Self-repairable, repeatedly-processed and degradable polyurethane material based on multi-bond action and preparation method of self-repairable, repeatedly-processed and degradable polyurethane material
By introducing a synergistic strategy of double dynamic covalent bonds and hydrogen bonds in polyurethane materials, self-repairable and degradable polyurethane materials are designed, which solves the problems of traditional materials being unable to repair after breakage and deterioration of mechanical properties at high temperatures, and achieves the High mechanical strength and efficient self-healing properties of the material.
Patent Information
- Application Number
- CN202411014669.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Traditional polyurethane materials cannot self-repair after breaking, and their mechanical properties deteriorate at high temperatures, making it difficult to have high self-repair efficiency and high mechanical strength.
Using a synergistic strategy of double dynamic covalent bonds and hydrogen bonds, a polyurethane based on double reversible dynamic covalent bonds and multiple hydrogen bonds is designed through the reversible exchange reaction and acid sensitivity characteristics of disulfide bonds and hexahydrotriazine rings. Materials, realize the self-healing, reprocessing and degradability of materials.
The material degrades rapidly under weak acid conditions, has excellent self-repair performance and high mechanical strength, and can maintain high mechanical strength after multiple processing and achieve efficient repair at a certain temperature and time.
Smart Images

Figure CN118930793A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of self-repairing polyurethane materials, and in particular to a self-repairing, repeatedly processable and degradable polyurethane material based on multiple bond effects and a preparation method thereof. Background Art
[0002] Polyurethane (PU) materials are widely used in coatings, elastomers, flexible protection and other fields due to their excellent properties such as high elasticity, easy synthesis and chemical resistance. However, traditional materials have irreversible covalent bonds inside, and once broken, they cannot be restored. It is difficult to achieve self-repair and it is easy to cause resource waste and environmental pollution.
[0003] In order to achieve self-repair of materials and restore their mechanical properties, researchers have endowed polyurethane with self-repairing properties by introducing reversible dynamic covalent bonds (Schiff bases, disulfide bonds, DA bonds, borate bonds, etc.) and non-covalent bonds (hydrogen bonds, metal coordination bonds, ionic bonds, etc.). An et al. proposed the use of thioxo-β-diketone-Cu 2+ The synergistic strategy of metal ligand coordination (ML) and hydrogen bonding was used to prepare an elastomer (fracture strength 4.35MPa, fracture strain 3400%). At the same time, the elastomer can achieve high self-healing efficiency (94%). Song et al. developed a new supramolecular polyurethane elastomer by combining dynamic covalent borate and boron nitrogen (BN) coordination. The prepared material has high self-healing efficiency, but its mechanical strength is low.
[0004] The above research introduces reversible dynamic bonds or non-covalent bonds into the polymer structure, giving the material self-healing properties. Although it has reconstruction properties, it is easily affected by temperature, dissociates at high temperatures or chemical changes occur inside the material, mechanical properties degrade, and it is impossible to have both high self-healing efficiency and high mechanical strength. In order to overcome the above problems, the present invention starts from the perspective of molecular structure design and develops a polyurethane material with a series of characteristics such as high mechanical strength, recyclability, self-healing and degradability based on the synergistic strategy of dual reversible dynamic covalent bonds and non-covalent bonds, so as to achieve sustainable development of polyurethane materials.
[0005] The disclosure of the above background technology content is only used to assist in understanding the inventive concept and technical solution of the present invention. It does not necessarily belong to the prior art of this patent application. In the absence of clear evidence that the above content has been disclosed on the filing date of this patent application, the above background technology should not be used to evaluate the novelty and creativity of the present application. Summary of the invention
[0006] The purpose of the present invention is to provide a self-repairing, repeatedly processable and degradable polyurethane material and a preparation method, so as to solve the technical problems existing in the above-mentioned prior art that high repair efficiency and mechanical properties cannot be achieved at the same time and the mechanical properties are degraded.
[0007] In order to solve the above technical problems, the present invention has the following technical solutions:
[0008] A self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds. Its polyurethane structure contains two reversible dynamic covalent bonds and multiple hydrogen bonds. Its strength and toughness can be regulated by the ratio of soft and hard segments. Its typical synthetic reaction structure features are as follows:
[0009]
[0010] The dynamic covalent bonds are disulfide bonds and hexahydrotriazine rings. The reversible exchange reaction characteristics of the disulfide bond structure endow the material with self-repairability and reprocessability, while the acid sensitivity of the hexahydrotriazine ring makes the material degradable.
[0011] A method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0012] S1. Under a nitrogen atmosphere, weigh the hydroxyl-terminated polyether / polyester after vacuum drying and dehydration, heat it to 110-120°C, remove water under vacuum for 1-2h under stirring, then cool it to 80°C, add diisocyanate and catalyst dibutyltin dilaurate, continue to react for 2-3h, and prepolymerize under the action of the catalyst to obtain -NCO-terminated polyurethane prepolymer; dissolve the chain extender 4,4-diaminodiphenyl sulfide in an organic solvent, add it to the reaction system for chain extension reaction, and the mixture obtained by the reaction is a polyurethane chain extension product based on a disulfide bond self-healing structure;
[0013] S2. Continue to add hydroxyethyl hexahydro-s-triazine to the polymerization system of step S1 and continue the reaction for 45 minutes; then pour the reaction solution into a polytetrafluoroethylene mold for leveling, put it into an oven to volatilize the solvent, and obtain a self-repairable, reprocessable and degradable polyurethane material.
[0014] Furthermore, the hydroxyl-terminated polyether / polyester described in step S1 includes one or more of hydroxyl-terminated polyethylene glycol, polypropylene glycol, polybutylene glycol, polycaprolactone, and polybutylene succinate, and the molecular weight thereof is 500-3000.
[0015] Furthermore, the diisocyanate described in step S1 includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate.
[0016] Furthermore, the catalyst described in step S1 includes one or more of dibutyltin dilaurate, N,N-dimethylcyclohexylamine, and stannous isooctanoate, and the usage amount accounts for 0.05-0.1wt% of the total mass of the reactants.
[0017] Furthermore, in step S1, the group ratio of NCO:(OH+NH2) is (1.2-1.5):1.
[0018] Furthermore, the solvent described in step S2 includes one or more of NN-dimethylformamide, tetrahydrofuran, dimethylene sulfoxide, and N-methylpyrrolidone.
[0019] Furthermore, the polyurethane prepared in step S1 and step S2 contains a carbamate structure and a urea group. The coexistence of these two structures enables hydrogen bonds to be formed within the polyurethane molecular chain and between molecules.
[0020] Furthermore, the preparation method of the self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds has the preparation conditions of heating and stirring the reaction at 80°C for 2-3 hours, and after curing, the self-repairable, reprocessable and degradable polyurethane material based on multiple bonds is obtained.
[0021] Furthermore, the curing time is 24 hours.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] (1) The polyurethane elastomer of the present invention has a synergistic effect of dual reversible covalent bonds and hydrogen bonds, forming a physical cross-linked structure, improving the mechanical properties of the material, and the polyurethane elastomer can be quickly and completely degraded under weak acid conditions.
[0024] (2) The polyurethane elastomer of the present invention has excellent self-healing properties at a certain temperature and time, and the synergistic effect of reversible dynamic covalent bonds and hydrogen bonds enables the elastomer to have both high mechanical strength and high repair efficiency.
[0025] (3) The polyurethane elastomer of the present invention can still maintain a relatively high mechanical strength after multiple processing cycles, and the tensile strength after three processing cycles is as high as 36.6 MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the structure of a polyurethane elastomer containing a hydrogen bond structure.
[0027] Figure 2 FTIR spectra of polyurethane elastomer under different NCO / (OH+NH2) and NH2:OH conditions.
[0028] Figure 3Microscope photos of the fracture surface of polyurethane elastomer before and after self-healing of scratches.
[0029] Figure 4 This is the stress-strain curve of the polyurethane elastomer at different time intervals after stretching.
[0030] Figure 5 This is the stress-strain curve of polyurethane elastomer under different repair times.
[0031] Figure 6 The stress-strain curves of polyurethane elastomers obtained with different processing cycles.
[0032] Figure 7 Digital image of the degradation of polyurethane elastomer in an acidic environment. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific implementation methods and with reference to the accompanying drawings. It should be emphasized that the following description is merely exemplary and is not intended to limit the scope of the present invention and its application. The advantages and all changes that can be thought of by relevant technicians in the field of polymer self-healing materials are included in the present invention, and the present invention covers all modifications, substitutions, equivalent methods and schemes within the concept and scope of the present invention as defined by the claims. The preparation process, reaction conditions, reagents, experimental methods, etc. for implementing the present invention, except for the contents specifically involved below, are all common knowledge and common sense in the field, and the present invention has no specific limiting contents. In order for the public to better understand the present invention, some specific details are described in detail here. For those skilled in the art, the present invention can be fully understood without these details.
[0034] Non-limiting and non-exclusive embodiments will be described with reference to the following figures, wherein like reference numerals refer to like parts unless otherwise specifically stated.
[0035] Example 1
[0036] A method for preparing a self-repairable and degradable polyurethane with dual reversible dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0037] (1) 4 g of hydroxyl-terminated polytetrahydrofuran with a molecular weight of 2000 and a substance amount of 2 mmol was placed in a three-necked flask with a stirrer, heated to 110° C., and vacuum-dried for 1 h under stirring. The mixture was then cooled to 80° C., 1.34 g of isophorone diisocyanate with a substance amount of 6 mmol, and a drop of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued for 3 h to form a prepolymer.
[0038] (2) 0.31 g of 4-4'-diaminodiphenyl disulfide (1.25 mmol) was dissolved in 3 mL of DMF and added to the above prepolymer for chain extension reaction for 3 h. Then 0.19 g of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine (0.83 mmol) was dissolved in 3 mL of DMF and added to the above mixture solution and stirred evenly. After reacting for 45 min, the reaction solution was poured into a polytetrafluoroethylene mold and dried at 80 °C for 48 h to obtain a self-healing and degradable polyurethane elastomer with dual reversible dynamic covalent bonds and hydrogen bonds with NCO / (NH2+OH) of 1.2 and NH2 / OH of 1:1.
[0039] Example 2
[0040] A method for preparing a self-repairable and degradable polyurethane with dual reversible dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0041] (1) 4 g of hydroxyl-terminated polytetrahydrofuran with a molecular weight of 2000 and a substance amount of 2 mmol was placed in a three-necked flask with a stirrer, heated to 110° C., and vacuum-dried for 1 h under stirring. The mixture was then cooled to 80° C., 1.34 g of isophorone diisocyanate with a substance amount of 6 mmol and a drop of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued for 3 h to form a prepolymer.
[0042] (2) 4-4'-diaminodiphenyl disulfide (0.31 g, 1.25 mmol) was dissolved in 3 mL of DMF and added to the above prepolymer for chain extension reaction for 3 h. Then, 0.19 g of hexahydro-1,3,5-tri(hydroxyethyl)-s-triazine (0.83 mmol) was dissolved in 3 mL of DMF and added to the above mixture solution and stirred evenly. After reacting for 45 min, the reaction solution was poured into a polytetrafluoroethylene mold and dried at 80 °C for 48 h to obtain a self-healing and degradable polyurethane elastomer with dual reversible dynamic covalent bonds and hydrogen bonds with NCO / (NH2+OH) of 1.3 and NH2 / OH of 1:1.
[0043] Example 3
[0044] A method for preparing a self-repairable and degradable polyurethane with dual reversible dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0045] (1) 4 g of hydroxyl-terminated polytetrahydrofuran with a molecular weight of 2000 and a substance amount of 2 mmol was placed in a three-necked flask with a stirrer, heated to 110° C., and vacuum-dried for 1 h under stirring. The mixture was then cooled to 80° C., 1.41 g of isophorone diisocyanate with a substance amount of 6.3 mmol and a drop of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued for 3 h to form a prepolymer.
[0046] (2) 0.31 g of 4-4'-diaminodiphenyl disulfide (1.25 mmol) was dissolved in 3 mL of DMF and added to the above prepolymer for chain extension reaction for 3 h. Then 0.19 g of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine (0.83 mmol) was dissolved in 3 mL of DMF and added to the above mixture solution and stirred evenly. After reacting for 45 min, the reaction solution was poured into a polytetrafluoroethylene mold and dried at 80 °C for 48 h to obtain a self-healing and degradable polyurethane elastomer with dual reversible dynamic covalent bonds and hydrogen bonds with NCO / (NH2+OH) of 1.4 and NH2 / OH of 1:1.
[0047] Example 4
[0048] A method for preparing a self-repairable and degradable polyurethane with dual reversible dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0049] (1) 4 g of hydroxyl-terminated polytetrahydrofuran with a molecular weight of 2000 and a substance amount of 2 mmol was placed in a three-necked flask with a stirrer, heated to 110° C., and vacuum-dried for 1 h under stirring. Then, the temperature was lowered to 80° C., 1.51 g of isophorone diisocyanate with a substance amount of 6.75 mmol and a drop of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued for 3 h to form a prepolymer.
[0050] (2) 0.31 g of 4-4'-diaminodiphenyl disulfide (1.25 mmol) was dissolved in 3 mL of DMF and added to the above prepolymer for chain extension reaction for 3 h. Then 0.19 g of hexahydro-1,3,5-tri(hydroxyethyl)-s-triazine (0.83 mmol) was dissolved in 3 mL of DMF and added to the above mixture solution and stirred evenly. After reacting for 45 min, the reaction solution was poured into a polytetrafluoroethylene mold and dried at 80 °C for 48 h to obtain a self-healing and degradable polyurethane elastomer with dual reversible dynamic covalent bonds and hydrogen bonds with NCO / (NH2+OH) of 1.5 and NH2 / OH of 1:1.
[0051] Example 5
[0052] A method for preparing a self-repairable and degradable polyurethane with dual reversible dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0053] (1) 4 g of hydroxyl-terminated polytetrahydrofuran with a molecular weight of 2000 and a substance amount of 2 mmol was placed in a three-necked flask with a stirrer, heated to 110° C., and vacuum-dried for 1 h under stirring. Then, the temperature was lowered to 80° C., 1.34 g of isophorone diisocyanate with a substance amount of 6 mmol and a drop of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued for 3 h to form a prepolymer.
[0054] (2) 0.25 g of 1 mmol of 4-4'-diaminodiphenyl disulfide was dissolved in 3 mL of DMF and added to the above prepolymer for chain extension reaction for 3 hours. Then 0.22 g of 1 mmol of hexahydro-1,3,5-tri(hydroxyethyl)-s-triazine was dissolved in 3 mL of DMF and added to the above mixture solution and stirred evenly. After reacting for 45 minutes, the reaction solution was poured into a polytetrafluoroethylene mold and dried at 80°C for 48 hours to obtain a self-repairable and degradable polyurethane elastomer with dual reversible dynamic covalent bonds and hydrogen bonds with NCO / (NH2+OH) of 1.3 and NH2 / OH of 2:3.
[0055] Example 6
[0056] A method for preparing a self-repairable and degradable polyurethane with dual reversible dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0057] (1) 4 g of hydroxyl-terminated polytetrahydrofuran with a molecular weight of 2000 and a substance amount of 2 mmol was placed in a three-necked flask with a stirrer, heated to 110° C., and vacuum-dried for 1 h under stirring. Then, the temperature was lowered to 80° C., 1.34 g of isophorone diisocyanate with a substance amount of 6 mmol and a drop of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued for 3 h to form a prepolymer.
[0058] (2) 0.37 g of 4-4'-diaminodiphenyl disulfide (1.5 mmol) was dissolved in 3 mL of DMF and added to the above prepolymer for chain extension reaction for 3 h. Then 0.15 g of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine (0.67 mmol) was dissolved in 3 mL of DMF and added to the above mixture solution and stirred evenly. After reacting for 45 min, the reaction solution was poured into a polytetrafluoroethylene mold and dried at 80 °C for 48 h to obtain a self-healing and degradable polyurethane elastomer with dual reversible dynamic covalent bonds and hydrogen bonds with NCO / (NH2+OH) of 1.3 and NH2 / OH of 3:2.
[0059] Example 7
[0060] A method for preparing a self-repairable and degradable polyurethane with dual reversible dynamic covalent bonds and hydrogen bonds, comprising the following steps:
[0061] (1) 4 g of hydroxyl-terminated polycaprolactone with a molecular weight of 2000 and a substance amount of 2 mmol was placed in a three-necked flask with a stirrer, heated to 110° C., and vacuum-dried for 1 h under stirring. Then, the temperature was lowered to 80° C., 1.34 g of isophorone diisocyanate with a substance amount of 6 mmol and a drop of dibutyltin dilaurate (DBTDL) were added, and the reaction was continued for 3 h to form a prepolymer.
[0062] (2) 0.37 g of 4-4'-diaminodiphenyl disulfide (1.5 mmol) was dissolved in 3 mL of DMF and added to the above prepolymer for chain extension reaction for 3 h. Then 0.15 g of hexahydro-1,3,5-tris(hydroxyethyl)-s-triazine (0.67 mmol) was dissolved in 3 mL of DMF and added to the above mixture solution and stirred evenly. After reacting for 45 min, the reaction solution was poured into a polytetrafluoroethylene mold and dried at 80 °C for 48 h to obtain a self-repairable and degradable polyurethane elastomer with dual reversible dynamic covalent bonds and hydrogen bonds with NCO / (NH2+OH) of 1.3 and NH2 / OH of 1:1.
[0063] See also Figure 1 The polyurethane elastomers prepared in Examples 1-6 contain dual reversible dynamic covalent bonds and hydrogen bonds, which form physical crosslinking points through the crosslinking points of the thermally reversible exchange of disulfide bonds and the multiple hydrogen bonds between the urea bonds and the carbamate bonds in the structure. The synergistic effect of the two further promotes the microphase separation of the polyurethane elastomer, so that the elastomer has high tensile strength, high toughness and high resilience. In addition, since the structure contains acid-sensitive hexahydrotriazine rings, the elastomer can be quickly degraded and completely in a weak acid environment. Due to the reversible properties of reversible covalent bonds and hydrogen bonds, the elastomer has excellent self-healing and processability. The presence of hydrogen bonds is conducive to the rapid repair of the elastomer, and the combined action of hydrogen bonds and reversible covalent bonds is conducive to deep repair of the elastomer. The self-healing, strength and toughness of the elastomer can be adjusted by adjusting the ratio of soft and hard segments in the polyurethane structure.
[0064] See also Figure 2 The different NCO / (OH+NH2) and NH2:OH of PU elastomer were characterized by ATR-FTIR at 3330cm -1 and 1542cm -1 The absorption peaks at 2937cm- -1 and 2854cm -1The absorption peaks at 1703 cm-1 are the symmetric and antisymmetric stretching vibration peaks of CH. In addition, the stretching vibration peak of C=O in carbamate is located at 1703 cm-1. -1 Nearby, at 1454cm -1 and 1366cm -1 The bending vibration of -CH2- can also be observed at 2260cm -1 No characteristic peak of -NCO was found, indicating that the remaining -NCO reacted completely with hydroxyethylhexahydro-s-triazine.
[0065] See also Figure 3 After obvious scratches were made on the surface of the polyurethane elastomer prepared in Example 5 with a blade, the surface was initially healed and then self-healed at 100°C. Through microscopic observation, the scratches disappeared, indicating its excellent self-healing performance.
[0066] See also Figure 4 , the stress-strain curve of the second stretching after an interval of 5 minutes is significantly lower than that of the first stretching. Although the strength when stretched to a strain of 200% increases with the extension of the interval time, the strength of the second stretching after 30 minutes has not been fully restored. This is because some hydrogen bonds have been damaged and broken during the first stretching, and the repair time is not enough for a large number of hydrogen bonds to reorganize. Figure 3 It can be found that when the interval between the second stretching and the first stretching is 12 hours, its stress-strain curve almost overlaps with the curve of the first stretching. The above table also further illustrates that the strength of 200% strain after 12 hours is higher than the strength after 30 minutes, and the longer the interval, the more conducive to the recovery of the strength of the elastomer. The tensile strength recovery rate of the elastomer after 12 hours is as high as 99.7%, so the reorganization after the hydrogen bond is broken is one of the key factors in the recovery of the mechanical properties of the elastomer.
[0067] See also Figure 5 , the polyurethane elastomer strip prepared in Example 5 was cut from the middle, the fracture surfaces were connected together, and the initial healing at room temperature was quickly achieved, and then it was repaired under heating conditions at 100°C. As time went on, the repair efficiency gradually increased. The tensile strength of the original polyurethane sample was 46.4Mpa, and the elongation at break was 932.6%. The repair efficiency of the polyurethane elastomer at 100°C for 4h, 8h, 12h, 18h and 24h reached 17%, 48%, 61%, 76% and 98% respectively. After repairing at 100°C for 24h, the tensile strength could reach 45.7Mpa. As the repair time was extended from 4h to 24h, during the longer repair time, the molecular chains had more time to diffuse to the damaged area, which was conducive to the reorganization of the dissociated disulfide bonds and hydrogen bonds, thereby increasing the repair efficiency of the elastomer over time.
[0068] See also Figure 6, using the reversibility of the disulfide bond and hydrogen bond dynamic network, the prepared elastomer can be recycled and reused through traditional polymer preparation methods. The hot pressing recycling method is to cut the film into pieces and then lay them together, and then clamp the upper and lower layers on a stainless steel mold plate, hot press for 1 hour under 0.5MPa and 100℃, and finally wait for the plate to cool to get a flat film. After recycling, its tensile strength and elongation at break decreased. After the third recycling, the tensile strength and elongation at break were still as high as 36.6Mpa and 871% respectively.
[0069] See also Figure 7 Four polyurethane elastomer films with different proportions were placed in a 1 mol / L phosphoric acid-ethanol solution for degradation experiments, and it was found that they could all be quickly and completely degraded at room temperature.
[0070] The above content is a further detailed description of the present invention in combination with specific implementation methods, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, they can also make several substitutions or modifications to these described embodiments without departing from the concept of the present invention, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention.
Claims
1. A self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds, characterized in that: The polyurethane structure is based on two reversible dynamic covalent bonds and multiple hydrogen bonds; its strength and toughness are regulated by the ratio of soft and hard segments. The structural diagram of its synthesis reaction process is as follows:
2. A method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds as claimed in claim 1, characterized in that: The following steps are involved: (1) Under a nitrogen atmosphere, weighing a hydroxyl-terminated polyether / polyester after vacuum drying and dehydration, adding a diisocyanate, and prepolymerizing under the action of a catalyst to obtain an -NCO-terminated polyurethane prepolymer; dissolving a chain extender 4,4-diaminodiphenyl sulfide in an organic solvent, adding the chain extender to the reaction system for a chain extension reaction, and the mixture obtained by the reaction is a polyurethane chain extension product based on a disulfide bond self-healing structure; (2) Continue to add hydroxyethyl hexahydrotriazine to the polymerization system in step (1) to continue the reaction, then pour the reaction solution into a polytetrafluoroethylene mold for leveling, put it into an oven to volatilize the solvent, and obtain a self-repairable, reprocessable and degradable polyurethane material.
3. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds as claimed in claim 2, characterized in that: The hydroxyl-terminated polyether / polyester described in step (1) includes one or more of hydroxyl-terminated polyethylene glycol, polypropylene glycol, polybutylene glycol, polycaprolactone, and polybutylene succinate.
4. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds as claimed in claim 2, characterized in that: The diisocyanate described in step (1) includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate.
5. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds as claimed in claim 2, characterized in that: The catalyst described in step (1) includes one or more of dibutyltin dilaurate, N,N-dimethylcyclohexylamine, and stannous isooctanoate, and the amount used accounts for 0.05-0.1wt% of the total mass of the reactants.
6. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds as claimed in claim 2, characterized in that: The group ratio of NCO:(OH+NH2) in step (1) is (1.2-1.5):
1.
7. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds as claimed in claim 2, characterized in that: The reaction time in step (2) is 45 min.
8. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds as claimed in claim 2, characterized in that: The solvent described in step (2) includes one or more of N-dimethylformamide, tetrahydrofuran, dimethylene sulfoxide, and N-methylpyrrolidone.
9. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds according to any one of claims 2 to 8, characterized in that: The preparation conditions are heating and stirring the reaction at 80°C for 2-3 hours, and after curing, a self-repairing, repeatedly processable and degradable polyurethane material based on multiple bond effects is obtained.
10. The method for preparing a self-repairable, reprocessable and degradable polyurethane material based on dual dynamic covalent bonds and hydrogen bonds according to claim 9, characterized in that: The curing time is 24h.
Citation Information
Patent Citations
Shape memory intrinsic type self-repairing material as well as preparation method and application thereof
CN105802195A
Conductive ink composition with self-repair functions, method for preparing conductive ink composition and application thereof
CN106833129A
Polyurethane modified organic silicone water-repellency and antibiotic finishing agent, preparation method and application
CN107059405A
High-stability polyurethane / quantum dot elastomer composite material and preparation method thereof
CN113651984A
Preparation method of super-tough polyurethane cross-linked network
CN116284638A
Cited By
Polycaprolactone-based functional polyurethane material as well as preparation method and application thereof
CN119463090A
A polycaprolactone-based functional polyurethane material, a preparation method and applications thereof
CN119463090B
Polyurethane material with shape memory function, biocompatibility and degradability and preparation method thereof
CN119463091A
A polyurethane material with shape memory function, biocompatibility and degradability and a preparation method thereof
CN119463091B
Preparation method and application of degradable and fluorescent self-repairing polyurethane film
CN119751935A