.2 parts of resin powder, 0.3-0.5 parts of polyvinyl alcohol, 0.8-1.2 parts of hydroxypropyl methylcellulose, 0.4-0.6 parts of organosilicon water repellent and 0.4-0.6 parts of polypropylene fiber. In the present invention, the polyurethane particles have low thermal conductivity, good thermal insulation effect, low water absorption, good waterproof performance, good compressive strength and adhesion. As a building exterior wall insulation material, it is convenient for the insulation layer to be fully bonded to the building exterior wall base layer, and no anchoring is required to achieve effective bonding between the wallboard and the insulation layer, truly realizing the integration of the insulation structure. In the present invention, talcum powder, redispersible latex powder, resin powder, polyvinyl alcohol and hydroxypropyl methylcellulose can improve the adhesion and hydrophilicity of the polyurethane particles. In the present invention, the organosilicon hydrophobic agent can improve the hydrophobicity of the insulation material, reduce the water absorption rate, and increase the service life of the material; polypropylene fiber can improve the crack resistance of the insulation material and reduce shrinkage. In the insulation slurry provided by the present invention, the inorganic gelling material wraps the organic insulation particles to form a fireproof differential compartment structure, which can effectively prevent the transfer of heat and improve the combustion grade and durability of polystyrene particles and polyurethane particles insulation materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The present invention is a schematic diagram of the process of preparing thermal insulation slurry and building exterior wall thermal insulation material in an embodiment. DETAILED DESCRIPTION
[0017] The present invention provides a thermal insulation slurry, comprising organic thermal insulation particles, an inorganic gelling material and water; the mass ratio of the inorganic gelling material to the volume of the organic thermal insulation particles is 3.8-4.4 kg:30-35 L, and the mass ratio of the inorganic gelling material to water is 3.8-4.4:4-5; The organic heat-insulating particles include the following components in parts by volume, where the volume is the bulk volume: 10-73 parts of polyurethane particles; 30-60 parts of polystyrene particles; The inorganic gelling material comprises the following components in parts by weight: 36~62 parts of cement; Fly ash 23-39 parts; 5-15 parts of talcum powder; 2~8 parts of redispersible latex powder; 1.8~2.2 parts of resin powder; Polyvinyl alcohol 0.3-0.5 parts; Hydroxypropyl methylcellulose 0.8-1.2 parts; 0.4~0.6 parts of silicone water repellent; 0.4~0.6 parts of polypropylene fiber.
[0018] In the present invention, the thermal insulation slurry includes organic thermal insulation particles. According to the bulk volume, the organic thermal insulation particles include 10 to 73 parts of polyurethane particles, preferably 40 to 70 parts, and more preferably 66 to 70 parts. In the present invention, the polyurethane particles preferably include polyurethane foam particles and recyclable polyurethane pellets. In the present invention, the raw material of the recyclable polyurethane pellets is preferably recycled waste polyurethane foam, and the waste polyurethane foam is preferably obtained by crushing the scraps, mold overflow or waste generated by the polyurethane foam production factory. In the present invention, the recyclable polyurethane pellets are preferably irregular polyhedrons; the average particle size of the recyclable polyurethane pellets is preferably ≤10mm, more preferably 3 to 8mm; the bulk density of the recyclable polyurethane pellets is preferably 40 to 50kg / m 3 , more preferably 45kg / m 3 In the present invention, the average particle size of the polyurethane foam particles is preferably 3-10 mm, more preferably 4-8 mm; the bulk density of the polyurethane foam particles is preferably 45-100 kg / m 3 , more preferably 50~80kg / m 3 The thermal conductivity of the polyurethane foam particles is preferably 0.032-0.038 W / (m·K), more preferably 0.034-0.036 W / (m·K). In the present invention, the mass ratio of the polyurethane foam particles to the recyclable polyurethane pellets is preferably 20-40:20-33, more preferably 33-40:30-33, specifically 4:3 or 1:1.
[0019] The present invention utilizes recyclable polyurethane pellets to replace part of the polyurethane foam particles to achieve the recycling and reuse of polyurethane waste, improves the environmental sustainability of the thermal insulation slurry, and reduces the production cost.
[0020] Based on the volume fraction of the polyurethane particles, the organic thermal insulation particles include 30 to 60 parts of polystyrene particles, preferably 30 to 33 parts. In the present invention, the average particle size of the polystyrene particles is preferably ≤5 mm, more preferably 1 to 4 mm; the bulk density of the polystyrene particles is preferably 15 to 25 kg / m 3 , more preferably 20kg / m 3 The thermal conductivity of the polystyrene particles is preferably 0.024~0.041W / (m·K), and more preferably 0.03~0.038W / (m·K).
[0021] The present invention limits the average particle size of polyurethane foam particles, recyclable polyurethane pellets and polystyrene particles within the above range, so that the three particles form a better gradation and are mixed with the inorganic gelling material, thereby improving the packing density of the thermal insulation material and further improving the thermal insulation performance of the thermal insulation material.
[0022] In the present invention, the thermal insulation slurry comprises an inorganic gelling material. In the present invention, the inorganic gelling material comprises 36 to 62 parts of cement, preferably 39 to 53 parts, by weight.
[0023] Based on the mass fraction of cement, the inorganic gelling material includes 23 to 39 parts of fly ash, preferably 27 to 36 parts. The present invention reduces the thermal conductivity of the material and increases the dry density of the insulation material by limiting the amount of fly ash, thereby improving the insulation performance; at the same time, the present invention replaces part of the cement with fly ash, thereby realizing waste resource utilization. The present invention adds fly ash to the insulation material to not only reduce the bulk density of the material, but also improve the fluidity of the insulation slurry, thereby solving the problems of waste pollution and the large bulk density and poor fluidity of the insulation material.
[0024] Based on the mass fraction of cement, the inorganic gelling material includes 5 to 15 parts of talc, preferably 5 to 10 parts. The present invention improves the thermal insulation performance, strength and stability of the thermal insulation slurry by adjusting the amount of talc, and improves its construction performance and water resistance.
[0025] Based on the mass fraction of cement, the inorganic gelling material includes 2 to 8 parts of redispersible latex powder, preferably 3 to 6 parts. In the present invention, the redispersible latex powder is added to the thermal insulation slurry as an organic modified additive to effectively improve the affinity between the thermal insulation particles and inorganic gelling materials such as cement, and improve the bonding force between the organic thermal insulation particles and the inorganic gelling material.
[0026] Based on the mass fraction of cement, the inorganic gelling material includes 1.8 to 2.2 parts of resin powder, preferably 2 parts.
[0027] Based on the mass fraction of cement, the inorganic gelling material includes 0.3-0.5 parts of polyvinyl alcohol, preferably 0.4 parts.
[0028] Based on the mass fraction of cement, the inorganic gelling material includes 0.8 to 1.2 parts of hydroxypropyl methylcellulose (HPMC), preferably 1 part.
[0029] Based on the mass fraction of cement, the inorganic gelling material includes 0.4 to 0.6 parts of organosilicon water repellent, preferably 0.5 parts.
[0030] Based on the mass fraction of cement, the inorganic gelling material includes 0.4 to 0.6 parts of polypropylene fiber, preferably 0.5 parts. In the present invention, the polypropylene fiber can improve the strength of the thermal insulation material, thereby improving the safety of use.
[0031] The present invention utilizes industrial solid waste fly ash to replace part of cement, and adds additives such as redispersible latex powder, talcum powder, hydroxypropyl methylcellulose, etc., to improve the thermal insulation performance and construction performance of the external thermal insulation material of the building exterior wall.
[0032] In the present invention, the thermal insulation slurry also includes water.
[0033] In the present invention, the mass ratio of the inorganic gelling material to the volume of the organic thermal insulation particles is 3.8-4.4 kg:30-35 L, preferably 4.2 kg:30-35 L; the mass ratio of the inorganic gelling material to water is 3.8-4.4:4-5, preferably 4.2:4-5.
[0034] The thermal insulation slurry provided by the present invention has good adhesion to the building exterior wall base, and when in use, the exterior wall insulation and leveling are integrated into a cavity-free structure, and the wallboard and the thermal insulation layer can be effectively bonded without using anchors, truly realizing the integration of the thermal insulation structure, and completely solving the thermal bridge problem of metal anchors. The thermal insulation layer formed by the thermal insulation slurry provided by the present invention is uniform and can release deformation stress layer by layer, and the microporous mesh structure absorbs deformation, and has good anti-cracking performance.
[0035] The present invention combines organic thermal insulation materials and inorganic thermal insulation materials to give full play to the advantages of both, so that the thermal insulation slurry has better comprehensive performance.
[0036] The present invention also provides a method for preparing the thermal insulation slurry described in the above technical solution, comprising the following steps: The organic thermal insulation particles, the inorganic gelling material and water are mixed to obtain the thermal insulation slurry.
[0037] In the present invention, the mixing preferably comprises the following steps: The cement, fly ash, talcum powder, redispersible latex powder, resin rubber powder, polyvinyl alcohol, hydroxypropyl methylcellulose, silicone water repellent and polypropylene fiber are dry-mixed to obtain a dry mix; The dry mixed material and a portion of water are first mixed, and then polyurethane particles, polystyrene particles and the remaining portion of water are added for a second mixing to obtain the thermal insulation slurry.
[0038] The present invention dry-mixes the cement, fly ash, talcum powder, redispersible latex powder, resin powder, polyvinyl alcohol, hydroxypropyl methylcellulose, silicone water repellent and polypropylene fiber to obtain a dry mix. In the present invention, the dry mixing is preferably carried out under stirring, and the stirring time is preferably greater than or equal to 8 minutes, more preferably 10 to 30 minutes. The present invention has no special requirements for the stirring speed, as long as it can be mixed evenly. In the present invention, the dry mixing is preferably carried out in a mortar mixer.
[0039] After obtaining the dry blend, the present invention first mixes the dry blend and part of the water, then adds polyurethane particles, polystyrene particles and the remaining part of the water for second mixing to obtain the thermal insulation slurry. The present invention has no special limitation on the mass percentage of the part of the water in the total water, as long as it can be mixed evenly. In the present invention, the first mixing is preferably carried out under stirring conditions, and the stirring time is preferably 3 to 5 minutes, more preferably 3 to 4 minutes. In the present invention, the first mixing is preferably carried out in a single-horizontal-shaft concrete mixer. In the present invention, the second mixing preferably includes the following steps: adding polyurethane particles and polystyrene particles to the first mixed material and then performing a third mixing; adding the remaining part of the water to the third mixed material for a fourth mixing. In the present invention, the third mixing is preferably carried out under stirring conditions, and the stirring time is preferably 3 to 5 minutes, more preferably 3 to 4 minutes. In the present invention, the fourth mixing is preferably carried out under stirring conditions, and the stirring time is preferably 3 to 5 minutes, more preferably 3 to 4 minutes. In the present invention, the second mixing is preferably carried out in a single-horizontal-shaft concrete mixer.
[0040] The invention can make the organic heat-insulating particles evenly distributed in the inorganic gelling material through step-by-step mixing, thereby improving the heat-insulating performance of the heat-insulating material.
[0041] The building exterior wall insulation material formed by the insulation slurry provided by the present invention has the following advantages over the existing building exterior wall insulation materials: inorganic gelling materials wrap organic insulation particles to form a fireproof differential compartment structure, effectively preventing heat transfer, improving the combustion level, and improving the durability and stability of the insulation material. Industrial solid waste resources are utilized to reduce production costs and improve environmental protection, which meets the requirements of environmental sustainability and resource recycling. The present invention combines a variety of insulation materials to meet the needs of different building exterior walls and improve the insulation effect.
[0042] The present invention also provides the use of the thermal insulation slurry described in the above technical solution or the thermal insulation slurry prepared by the preparation method described in the above technical solution as a building exterior wall thermal insulation material. When the thermal insulation slurry is used as a building exterior wall thermal insulation material in the present invention, the following steps are preferably included: the thermal insulation slurry is placed in a mold for molding, and then demolding, curing, drying and trimming are performed in sequence to obtain the building exterior wall thermal insulation material. The present invention has no special requirements on the shape and size of the mold, and it can be designed according to the actual needs of the building exterior wall thermal insulation material. The present invention has no special restrictions on the curing, drying and trimming, and conventional methods in the field can be used.
[0043] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0044] Embodiment Figure 1 The process shown is to prepare thermal insulation slurry, and use the thermal insulation slurry to prepare building exterior wall insulation materials.
[0045] Example 1 The recycled waste polyurethane foam (scraps, mold overflow or waste produced by polyurethane foam production plants) is crushed by a crusher to obtain an average particle size of 8mm and a bulk density of 45kg / m 3 Recyclable polyurethane pellets with irregular polyhedrons; According to the bulk volume, the organic thermal insulation particles include the following raw materials: average particle size 5mm, bulk density 60kg / m 3 , 40 parts of polyurethane foam particles with a thermal conductivity of 0.035W / (m·K); 30 parts of polystyrene particles; average particle size of 8mm, bulk density of 45kg / m 3 30 portions of recyclable polyurethane pellets with irregular polyhedrons; In terms of weight, the inorganic gelling materials include 62 parts of cement, 27 parts of fly ash, 5 parts of talc, 2 parts of redispersible latex powder, 2 parts of resin powder, 0.4 parts of polyvinyl alcohol, 1 part of hydroxypropyl methylcellulose, 0.5 parts of silicone water repellent, and 0.5 parts of polypropylene fiber; Cement, fly ash, talcum powder, redispersible latex powder, resin powder, polyvinyl alcohol, hydroxypropyl methylcellulose, silicone water repellent and polypropylene fiber are dry mixed in a mortar mixer for 20 minutes to obtain a dry mix (inorganic gelling material); 4.2 kg of dry mix and 2 kg of water were placed in a single-shaft concrete mixer and stirred for 3 min, then 33 L of organic thermal insulation particles were added and stirred for 3 min, then 2 kg of water was added and stirred for another 3 min to obtain thermal insulation slurry; The thermal insulation slurry is placed in a mold for molding, and then demoulding, curing, drying and trimming are performed in sequence to obtain the building exterior wall thermal insulation material.
[0046] Embodiment 2~4 The thermal insulation slurry and the building exterior wall thermal insulation material were prepared according to the method of Example 1, except for the amount of some materials used, as shown in Table 1.
[0047] Comparative Examples 1 to 3 The thermal insulation slurry and the building exterior wall thermal insulation material were prepared according to the method of Example 1, except for the amount of some materials used, as shown in Table 1.
[0048] Table 1 Amounts of materials used in Examples 1 to 4 and Comparative Examples 1 to 3
[0049] The properties of the building exterior wall thermal insulation materials prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were tested according to the following methods, and the results are listed in Table 2. The compressive strength and tensile strength were tested with reference to the test method for basic properties of building mortar (JGJ 70-1990), the softening coefficient was tested with reference to the lightweight partition board for building (GB / T 23451-2023), the thermal conductivity was tested with reference to the protective hot plate method for determination of steady-state thermal resistance and related properties of thermal insulation materials (GB / T 10294-2008), and the dry density was tested with reference to foamed concrete (JG / T266-2011).
[0050] Table 2 Performance of building exterior wall thermal insulation materials prepared in Examples 1 to 4 and Comparative Examples 1 to 3
[0051] It can be seen from Table 2 that the thermal insulation slurry provided by the present invention has a lower thermal conductivity, indicating that it has good thermal insulation performance. The thermal insulation slurry provided by the present invention has higher compressive strength and tensile strength, indicating that it has good mechanical properties. From the softening coefficient in Table 2, it can be seen that the exterior wall thermal insulation material provided by the present invention has good water resistance.
[0052] The durability, fire resistance and adhesion of the building exterior wall insulation material prepared in Example 3 were tested according to the following methods, and the results are listed in Table 3. The shrinkage performance was tested with reference to the test method for basic properties of building mortar (JGJ 70-2009), the antifreeze performance was tested with reference to the test method for frost resistance of aerated concrete (GB / T 11973-1997), the tensile bonding strength between the insulation material and cement mortar was tested with reference to the material for external wall insulation system of glue powder polystyrene particles (JG / T 158-2013), and the combustion performance was tested with reference to the monomer combustion test of building materials or products (GB / T 20284-2006) and the test method for non-combustibility of building materials (GB / T 5464-2010).
[0053] Table 3 Performance of the building exterior wall thermal insulation material prepared in Example 3
[0054] It can be seen from Tables 2 and 3 that when the ratio of polyurethane foam particles, benzene particles and recyclable polyurethane pellets is 1:1:1, the compressive strength of the building exterior wall insulation material is 434.64MPa, and the thermal conductivity reaches 0.042W / (m·K). The thermal conductivity of the commonly used external insulation material rock wool is 0.4W / (m·K). Compared with rock wool, the thermal conductivity of the building exterior wall insulation material provided by the present invention has been significantly reduced. After 25 freeze-thaw cycles, the mass loss rate was 6.5% and the strength loss rate was 22.6%, with good durability. After the combustion performance test, it reached A2 level, showing good flame retardant properties.
[0055] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A thermal insulation slurry, characterized in that: It comprises organic thermal insulation particles, inorganic gelling materials and water; the mass ratio of the inorganic gelling materials to the volume of the organic thermal insulation particles is 3.8-4.4 kg:30-35 L, and the mass ratio of the inorganic gelling materials to water is 3.8-4.4:4-5; The organic heat-insulating particles include the following components in parts by volume, where the volume is the bulk volume: 10-73 parts of polyurethane particles; 30-60 parts of polystyrene particles; The inorganic gelling material comprises the following components in parts by weight: 36~62 parts of cement; Fly ash 23-39 parts; 5-15 parts of talcum powder; 2~8 parts of redispersible latex powder; 1.8~2.2 parts of resin powder; Polyvinyl alcohol 0.3-0.5 parts; Hydroxypropyl methylcellulose 0.8-1.2 parts; 0.4~0.6 parts of silicone water repellent; 0.4~0.6 parts of polypropylene fiber.
2. The thermal insulation slurry according to claim 1, characterized in that: The polyurethane particles include polyurethane foam particles and recyclable polyurethane granules; the mass ratio of the polyurethane foam particles to the recyclable polyurethane granules is 20-40:20-33.
3. The thermal insulation slurry according to claim 2, characterized in that: The average particle size of the polyurethane foam particles is 3-10 mm, and the bulk density is 45-100 kg / m 3 , thermal conductivity is 0.032~0.038W / (m·K); The average particle size of the recyclable polyurethane pellets is ≤10mm, and the bulk density is 40-50kg / m 3 .
4. The thermal insulation slurry according to claim 1, characterized in that: The average particle size of the polystyrene particles is ≤5mm, and the bulk density is 15-25kg / m 3 , the thermal conductivity is 0.024~0.041W / (m·K).
5. The thermal insulation slurry according to any one of claims 1 to 4, characterized in that: The mass ratio of the inorganic gelling material to the volume of the organic thermal insulation particles is 4.2 kg:30-35 L, and the mass ratio of the inorganic gelling material to water is 4.2:4-5.
6. The method for preparing the thermal insulation slurry according to any one of claims 1 to 5, characterized in that: The following steps are involved: The organic thermal insulation particles, the inorganic gelling material and water are mixed to obtain the thermal insulation slurry.
7. The preparation method according to claim 6, characterized in that: The mixing comprises the following steps: The cement, fly ash, talcum powder, redispersible latex powder, resin rubber powder, polyvinyl alcohol, hydroxypropyl methylcellulose, silicone water repellent and polypropylene fiber are dry-mixed to obtain a dry mix; The dry mixed material and a portion of water are first mixed, and then polyurethane particles, polystyrene particles and the remaining portion of water are added for a second mixing to obtain the thermal insulation slurry.
8. The preparation method according to claim 7, characterized in that: The dry mixing is carried out under stirring conditions, and the stirring time is greater than or equal to 8 minutes.
9. The preparation method according to claim 7, characterized in that: The first mixing and the second mixing are performed under stirring conditions, respectively, and the first mixing stirring time and the second mixing stirring time are independently 3 to 5 minutes.
10. Use of the thermal insulation slurry according to any one of claims 1 to 5 or the thermal insulation slurry prepared by the preparation method according to any one of claims 6 to 9 as a thermal insulation material for building exterior walls.
Citation Information
Cited By
Hollow laminated light steel keel sandwich heat insulation wallboard and installation method thereof
CN119777516A
A hollow laminated light steel keel sandwich thermal insulation wall panel and its installation method
CN119777516B