Method for continuously preparing MOF-303 metal framework material and purification method
Through continuous flow method and ultrasonic water bath purification method, the problems of long time and large solvent usage in the preparation and purification of MOF-303 are solved, and high-efficiency and low-cost large-scale production and acquisition of high-purity products are achieved.
Patent Information
- Application Number
- CN202411275608.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing MOF-303 preparation methods exist in the problems of long time, large solvent usage, high cost and difficulty in large-scale production. Especially the difficulties in batch operations and solvent reuse in the existing technology, which limits its large-scale production and purification efficiency. .
MOF-303 is prepared by continuous flow method, and the continuous flow reaction of mixed solutions in the reactor is combined with the purification method of ultrasonic water bath to shorten the reaction time, reduce the amount of solvent, and achieve repeatable recovery of solvents, which is suitable for large-scale production.
It realizes efficient continuous preparation and purification of MOF-303, with short reaction time, high spatiotemporal yield and low solvent usage, which reduces the preparation cost, is suitable for large-scale production, and improves purification efficiency.
Smart Images

Figure CN118930896A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal skeleton materials, and in particular to a method for continuously preparing a MOF-303 metal skeleton material and a method for purifying a crude MOF-303 product prepared by the method for continuously preparing a MOF-303 metal skeleton material. Background Art
[0002] MOF-303 is a new type of aluminum-based MOF material that can extract water from the air. [1] , seawater desalination [2] , Excessive metal separation [3] , Gas Separation [4] The water reserves in the atmosphere account for about 10% of the total fresh water resources available to humans, which can effectively alleviate the plight of water shortage. However, it is still difficult to collect water in the atmosphere under low humidity conditions. MOF-303 has a higher adsorption capacity for water under low humidity conditions. Fathieh et al. [1] AlCl3·6H2O and 3,5-pyrazole dicarboxylic acid were dissolved in water by hydrothermal synthesis, NaOH was added to the water, stirred and dripped into the above mixture, and then sealed in a bottle, heated at 100°C for 24 hours, and the resulting white precipitate was separated by filtration. Washed with water 3 times a day for 3 days, then washed with methanol 3 times a day, filtered and dried after 3 days. Comparing MOF-303 with 13X and MOF-801, MOF-303 has 175g water / kg MOF The water extraction rate far exceeds that of other materials, which strongly proves the advantage of MOF-303 in extracting water from desert air. Seawater desalination is also a way to obtain fresh water. Cong et al. [2] A continuous polycrystalline MOF-303 membrane was prepared on a porous α-Al2O3 substrate by an in-situ hydrothermal synthesis method. The synthesized membrane has a high divalent ion removal rate of 93.5% for MgCl2 and 96.0% for Na2SO4. These properties indicate that MOF-303 is a promising water softening membrane material. MOF-303 has certain prospects in the separation and recovery of transition metals. Liu et al. [3] Using the reflux method, AlCl3·6H2O and 3,5-pyrazole dicarboxylic acid were dissolved in deionized water. Then, NaOH aqueous solution was slowly added. MOF-303 was synthesized by reflux in an oil bath at 100°C for 24 hours. The synthesized MOF-303 was prepared from Cu 2+ / Ni 2+ and Cu 2+ / Co 2+ Selective capture of Cu in polluted wastewater 2+ It has large adsorption capacity and good separation selectivity, and can be used from Cu 2+ / Ni2+ The Ni-based product with high purity (98.9%) was recovered from the solution. MOF-303 can be effectively used in C2H2 / C2H4 separation, C2H2 / CO2 separation, etc., and the separation effect is significantly improved compared with other industrial adsorbents. Xian et al. [4] AlCl3·6H2O and 3,5-pyrazoledicarboxylic acid were dissolved in water, and NaOH aqueous solution was dripped into the above mixture. The flask was refluxed at 100℃ for 12h to synthesize MOF-303. The separation effect of MOF-303 on C2 hydrocarbons was studied, showing high C2H6 absorption rate and good C2H6 / C2H4 selectivity. The C2H6 absorption rate of MOF-303 at 298K and 1bar was as high as 4.96mmol g -1 , which is superior to most ethane-selective MOFs reported so far. Considering the ultrahigh C2H2 adsorption at low pressure (e.g., 0.1 bar), the adsorption capacity of MOF-303 is 2.42 mmol g -1 , and an excellent C2H2 / C2H4 selectivity of 2.45. MOF-303, an aluminum-based MOF, has achieved a good balance between stability, cost, and performance, and is expected to become a candidate material for industrial adsorption-based C2H4 purification.
[0003] However, the key to transforming existing MOFs into commercial materials lies in the ability to produce them on a large scale, with high purity and at low cost. [1] et al. synthesized MOF-303 for the first time by hydrothermal method, using water solvent, aluminum chloride hexahydrate and 3,5-pyrazoledicarboxylic acid monohydrate as reaction raw materials, adding NaOH, heating at 100 ° C for 24 hours; the crude product was washed with water 3 times for 72 hours with a liquid-to-solid ratio of 50; then washed with methanol 3 times for 72 hours with a liquid-to-solid ratio of 50, filtered and dried in air. Zheng et al. [5] MOF-303 is synthesized by hydrothermal synthesis, reflux and microwave methods. Intermittent purification is used to centrifuge the crude product, add water to the purified liquid-solid ratio of 80, mix evenly, and centrifuge again to repeat the above process twice. After adding ethanol at the same liquid-solid ratio of 80 and repeating the above washing steps twice, the washed MOF-303 is dried in air overnight. The prepared MOF-303 can be obtained from the 25°C water absorption isotherm. Its static adsorption capacity is 0.32g / g at a relative humidity of 20%, and its static adsorption capacity is 0.42g / g at a relative humidity of 74%. The stability at 400°C is good. CN115449087A discloses a method for preparing MOF-303 by atmospheric pressure reflux method. After the reaction is completed at 100°C for 15h, the precipitate is filtered out and the purified liquid-solid ratio is 250. It is washed 3 times with deionized water; then washed 3 times with anhydrous methanol at a liquid-solid ratio of 250, 500mL each time.
[0004] The hydrothermal synthesis method is an intermittent operation and takes a long time to synthesize. The microwave method has a high space-time yield, but is limited by the volume of the microwave synthesizer and is only suitable for small-scale synthesis. The solvothermal method is simple to operate, but has a low yield. The reflux method can be expanded to 10mL-5000mL, and the MOF-303 yield is >90%, but it is still an intermittent operation and is limited by the size of the flask. At the same time, the current purification methods are all intermittent purification, which takes a long time, uses a large amount of solvent, and is difficult to recycle. Summary of the invention
[0005] In view of this, in order to solve the above-mentioned problems existing in the prior art, on the one hand, the present invention provides a method for continuously preparing MOF-303 metal skeleton materials, which prepares MOF-303 by adopting a continuous flow method, with mild synthesis conditions, short reaction time, high MOF-303 time-space yield, and small amount of solvent, which can be repeatedly recycled, effectively reducing the preparation cost of MOF-303, and is suitable for large-scale production of MOF-303.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for continuously preparing MOF-303 metal skeleton material comprises the following steps:
[0008] Step 1), 3,5-dicarboxypyrazole monohydrate, NaOH mixed solution and aluminum salt aqueous solution are pumped into a mixer respectively and mixed thoroughly to obtain a mixed solution;
[0009] Step 2), pumping the mixed solution into a reactor for reaction, and continuously preparing a crude MOF-303 product.
[0010] Preferably, in step 2), the feed flow rate is 0.5 to 2 mL / min, the reaction temperature is 85 to 120° C., and the residence time is 0.5 to 3 h.
[0011] Preferably, the reaction temperature is 90-100°C.
[0012] Preferably, the residence time is 1 to 2 hours.
[0013] Preferably, the molar ratio of 3,5-dicarboxypyrazole monohydrate: aluminum source: NaOH is 1: (0.8-1.2): (2.5-3.5).
[0014] On the other hand, the present invention also provides a method for purifying a MOF-303 metal skeleton material, comprising the following steps:
[0015] Step 3), the crude MOF-303 product prepared by the above-mentioned method for continuously preparing the MOF-303 metal skeleton material and the purified solvent are pumped into a mixer and mixed to obtain a purified mixed solution;
[0016] Step 4), pumping the purified mixed solution in step 3) into the coil of an ultrasonic water bath for purification, separation, drying, and refining to obtain the MOF-303 product.
[0017] Preferably, in step 3), the liquid-to-solid ratio of the MOF-303 crude product and the purification solvent is 10 to 70 mL / g.
[0018] Preferably, in step 4), the feed flow rate is 1-10 mL / min, the purification temperature is 30-70° C., the ultrasonic frequency is 30-130 KHz, and the purification time is 2-20 min.
[0019] Preferably, the purification time is 2 to 10 minutes.
[0020] Preferably, the purification is performed 1 to 2 times.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The method for continuously preparing MOF-303 metal skeleton material provided by the present invention adopts a continuous flow method to prepare MOF-303, with mild synthesis conditions and short reaction time, and the maximum space-time yield of MOF-303 can reach 1851kg·m -3 ·day -1 , and the solvent consumption is small, and it can be recycled repeatedly, which effectively reduces the preparation cost of MOF-303 and is suitable for large-scale production of MOF-303.
[0023] The method for purifying the MOF-303 metal skeleton material provided by the present invention can continuously purify MOF-303 with high purification efficiency, and can provide a new approach for large-scale production of MOF-303. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope image of MOF-303 synthesized in Example 1 of the present invention;
[0025] Figure 2 The XRD spectrum of MOF-303 synthesized in Example 1 of the present invention;
[0026] Figure 3 This is the N2 adsorption-desorption isotherm of MOF-303 synthesized in Example 1 of the present invention;
[0027] Figure 4 This is the adsorption isotherm of water for MOF-303 synthesized in Example 1 of the present invention at 25°C;
[0028] Figure 5 This is the thermogravimetric curve of MOF-303 synthesized in Example 1 of the present invention. DETAILED DESCRIPTION
[0029] The present invention provides a method for continuously preparing MOF-303 metal skeleton material, comprising the following steps:
[0030] Step 1), 3,5-dicarboxypyrazole monohydrate, NaOH mixed solution and aluminum salt aqueous solution are pumped into a mixer and mixed thoroughly to obtain a mixed solution, wherein the molar ratio of 3,5-dicarboxypyrazole monohydrate: aluminum source: NaOH is preferably 1: (0.8-1.2): (2.5-3.5), such as 1: (0.8-1): (2.5-3), 1: (0.9-1.2): (3-3.5), etc., which can be selected according to actual needs;
[0031] Step 2), pumping the mixed solution into the reactor for reaction, and continuously preparing the crude MOF-303 product, wherein the reaction conditions are preferably: the feed flow rate is 0.5-2 mL / min (e.g., 40-120 mL / min, 30-40 mL / min, etc., which can be selected according to actual needs), the reaction temperature is 85-120°C (e.g., 90-100°C, 95-120°C, 85-95°C, etc., which can be selected according to actual needs), and the residence time is 0.5-3 h (e.g., 1-2 h, 1.5-3 h, etc., which can be selected according to actual needs).
[0032] In the above-mentioned method for continuously preparing MOF-303 metal skeleton material provided by the present invention, the mixer can be selected as a T-type mixer, the reaction gas can be preferably a coil reactor with a volume of 15-360mL, and the 3,5-dicarboxylpyrazole monohydrate, the NaOH mixed solution and the aluminum salt aqueous solution and the mixed solution thereof are preferably pumped into the mixer and the reactor by a peristaltic pump. The aluminum salt aqueous solution is preferably an AlCl3·6H2O aqueous solution.
[0033] In the method for continuously preparing MOF-303 metal skeleton material provided by the present invention, the yield is as high as 92%, and the time-space yield is as high as 1851 kg·m -3 ·day -1 .
[0034] On the other hand, the present invention also provides a method for purifying a MOF-303 metal skeleton material, comprising the following steps:
[0035] Step 3), the crude MOF-303 prepared by the above-mentioned method for continuously preparing MOF-303 metal skeleton material and the purified solvent are pumped into a mixer for mixing to obtain a purified mixed solution, wherein the liquid-to-solid ratio of the crude MOF-303 product and the purified solvent is preferably 10-70 mL / g (e.g., 10-30 mL / g, 10-20 mL / g, 10-30 mL / g, 20-30 mL / g, etc., which can be selected according to actual needs);
[0036] Step 4), pump the purified mixed solution in step 3) into the coil of an ultrasonic water bath for purification, separation, drying, and refinement to obtain the MOF-303 product, wherein the purification conditions are preferably: a feed flow rate of 1 to 10 mL / min (e.g., 2 to 4 mL / min, 4 to 10 mL / min, etc., which can be selected according to actual needs), a purification temperature of 30 to 70°C (e.g., 30 to 50°C, 40 to 50°C, 30 to 40°C, etc., which can be selected according to actual needs), an ultrasonic frequency of 30-130 KHz (e.g., 40-130 KHz, 40-120 KHz, 30-40 KHz, etc., which can be selected according to actual needs), and a purification time of 2 to 20 min (e.g., 3 to 10 min, 4 to 10 min, etc., which can be selected according to actual needs).
[0037] In the purification method provided by the present invention, the purification times are preferably 1 to 2 times.
[0038] In the purification method provided by the present invention, the separation method is preferably centrifugal separation, the centrifugal speed is preferably 8000-12000 r / min, the centrifugal time is preferably 4-10 min. The drying conditions are: the drying temperature is preferably 60-80° C., and the drying time is preferably 8-24 h.
[0039] The MOF-303 metal skeleton material purified by the above purification method provided by the present invention has a static water adsorption capacity of 0.30-0.34 g / g in a saturated potassium acetate solution at 25°C (relative humidity 21%); and a static water adsorption capacity of 0.42-0.43 g / g in a saturated salt water solution at 25°C (relative humidity 74%).
[0040] The technical solution of the present invention is clearly described in detail below in conjunction with specific embodiments.
[0041] Example 1
[0042] The mixed solution of 3,5-dicarboxypyrazole monohydrate and NaOH (molar ratio of 3) and AlCl3·6H2O aqueous solution (molar ratio of AlCl3·6H2O to 3,5-dicarboxypyrazole monohydrate of 1) were pumped at 40 h for 1 h. -1 The feed space velocity was respectively mixed with a T-type mixer through a peristaltic pump and then entered into a PFA coil reactor (volume 60 mL) for reaction. The reaction temperature was 95° C. and the residence time was 1.5 h. The crude MOF-303 was continuously prepared.
[0043] The crude MOF-303 product and ethanol (liquid-to-solid ratio 20 mL / g) were respectively fed into a T-type mixer through a peristaltic pump, and the mixed solution was fed into a PFA coil reactor (volume 40 mL) in an ultrasonic bath. The ultrasonic frequency was 130 KHz, the feed flow rate was 10 mL / min, the purification temperature was 30°C, and the purification time was 4 min. The purified product was centrifuged at a centrifugal speed of 8000 r / min and a centrifugal time of 5 min. The solid sample was dried at 60°C for 24 h to obtain a purified MOF-303 product. The purity of the MOF-303 product was >99% (the purity of MOF-303 before purification was 82.4%). The yield of MOF-303 was 92%, and the space-time yield was 740 kg·m -3 ·day -1 The static water adsorption capacity of MOF-303 in saturated potassium acetate solution at 25°C (relative humidity 21%) is 0.34 g / g; the static water adsorption capacity in saturated salt water at 25°C (relative humidity 74%) is 0.43 g / g.
[0044] Example 2
[0045] The mixed solution of 3,5-dicarboxypyrazole monohydrate and NaOH (molar ratio of 2.5) and AlCl3·6H2O aqueous solution (molar ratio of AlCl3·6H2O to 3,5-dicarboxypyrazole monohydrate of 0.8) were respectively stirred for 120 h by peristaltic pump. -1 The feed space velocity was respectively mixed with a T-type mixer through a peristaltic pump and then entered into a PFA coil reactor (volume 360 mL) for reaction. The reaction temperature was 85° C. and the residence time was 3 h. MOF-303 crude product was continuously prepared.
[0046] The crude MOF-303 product and ethanol (liquid-solid ratio 10mL / g) were respectively fed into a T-type mixer through a peristaltic pump, and the mixed solution was fed into a PTFE coil reactor (volume 20mL) in an ultrasonic bath, with an ultrasonic frequency of 120KHz, a feed flow rate of 2mL / min, a purification temperature of 40°C, and a purification time of 10min; the purified product was centrifuged at a centrifugal speed of 8000r / min and a centrifugal time of 4min; methanol solvent was selected to repeat the above purification steps twice; after pouring out the supernatant, the solid sample was dried at 80°C for 12h to obtain the purified MOF-303 product. The purity of the MOF-303 product was 99% (the purity of MOF-303 before purification was 71.6%); the yield of MOF-303 was 85%, and the space-time yield was 312kg·m -3 ·day -1 The static water adsorption capacity of MOF-303 in saturated potassium acetate solution at 25°C (relative humidity 21%) is 0.33 g / g; the static water adsorption capacity in saturated salt water at 25°C (relative humidity 74%) is 0.42 g / g.
[0047] Example 3
[0048] The mixed solution of 3,5-dicarboxypyrazole monohydrate and NaOH (molar ratio of 3.5) and AlCl3·6H2O aqueous solution (molar ratio of AlCl3·6H2O to 3,5-dicarboxypyrazole monohydrate was 1.2) were respectively stirred for 30 h by peristaltic pump. -1 The feed space velocity was respectively mixed with a T-type mixer through a peristaltic pump and then entered into a stainless steel coil reactor (volume 15 mL) for reaction. The reaction temperature was 120° C. and the residence time was 0.5 h. MOF-303 crude product was continuously prepared.
[0049] The crude MOF-303 product and ethanol (liquid-solid ratio 30mL / g) were respectively fed into a T-type mixer through a peristaltic pump, and the mixed solution was fed into a PTFE coil reactor (volume 16mL) in an ultrasonic bath, with an ultrasonic frequency of 40KHz, a feed flow rate of 4mL / min, a purification temperature of 50°C, and a purification time of 3min; the purified product was centrifuged at a centrifugal speed of 12000r / min and a centrifugal time of 10min; ethanol was selected as the solvent and the above purification steps were repeated once; after the supernatant was poured out, the solid sample was dried at 70°C for 8h to obtain the purified MOF-303 product. The purity of the MOF-303 product was 99% (the purity of MOF-303 before purification was 53.1%); the yield of MOF-303 was 75%, and the space-time yield was 1851kg·m -3 ·day -1 The static water adsorption capacity of MOF-303 in saturated potassium acetate solution at 25°C (relative humidity 21%) is 0.30 g / g; the static water adsorption capacity in saturated salt water at 25°C (relative humidity 74%) is 0.42 g / g.
[0050] Comparative Example 1
[0051] Hydrothermal synthesis of MOF-303
[0052] Dissolve 3.48 g of 3,5-dicarboxypyrazole monohydrate in an aqueous solution containing 2.4 g of NaOH (the concentration of the aqueous solution of NaOH is 3.2 mg / mL, and the molar ratio of 3,5-dicarboxypyrazole monohydrate to NaOH is 1:1), and continue stirring until a clear solution is obtained. Then add 4.82 g of AlCl3·6H2O (the concentration of the aqueous solution of AlCl3 is 64.3 mg / mL) to the solution, repeatedly ultrasonicate and stir to dissolve the precipitate. Place the mixture in a Teflon-lined high-pressure closed reactor, react in an oven at 100°C for 24 hours, and centrifuge at 6000 rpm for 3 minutes to separate the solid. Transfer 60 mL of the reaction mixture to 2×50 mL covered centrifuge tubes (30 mL per tube). Centrifuge at 6050 r / min for 1 minute at room temperature to separate the solid, pour off the supernatant, add 40 mL of water and mix evenly. Centrifuge again and repeat the above process twice. After adding 40 mL of ethanol and repeating the above washing steps twice, the washed MOF-303 was dried in air overnight. The purity of MOF-303 product was 99% (the purity of MOF-303 before purification was 42%); the yield of MOF-303 was 25%. The hydrothermal synthesis method was a batch reaction, and the reaction time required 24 hours, the yield was low, and the synthesis time was long. Its time-space yield was only 3 kg·m -3 ·day -1 The static water adsorption capacity of MOF-303 in saturated potassium acetate solution at 25°C (relative humidity 21%) is 0.31 g / g; the static water adsorption capacity in saturated salt water at 25°C (relative humidity 74%) is 0.42 g / g.
[0053] Comparative Example 2
[0054] Synthesis of MOF-303 by reflux method
[0055] Add 1.044g 3,5-dicarboxypyrazole monohydrate and 30mL NaOH solution dissolved with 0.72g to a 150mL round-bottom flask. Dissolve AlCl3·6H2O (1.446g) in 30mL deionized water. Then slowly add 30mL AlCl3·6H2O solution to the mixed solution of 3,5-dicarboxypyrazole monohydrate and NaOH at a rate of 60mL per hour, with a total addition time of 0.5h. Transfer the round-bottom flask to an oil bath, react at 120℃ for 2 hours, and centrifuge at 6000 rpm for 3min to separate the solid. Transfer 60mL of the reaction mixture to 2×50mL covered centrifuge tubes (30mL per tube). Centrifuge at 6050r / min for 1 minute at room temperature to separate the solid, pour off the supernatant and add 40mL water to mix evenly. Centrifuge again and repeat the above process twice. After adding 40 mL of ethanol and repeating the above washing steps twice, the washed MOF-303 was dried in air overnight. The purity of MOF-303 product was 99% (the purity of MOF-303 before purification was 78.3%); the yield of MOF-303 was 90%, and the space-time yield was 85 kg·m -3 ·day -1 The static water adsorption capacity of MOF-303 in saturated potassium acetate solution at 25°C (relative humidity 21%) is 0.33 g / g; the static water adsorption capacity in saturated salt water at 25°C (relative humidity 74%) is 0.43 g / g.
[0056] Comparative Example 3
[0057] Microwave Synthesis of MOF-303
[0058] Add 522 mg of 3,5-dicarboxypyrazole monohydrate and 360 mg of NaOH to a 20 mL microwave reactor. Add 12 mL of deionized water to the reactor and stir the solution with a stirring bar for 10 minutes to dissolve the solid. Prepare 723 mg of AlCl3·6H2O solution with 3 mL of deionized water in another 20 mL microwave reactor. Transfer the solutions in the two vials to a 35 mL microwave reactor. The solution becomes turbid immediately after the liquids are mixed. Place a magnetic stirring bar in the microwave reactor and seal it with a silicone cap. Heat the reaction mixture to 120 °C at 300 W in the microwave reactor while stirring for 10 minutes. Cool the reaction mixture to room temperature, and the MOF-303 product will appear at the bottom of the vial as a white precipitate. Transfer 15 mL of the reaction mixture to a 50 mL covered centrifuge tube. Centrifuge at 6050 r / min for 1 minute at room temperature to separate the solids, pour off the supernatant and add 40 mL of water to mix evenly. Centrifuge again and repeat the above process twice. After adding 40 mL of ethanol and repeating the above washing steps twice, the washed MOF-303 was dried in air overnight. The purity of MOF-303 product was 99% (the purity of MOF-303 before purification was 82.8%); the yield of MOF-303 was 90%, and the space-time yield was 280 kg·m -3 ·day -1 The static water adsorption capacity of MOF-303 in saturated potassium acetate solution at 25°C (relative humidity 21%) is 0.34 g / g; the static water adsorption capacity in saturated salt water at 25°C (relative humidity 74%) is 0.43 g / g.
[0059] It can be seen from the above Examples 1-3 and Comparative Examples 1-3 that the present invention can achieve a static water adsorption amount equivalent to that of the prior art, and the synthesis time of the present invention is much lower than that of the prior art, and the time-space yield is much higher than that of the prior art.
[0060] The above are only preferred specific implementations of the present invention; however, the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and improved concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0061] The references cited in the background technology are as follows:
[0062] [1] Fathieh F, Kalmutzki MJ, Kapustin EA, et al. Practical waterproduction from desert air. Science advances 4.6 (2018): eaat3198.
[0063] [2]Cong S Z,Yuan Y,Wang J X,et al.Highly water-permeable metal-organic framework MOF-303membranes for desalination.Journal oftheAmericanChemical Society 143.48(2021):20055-20058。
[0064] [3]Liu B,Pei L,Zhao X,et al.Synergistic dual-pyrazol sites ofmetal-organic framework for efficient separation and recovery oftransition metalsfrom wastewater.Chemical Engineering Journal 410(2021):128431。
[0065] [4]Xian S K,Peng J J,Pandey H,et al.Simultaneous removal of C2H2andC2H6 for C2H4 purification by robust MOFs featuring a high densityofheteroatoms[J].Journal ofMaterials ChemistryA,2023,11(39):21401-21410。
[0066] [5]Zheng Z L,Nguyen H L,Hanikel N,et al.High-yield,green andscalablemethods for producing MOF-303 for water harvesting from desert air[J].NatureProtocols 18.1(2023):136-156。
Claims
1. A method for continuously preparing MOF-303 metal skeleton material, characterized in that: The steps include: Step 1), 3,5-dicarboxypyrazole monohydrate, NaOH mixed solution and aluminum salt aqueous solution are pumped into a mixer respectively and mixed thoroughly to obtain a mixed solution; Step 2), pumping the mixed solution into a reactor for reaction, and continuously preparing a crude MOF-303 product.
2. The method for continuously preparing MOF-303 metal skeleton material according to claim 1, characterized in that: In step 2), the feed flow rate is 0.5-2 mL / min, the reaction temperature is 85-120° C., and the residence time is 0.5-3 h.
3. A method for continuously preparing MOF-303 metal skeleton material according to claim 2, characterized in that: The reaction temperature is 90-100°C.
4. The method for continuously preparing MOF-303 metal skeleton material according to claim 2, characterized in that: The residence time is 1 to 2 hours.
5. A method for continuously preparing MOF-303 metal skeleton material according to any one of claims 1 to 4, characterized in that: The molar ratio of 3,5-dicarboxypyrazole monohydrate: aluminum source: NaOH is 1:(0.8-1.2):(2.5-3.5).
6. A method for purifying MOF-303 metal framework material, characterized in that: The steps include: Step 3), pumping the crude MOF-303 product prepared by the method for continuously preparing MOF-303 metal skeleton material described in any one of claims 1 to 5 and the purified solvent into a mixer and mixing them to obtain a purified mixed solution; Step 4), pumping the purified mixed solution in step 3) into the coil of an ultrasonic water bath for purification, separation, drying, and refining to obtain the MOF-303 product.
7. The method for purifying a MOF-303 metal skeleton material according to claim 6, characterized in that: In step 3), the liquid-to-solid ratio of the MOF-303 crude product and the purification solvent is 10 to 70 mL / g.
8. The method for purifying a MOF-303 metal skeleton material according to claim 6, characterized in that: In step 4), the feed flow rate is 1-10 mL / min, the purification temperature is 30-70° C., the ultrasonic frequency is 30-130 KHz, and the purification time is 2-20 min.
9. The method for purifying a MOF-303 metal skeleton material according to claim 8, characterized in that: The purification time is 2 to 10 minutes.
10. A method for purifying a MOF-303 metal skeleton material according to claims 6-9, characterized in that: The purification times are 1 to 2 times.
Citation Information
Patent Citations
Production of metal-organic frameworks
CN107614097A
Method for continuously and rapidly purifying MOFs
CN112029105A
Method for continuously preparing nano bimetallic zeolite imidazolate framework by micro-reactor
CN112210083A
Method for continuously preparing UiO series metal framework material through mother liquor dehydration circulation
CN113248726A
Micron-sized MOF-303 and preparation method thereof
CN113549223A
Cited By
Preparation method and application of organosilicon / MOF-303 mixed matrix membrane
CN119524645A
Preparation method and application of a hybrid silicone / mof-303 matrix membrane
CN119524645B