Construction material for security inspection machine main body structure and preparation method thereof

By using radiation-proof concrete materials, the problems of security inspection machine assembly complexity and anti-corrosion pollution of traditional materials are solved, and assembly is simplified, cost reduction and corrosion resistance are achieved, radiation protection requirements are met, and the service life and performance of the equipment are improved. .

CN118930162APending Publication Date: 2024-11-12JIANGSU WEIERLUOLIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999041.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing security inspection machines must fully penetrate the channel size in the longitudinal direction, resulting in the inability to arrange reinforced parts. In order to avoid the X-ray transmission of three points and one line, there are many parts assembled, which is time-consuming and labor-intensive, and the corrosion protection of traditional materials is anti-corrosion. There is a pollution problem in the process.

Method used

Use radiation-proof concrete as the main structural material of the security machine, including barium cement, lead powder, fine aggregate, coarse aggregate, water reducing agent and admixture. It is formed in one mold through the mold to avoid riveting or bolting assembly, and in the formula Barium aluminate and fume are added to improve radiation resistance and corrosion resistance.

Benefits of technology

It simplifies the assembly process of security inspection machines, reduces production costs, improves the environmental protection and corrosion resistance of materials, meets radiation protection requirements, improves compressive strength and frost resistance, and extends the service life of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004961046500000061
    Figure BDA0004961046500000061
  • Figure BDA0004961046500000081
    Figure BDA0004961046500000081
  • Figure BDA0004961046500000091
    Figure BDA0004961046500000091
Patent Text Reader

Abstract

The invention relates to the technical field of security inspection machine construction materials, in particular to a construction material for a security inspection machine main body structure and a preparation method of the construction material for the security inspection machine main body structure. Comprising 160 to 240 parts of cement, 400 to 600 parts of fine aggregate, 800 to 900 parts of coarse aggregate, 30 to 60 parts of lead powder, 0.2 to 0.3 part of a water reducing agent, 8 to 15 parts of an additive and 80 to 110 parts of water, and the cement is barium cement. The anti-radiation concrete is used as a construction material of the security inspection machine main body structure, the security inspection machine main body structure can be formed at a time by using a mold, and compared with a traditional method that profile steel and steel plates are used as the construction material of the security inspection machine main body structure, the security inspection machine main body component does not need to be assembled through rivet welding or bolting, and time and labor are not needed for assembling accessories; and the assembly of the security inspection machine is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of structural materials for security inspection machines, and in particular to a structural material for a main structure of a security inspection machine and a preparation method thereof. Background Art

[0002] With the development of society, security issues have attracted more and more attention, especially in public places such as airports, subway stations, and railway stations. In order to ensure people's safety, security inspection machines are needed to check passengers' luggage and personal packages to ensure public safety.

[0003] The existing security inspection machine is made of traditional steel and steel plates through riveting or bolting. In order to prevent rust, the surface is sprayed with plastic or painted. In order to prevent radiation to staff and passengers, lead sheets are glued on the inner or outer side of the security inspection machine for shielding protection. The above-mentioned security inspection machine must be completely penetrated in the longitudinal direction, and no reinforcement parts shall be arranged in the channel. In order to avoid the X-ray penetration seam in the horizontal direction, the existing security inspection machine has more assembly parts, which consumes time and labor to assemble, bringing inconvenience to the assembly of the security inspection machine. Summary of the invention

[0004] In order to solve the technical problem that the channel dimension of the security inspection machine must be completely penetrated in the longitudinal direction and no reinforcing components may be arranged in the channel, and in order to avoid the X-ray penetration seam in the horizontal direction, the existing security inspection machine has more assembly parts and the assembly is time-consuming and labor-intensive, the present application provides a structural material for the main structure of the security inspection machine and a preparation method thereof.

[0005] The present application provides a structural material for the main structure of a security inspection machine using the following technical solution:

[0006] A structural material for a main structure of a security inspection machine, the structural material being radiation-proof concrete, the radiation-proof concrete comprising, by weight, 160-240 parts of cement, 400-600 parts of fine aggregate, 800-900 parts of coarse aggregate, 30-60 parts of lead powder, 0.2-0.3 parts of a water reducing agent, 8-15 parts of an admixture, and 80-110 parts of water, wherein the cement is barium cement.

[0007] Furthermore, the radiation-proof concrete includes, by weight, 200 parts of cement, 500 parts of fine aggregate, 840 parts of coarse aggregate, 38 parts of lead powder, 0.26 parts of water reducer, 12 parts of admixture, and 100 parts of water.

[0008] Furthermore, the fine aggregate includes copper slag and first barite in a weight ratio of (2-3):(5-7).

[0009] Furthermore, the copper slag is ground copper slag, and the particle size distribution of the ground copper slag is: 4.75mm sieve residue within 0.06%, 2mm sieve residue within 4.65%, 1.4mm sieve residue within 10%, 0.2mm sieve residue 64-75%, 0.1mm sieve residue more than 87.9%.

[0010] Furthermore, the particle size of the first barite is less than 4.75 mm.

[0011] Furthermore, the coarse aggregate is selected from crushed stone and second barite in a weight ratio of 5:(3.5-4).

[0012] Furthermore, the particle size of the coarse aggregate is less than or equal to 15 mm.

[0013] Furthermore, the admixture comprises porous silicon and hyperbranched epoxy resin in a weight ratio of (12-15):1.

[0014] Furthermore, the radiation-proof concrete also includes 30-50 parts by weight of silica fume.

[0015] The present application also provides a method for preparing the aforementioned structural material for the main structure of the security inspection machine, comprising the following steps:

[0016] After cement, fine aggregate and coarse aggregate are mixed evenly, lead powder is added and mixing is continued for 5-10 minutes to obtain a mixture;

[0017] Mixing the water reducing agent, the admixture and water to obtain a mixed solution;

[0018] While stirring, slowly add the mixed liquid into the mixture.

[0019] In summary, this application has the following beneficial effects:

[0020] 1. The structural material used for the main structure of the security inspection machine in the present application is radiation-proof concrete. By using radiation-proof concrete as the structural material for the main structure of the security inspection machine, the main structure of the security inspection machine can be formed in one step using a mold. Compared with the traditional steel sections and steel plates used as the main structural materials of the security inspection machine, there is no need to assemble the main components of the security inspection machine through riveting or bolting. On the one hand, there is no need to spend time and effort to assemble accessories, which facilitates the assembly of the security inspection machine. On the other hand, there is no need to arrange reinforcing parts in the channel, so that the three-point straight line of the main optical path is more stable.

[0021] Furthermore, the main structure of the traditional security inspection machine is usually anti-corrosive by spraying plastic, painting or galvanizing on the surface of carbon steel or steel, and the painting and galvanizing process is easy to cause environmental pollution. The use of radiation-proof cement as the structural material of the main structure of the security inspection machine is more environmentally friendly than using traditional steel or carbon steel. In order to improve the corrosion resistance of the existing security inspection machines in coastal cities, stainless steel is usually used as the structural material of the main structure of the security inspection machine, which is more expensive. The radiation-proof cement of the present application has high corrosion resistance in high humidity, high temperature and high salinity air environments. The structural material of the present application is used to replace stainless steel materials to manufacture security inspection machines, which further reduces the cost of the security inspection machine and extends the service life of the security inspection machine when used in coastal cities.

[0022] 2. The structural material of the main structure of the security inspection machine of the present application, the barium aluminate and lead powder in its formula have good radiation protection performance, can meet the radiation protection requirements of the security inspection machine, and there is no need to stick lead sheets on the inside or outside of the security inspection machine. The price of concrete is lower than that of steel or stainless steel, which greatly reduces the production cost of the security inspection machine. Furthermore, through the mutual coordination of coarse aggregate, fine aggregate and admixtures, the problems of segregation and low compressive strength when the main structure of the security inspection machine is made of radiation-proof concrete are greatly reduced.

[0023] 3. The structural material of the present application is a combination of fine aggregate and coarse aggregate with good particle grading, and is supplemented with a certain ratio of nano-silicon and hyperbranched epoxy resin as admixtures. While solving the segregation problem, it improves the homogeneity of the structural material and improves the construction performance of the structural material.

[0024] 4. The structural material of the present application, the added silica fume interacts with the well-graded fine aggregate and admixtures, which improves the compressive strength and also has excellent frost resistance, making it easy to use the security inspection machine made of it in a colder environment, thereby increasing the scope of use of the structural material. DETAILED DESCRIPTION

[0025] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0026] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0027] The barium cement used in this application is barium sulfate cement, the product number of which is 230906, purchased from Shandong Qixin Radiation Protection Equipment Co., Ltd.;

[0028] The copper slag used in this application was purchased from a copper manufacturing plant, and its main chemical components are: Fe48.2%, Cu 0.5%, Fe3O47.3%, Al2O312.7%, SiO221.5%, CaO 7.9% and trace amounts of MgO;

[0029] The particle size of the first barite used in this application is 1-3 mm, purchased from Xi'an Jintianjiang Mining Co., Ltd.;

[0030] The particle size of the second barite used in this application is 5-8 mm, purchased from Xi'an Jintianjiang Mining Co., Ltd.;

[0031] The particle size of the crushed stone used in this application is 6-15 mm and was purchased from Xi'an Baidaxin Building Materials Co., Ltd.;

[0032] The lead powder used in this application has a particle size of 600 mesh and was purchased from Shandong Xinbaiyi Metal Materials Co., Ltd.;

[0033] The water reducer used in this application is a high-performance polycarboxylate water reducer, the model of which is RHEOPLUS 410, purchased from Guangzhou Xianrenhui International Trade Co., Ltd.;

[0034] The specific surface area of ​​the porous silicon used in this application is about 622m 2 / g, purchased from Angxing New Carbon Materials Changzhou Co., Ltd.;

[0035] The hyperbranched epoxy resin used in this application is a hyperbranched epoxy resin HyPer E102 purchased from Wuhan Hyperbranched Resin Technology Co., Ltd.;

[0036] Example 1

[0037] This embodiment provides a structural material for the main structure of a security inspection machine, and the preparation method thereof includes the following steps:

[0038] S1, 20kg cement, 50kg fine aggregate, 84kg coarse aggregate are mixed evenly, then 3.8kg lead powder is added and stirred for 10min to obtain a mixture;

[0039] S2, 0.026 kg of water reducing agent, 1.2 kg of admixture and 10 kg of water are mixed to obtain a mixed solution;

[0040] S3. While stirring, slowly add the mixed liquid into the mixture, and then continue stirring for 5 minutes.

[0041] In Example 1, the barium cement used is barium sulfate cement, the copper slag of the fine aggregate is the copper slag that is mechanically ground for 8 minutes, and the particle size distribution of the ground copper slag is: 4.75mm sieve residue within 0.06%, 2mm sieve residue within 4.65%, 1.4mm sieve residue within 10%, 0.2mm sieve residue 64-75%, 0.15mm sieve residue more than 98%, and the main chemical components of the copper slag are: Fe is 48.2%, Cu is 0.5%, Fe3O 4 is 7.3%, Al2O3 is 12.7%, SiO2 is 21.5%, CaO is 7.9% and a trace of MgO; the particle size of the first barite is 1-3mm, the weight ratio of copper slag to the first barite in the fine aggregate is 3:7, the particle size of crushed stone is 6-15mm, the particle size of the second barite is 5-8mm, the weight ratio of crushed stone to the second barite in the coarse aggregate is 5:3.5, the admixture is a hyperbranched epoxy resin and the specific surface area is about 622m 2 / g of porous silicon, the weight ratio of porous silicon to hyperbranched epoxy resin is 13:1.

[0042] Example 2-3

[0043] Example 2-3 is the same as Example 1, and the difference between them and Example 1 is only the content and ratio of raw materials, as shown in Table 1.

[0044] Table 1 Ratio of raw materials and preparation conditions of Examples 1-3

[0045]

[0046] Example 4

[0047] Example 4 is based on Example 1, and the only difference from Example 1 is that in step S1, 3 kg of silica ash is added after the lead powder is added. The main chemical components of the silica ash used in Example 4 are: SiO2 86-95%, Al2O3 1±0.2%, MgO 0.7±0.1%, Na2O1.3±0.2%, its pH is medium, and more than 80% of the silica ash has a fineness of less than 1 μm. It was purchased from Beijing Shunjian Xingye Engineering Technology Co., Ltd.

[0048] Example 5

[0049] Example 5 is based on Example 1, and the only difference from Example 1 is that the fine aggregate is copper slag and first barite in a weight ratio of 1:7.

[0050] Example 6

[0051] Example 6 is based on Example 1, and the only difference from Example 1 is that the particle size distribution of the copper slag is as follows: 4.75 mm sieve residue 0.6%, 2.36 mm sieve residue 3.7%, 1.18 mm sieve residue 19%, 0.6 mm sieve residue 63.5%, 0.3 mm sieve residue 89.2%, 0.15 mm sieve residue 96.7%; the copper slag used in Example 6 is the copper slag that has been mechanically ground for 3 minutes.

[0052] Example 7

[0053] Example 7 is based on Example 1, and the only difference from Example 1 is that the coarse aggregate is crushed stone and second barite in a mass ratio of 1:1.

[0054] Example 8

[0055] Example 8 is based on Example 1, and the only difference from Example 1 is that the weight ratio of porous silicon to hyperbranched epoxy resin in the admixture is 10:1.

[0056] Example 9

[0057] Example 9 is based on Example 1, and the only difference from Example 1 is that an equal amount of hyperbranched epoxy resin is used to replace porous silicon.

[0058] Example 10

[0059] Example 10 is based on Example 1, and the only difference from Example 1 is that an equal amount of porous silicon is used instead of the hyperbranched epoxy resin.

[0060] Comparative Example 1

[0061] Comparative Example 1 is based on Example 1, and the only difference from Example 1 is that an equal amount of barium sulfate cement is used instead of lead powder.

[0062] Comparative Example 2

[0063] Comparative Example 2 is based on Example 1, and the only difference from Example 1 is that the amount of fine aggregate used is 65 kg.

[0064] Comparative Example 3

[0065] Comparative Example 3 is based on Example 1, and the only difference from Example 1 is that the amount of the admixture is 0.7 kg.

[0066] Performance testing

[0067] According to the provisions of GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", the slump of the structural materials prepared in the embodiments and comparative examples was measured, and whether the structural materials had segregation was observed. The test results are shown in Table 2;

[0068] According to the provisions of GB / T50081-2016 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", the compressive strength of the structural materials prepared in the embodiments and comparative examples was tested, and the search results are shown in Table 2;

[0069] According to the provisions of GB / T50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete", the structural materials prepared in the examples and comparative examples were subjected to antifreeze tests. The antifreeze test was conducted by measuring the freeze-thaw compressive strength of the concrete specimens after the freeze-thaw test (freeze-thaw cycles were 20 times) after 28 days of standard curing, and calculating the loss rate of the freeze-thaw compressive strength relative to the initial compressive strength. The compressive strength before the freeze-thaw test after 28 days of standard curing was recorded as the initial compressive strength. The test results are shown in Table 2.

[0070] Table 2 Test results of examples and comparative examples

[0071]

[0072]

[0073] Referring to the test results, it can be seen that the structural material of the present application is a combination of fine aggregate and coarse aggregate with good particle grading in a specific proportion, and is assisted by a certain proportion of nano-silicon and hyperbranched epoxy resin as admixtures. While solving the segregation problem, it improves the homogeneity of the structural material and improves the construction performance of the structural material; the added specific amount of silica fume interacts with the specific proportion of well-graded fine aggregate and admixture, which improves the compressive strength and also has excellent frost resistance, making it convenient for the security inspection machine made of it to be used in a colder environment, thereby increasing the scope of use of the structural material.

[0074] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A structural material for the main structure of a security inspection machine, characterized in that: The structural material is radiation-proof concrete, which includes, by weight, 160-240 parts of cement, 400-600 parts of fine aggregate, 800-900 parts of coarse aggregate, 30-60 parts of lead powder, 0.2-0.3 parts of water reducer, 8-15 parts of admixture, and 80-110 parts of water. The cement is barium cement.

2. The structural material for the main structure of the security inspection machine according to item 1, characterized in that: The radiation-proof concrete comprises, by weight, 200 parts of cement, 500 parts of fine aggregate, 840 parts of coarse aggregate, 38 parts of lead powder, 0.26 parts of water reducer, 12 parts of admixture, and 100 parts of water.

3. The structural material for the main structure of the security inspection machine according to item 1, characterized in that: The fine aggregate includes copper slag and first barite in a weight ratio of (2-3):(5-7).

4. The structural material for the main structure of the security inspection machine according to item 3 is characterized in that: the copper slag is ground copper slag, and the particle size distribution of the ground copper slag is: The sieve residue of 4.75mm is within 0.06%, the sieve residue of 2mm is within 4.65%, the sieve residue of 1.4mm is within 10%, the sieve residue of 0.2mm is 64-75%, and the sieve residue of 0.1mm is more than 87.9%.

5. The structural material for the main structure of the security inspection machine according to item 3 is characterized in that: The particle size of the first barite is less than 4.75 mm.

6. The structural material for the main structure of the security inspection machine according to item 1, characterized in that: The coarse aggregate is selected from crushed stone and second barite in a weight ratio of 5:(3.5-4).

7. The structural material for the main structure of the security inspection machine according to item 1, characterized in that: The particle size of the coarse aggregate is less than or equal to 15 mm.

8. The structural material for the main structure of the security inspection machine according to item 1, characterized in that: The additive comprises porous silicon and hyperbranched epoxy resin in a weight ratio of (12-15):

1.

9. The structural material for the main structure of the security inspection machine according to item 1, characterized in that: The radiation-proof concrete also includes 30-50 parts by weight of silica fume.

10. The method for preparing the structural material for the main structure of the security inspection machine according to any one of claims 1 to 9, characterized in that: The steps include: mixing cement, fine aggregate and coarse aggregate evenly and adding The lead powder is stirred for 5-10 minutes to obtain a mixture; the water reducing agent, the admixture and the water are mixed to obtain a mixed solution; While stirring, slowly add the mixed liquid into the mixture.