Bio-based antibacterial packaging material and preparation method thereof
By preparing antibacterial substrates, combined with doped zinc oxide, modified chitosan and polygroup silicone react with polylactic acid, the problems of non-degradable and poor antibacterial performance of traditional packaging materials are solved, and bio-based antibacterial packaging is achieved The material's efficient inhibits bacterial growth and environmentally friendly degradability.
Patent Information
- Application Number
- CN202411237938.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-05
AI Technical Summary
Traditional petroleum-based plastic packaging materials are non-degradable, resulting in environmental pollution, and polylactic acid itself is not antibacterial, which limits its application in the field of antibacterial packaging.
By preparing antibacterial substrates, zinc acetate, silver nitrate and chitosan are used to form doped zinc oxide and modified chitosan, and combined with polygroup siloxane and polylactic acid to react to form bio-based antibacterial with antibacterial ability Packaging materials.
It significantly improves the antibacterial and mechanical properties of packaging materials, can effectively inhibit the growth of bacteria and mold, extend the shelf life, and has good biocompatibility and degradability, promoting the green development of the packaging industry.
Smart Images

Figure BDA0005028290360000181
Abstract
Description
Technical Field
[0001] The present invention relates to the field of packaging materials, and in particular to a bio-based antibacterial packaging material and a preparation method thereof. Background Art
[0002] Traditional food packaging materials usually use petroleum-based raw materials, which are non-renewable and difficult to degrade, and can easily cause serious pollution to the environment. With the enhancement of environmental awareness and the increase in consumer demand for healthy and safe food, traditional petroleum-based plastic packaging materials have been difficult to meet market demand due to their non-degradability and potential environmental pollution problems. Bio-based materials have gradually become a research hotspot in the field of packaging materials due to their renewable and degradable properties. Polylactic acid, as a bio-based plastic, has been widely studied due to its good biodegradability and biocompatibility. However, polylactic acid itself does not have antibacterial properties, which makes the prepared packaging material have poor antibacterial properties, limiting its application in the field of antibacterial packaging. Therefore, it is of great significance to develop a bio-based antibacterial packaging material and its preparation method. Summary of the invention
[0003] In order to overcome the above technical problems, the purpose of the present invention is to provide a bio-based antibacterial packaging material and a preparation method thereof, which solves the problem that the existing packaging materials have poor antibacterial properties and limit their application in the field of antibacterial packaging.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A bio-based antibacterial packaging material, comprising the following components in parts by weight:
[0006] 35-45 parts of antibacterial base material, 7-14 parts of plasticizer, 5-11 parts of talc, 2-6 parts of titanium dioxide, 1.5-5.5 parts of compatibilizer, 1-3 parts of antioxidant and 1-3 parts of ultraviolet absorber;
[0007] Wherein, the antibacterial substrate is prepared by the following steps:
[0008] Step s1: zinc acetate and deionized water are added to a three-necked flask equipped with a thermometer and a stirrer, and the mixture is stirred for reaction for 10-15 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, and then the pH is adjusted to 10-11 with a sodium hydroxide solution, and then the mixture is heated to 50-55° C. and stirred for reaction for 30-40 minutes, and then heated to 160-170° C. and stirred for reaction for 10-12 hours, and after the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged, and the precipitate is washed with distilled water and anhydrous ethanol for 2-3 times in sequence, and then placed in a vacuum drying oven and dried at a temperature of 60-65° C. for 2-3 hours to obtain nano zinc oxide;
[0009] Step s2: Add nano zinc oxide and deionized water to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, stir and react for 10-15 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then add silver nitrate solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the dropwise addition is completed, continue to stir and react for 1-1.5 hours, then adjust the pH to 8-9 with sodium hydroxide solution, then continue to stir and react for 4-5 hours under the condition of heating to 80-85°C, and after the reaction is completed, cool the reaction product to room temperature, then centrifuge, wash the precipitate with distilled water and anhydrous ethanol for 2-3 times in turn, then place it in a vacuum drying oven, and dry it at a temperature of 60-65°C for 2-3 hours to obtain doped zinc oxide;
[0010] Step s3: adding chitosan and acetic acid solution to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, stirring and reacting for 30-40 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then adjusting the pH to 7 with a sodium hydroxide solution, then adding isopropanol and continuing to stir and react for 20-30 minutes, then heating to 80-85°C and adding trimethylammonium chloride glycidyl solution dropwise while stirring, controlling the dropping rate to 1-2 drops / s, and continuing to stir and react for 2-3 hours after the dropwise addition is completed. After the reaction is completed, the reaction product is cooled to room temperature, then added to anhydrous ethanol, then allowed to stand and precipitate, then vacuum filtered, and the filter cake is placed in a vacuum drying oven, and dried at a temperature of 50-55°C for 2-3 hours to obtain modified chitosan;
[0011] Step s4: add glycerol, (3-chloropropyl)triethoxysilane, anhydrous potassium carbonate, potassium iodide and anhydrous toluene into a three-necked flask equipped with a stirrer, a thermometer and a nitrogen inlet tube, introduce nitrogen protection, stir and react for 30-50 minutes at a temperature of -5-0°C and a stirring rate of 300-400r / min, then raise the temperature to 80-85°C and continue to stir and react for 20-25 hours. After the reaction is completed, cool the reaction product to room temperature, then vacuum filter, rotary evaporate the filtrate to remove the solvent, then place it in a vacuum drying oven, and dry it at a temperature of 50-55°C for 2-3 hours to obtain a multi-group siloxane;
[0012] Step s5: Add polylactic acid, doped zinc oxide, modified chitosan and N,N-dimethylformamide to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, stir and react for 30-40 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to 80-85°C and continue stirring and reacting for 2-3 hours, then add the multi-group siloxane solution dropwise while stirring, control the dropping rate to 1-2 drops / s, continue stirring and reacting for 2-3 hours after the addition is completed, and after the reaction is completed, cool the reaction product to room temperature, then place it in a vacuum drying oven, and dry it at a temperature of 50-55°C for 4-5 hours to obtain an antibacterial substrate.
[0013] As a further solution of the present invention: the dosage ratio of the zinc acetate and deionized water in step s1 is 4.5-5.5 g:50 mL.
[0014] The mass fraction of the sodium hydroxide solution in step s1 is 20-25%.
[0015] As a further solution of the present invention: the usage ratio of the nano zinc oxide, deionized water and silver nitrate solution in step s2 is 5g:100-120mL:10-15mL.
[0016] As a further solution of the present invention: the mass fraction of the silver nitrate solution in step s2 is 5-9%, and the mass fraction of the sodium hydroxide solution is 20-25%.
[0017] As a further solution of the present invention: the amount ratio of the chitosan, acetic acid solution, isopropanol and glycidyl trimethylammonium chloride solution in step s3 is 5g:80-100mL:30-50mL:10-15mL.
[0018] As a further solution of the present invention: the mass fraction of the sodium hydroxide solution in step s3 is 20-25%, the mass fraction of the acetic acid solution is 1-2%, and the mass concentration of the glycidyl trimethylammonium chloride solution is 0.5-0.9 g / mL.
[0019] As a further scheme of the present invention: the dosage ratio of the glycerol, (3-chloropropyl)triethoxysilane, anhydrous potassium carbonate, potassium iodide and anhydrous toluene in step s4 is 10 mmol: 30 mmol: 35-40 mmol: 0.2-0.6 g: 100-120 mL.
[0020] As a further solution of the present invention: the dosage ratio of the polylactic acid, doped zinc oxide, modified chitosan, N,N-dimethylformamide and multi-group siloxane solution in step s5 is 10g: 0.05-0.15g: 0.4-0.8g: 100-120mL: 10-12mL.
[0021] As a further solution of the present invention: the polylactic acid in step s5 is 4032d polylactic acid, and the multi-group siloxane solution is a mixture of multi-group siloxane, deionized water and anhydrous ethanol in a mass ratio of 1-5g:85-95mL:10-15mL.
[0022] As a further solution of the present invention: a method for preparing a bio-based antibacterial packaging material comprises the following steps:
[0023] Step 1: Weigh 35-45 parts of antibacterial substrate, 7-14 parts of plasticizer, 5-11 parts of talcum powder, 2-6 parts of titanium dioxide, 1.5-5.5 parts of compatibilizer, 1-3 parts of antioxidant and 1-3 parts of ultraviolet absorber according to weight parts, and set aside;
[0024] Step 2: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0025] Step 3: The mixed material is melt-extruded through an extruder, and then granulated and pelletized to obtain a bio-based antibacterial packaging material.
[0026] As a further solution of the present invention: the plasticizer is one of dioctyl phthalate, butyl benzyl phthalate, and diisononyl phthalate.
[0027] As a further solution of the present invention: the compatibilizer is one of PP-g-ST, ABS-g-MAH and PE-g-MAH.
[0028] As a further solution of the present invention: the antioxidant is one of antioxidant 1024, antioxidant 1076 and antioxidant 1330.
[0029] As a further solution of the present invention: the ultraviolet absorber is one of the ultraviolet absorber UV-P, ultraviolet absorber UV-O and ultraviolet absorber UV-9.
[0030] Beneficial effects of the present invention:
[0031] The invention discloses a bio-based antibacterial packaging material and a preparation method thereof. The antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber are added into a mixer, stirred and mixed to obtain a mixture, and then the mixture is melt-extruded through an extruder, and then granulated and pelletized to obtain the bio-based antibacterial packaging material. The preparation method uses zinc oxide, modified chitosan and multi-group siloxane to react and modify polylactic acid to form an antibacterial substrate, thereby giving the bio-based antibacterial packaging material a strong antibacterial ability and effectively inhibiting the growth of bacteria and molds. Moreover, polylactic acid is a bio-based material and can be naturally degraded, thereby reducing pollution to the environment. Therefore, the prepared packaging material has excellent antibacterial properties, mechanical properties and biodegradability, has broad application prospects in the fields of food, medicine and medical equipment, and is of great significance for promoting the green development and sustainable development of the packaging industry.
[0032] In the process of preparing bio-based antibacterial packaging materials, an antibacterial substrate is first prepared. First, zinc acetate is used as a raw material to prepare nano zinc oxide. Then, silver ions are loaded and doped on the nano zinc oxide using silver nitrate as a raw material to obtain doped zinc oxide. Then, chitosan and trimethylammonium chloride are reacted. The amino and hydroxyl groups on the chitosan react with the epoxy groups on the trimethylammonium chloride, and a large number of quaternary ammonium groups are introduced to obtain modified chitosan. Then, glycerol and (3-chloropropyl) triethoxysilane are reacted. The hydroxyl groups on the glycerol react with the chlorine atoms on the (3-chloropropyl) triethoxysilane, and a large number of siloxane groups are introduced to obtain multi-group siloxane. Finally, polylactic acid is modified using doped zinc oxide, modified chitosan and multi-group siloxane. The multi-group siloxane is hydrolyzed to form silanols, which can be grafted onto the surface of doped zinc oxide and can also be grafted onto the surface of modified chitosan. The PLA substrate is prepared by combining PLA matrix with modified chitosan and doped zinc oxide to obtain an antibacterial substrate. The PLA substrate is prepared by combining PLA matrix with modified chitosan and doped zinc oxide to obtain an antibacterial substrate. The antibacterial substrate is prepared by combining PLA matrix with modified chitosan and doped zinc oxide to obtain an antibacterial substrate. The antibacterial substrate significantly improves the mechanical strength and toughness of the antibacterial substrate. At the same time, the quaternary ammonium group on the modified chitosan and the synergistic effect of zinc ions and silver ions in doped zinc oxide give the antibacterial substrate a strong antibacterial ability, effectively inhibit the growth of bacteria and mold, and can effectively extend the shelf life of the product in the package. The addition of multi-group siloxane can make the doped zinc oxide better dispersed in the polylactic acid, so that the antibacterial substrate has good biocompatibility and degradability, is environmentally friendly, and is of great significance for promoting the green development and sustainable development of the packaging industry. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Embodiment 1:
[0035] This embodiment is a method for preparing a bio-based antibacterial packaging material, comprising the following steps:
[0036] Step S1: 4.5 g of zinc acetate and 50 mL of deionized water are added to a three-necked flask equipped with a thermometer and a stirrer, and the mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 10 min, and then the pH is adjusted to 10 with a 20% sodium hydroxide solution by mass, and then the mixture is heated to 50° C. and stirred for reaction for 30 min, and then heated to 160° C. and stirred for reaction for 10 h. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed twice with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 60° C. for 2 h to obtain nano zinc oxide;
[0037] Step S2: 5 g of nano zinc oxide and 100 mL of deionized water are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 10 min at a temperature of 25° C. and a stirring rate of 300 r / min, and then 10 mL of a 5% silver nitrate solution is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the addition is completed, the mixture is stirred for reaction for 1 h, and then the pH is adjusted to 8 with a 20% sodium hydroxide solution, and then the mixture is stirred for reaction for 4 h at a temperature of 80° C. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed twice with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 60° C. for 2 h to obtain doped zinc oxide;
[0038] Step S3: 5 g of chitosan and 80 mL of 1% acetic acid solution are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 30 min, and then the pH is adjusted to 7 with a 20% sodium hydroxide solution, and then 30 mL of isopropanol is added to continue stirring for reaction for 20 min, and then 10 mL of 0.5 g / mL trimethylammonium chloride solution of glycidyl chloride is added dropwise while stirring at a temperature of 80° C., and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the stirring reaction is continued for 2 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to anhydrous ethanol, and then allowed to stand for precipitation, and then vacuum filtered, and the filter cake is placed in a vacuum drying oven, and dried at a temperature of 50° C. for 2 h to obtain modified chitosan;
[0039] Step S4: 10 mmol glycerol, 30 mmol (3-chloropropyl) triethoxysilane, 35 mmol anhydrous potassium carbonate, 0.2 g potassium iodide and 100 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen inlet tube, and nitrogen protection is introduced. The mixture is stirred at a temperature of -5°C and a stirring rate of 300 r / min for 30 minutes, and then the temperature is raised to 80°C and the stirring reaction is continued for 20 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered, the filtrate is rotary evaporated to remove the solvent, and then placed in a vacuum drying oven and dried at a temperature of 50°C for 2 hours to obtain a multi-group siloxane;
[0040] Step S5: 10g of polylactic acid 4032d, 0.05g of doped zinc oxide, 0.4g of modified chitosan and 100mL of N,N-dimethylformamide are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and stirred for reaction for 30min at a temperature of 25°C and a stirring rate of 300r / min, and then the temperature is raised to 80°C and the stirring reaction is continued for 2h, and then 10mL of a multi-group siloxane solution prepared by mixing multi-group siloxane, deionized water and anhydrous ethanol in a mass ratio of 1g:85mL:10mL is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the stirring reaction is continued for 2h. After the reaction is completed, the reaction product is cooled to room temperature, and then placed in a vacuum drying oven and dried at a temperature of 50°C for 4h to obtain an antibacterial substrate;
[0041] Step S6: weigh 35 parts of polylactic acid, 7 parts of plasticizer, 5 parts of talc, 2 parts of titanium dioxide, 1.5 parts of compatibilizer, 1 part of antioxidant and 1 part of ultraviolet absorber according to weight parts, and set aside; the plasticizer is dioctyl phthalate; the compatibilizer is PP-g-ST; the antioxidant is antioxidant 1024; the ultraviolet absorber is ultraviolet absorber UV-P;
[0042] Step S7: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0043] Step S8: melt-extrude the mixture through an extruder, and then granulate and pelletize to obtain a bio-based antibacterial packaging material.
[0044] Embodiment 2:
[0045] This embodiment is a method for preparing a bio-based antibacterial packaging material, comprising the following steps:
[0046] Step S1: 5 g of zinc acetate and 50 mL of deionized water are added to a three-necked flask equipped with a thermometer and a stirrer, and the mixture is stirred for reaction at a temperature of 28° C. and a stirring rate of 350 r / min for 12 min, and then the pH is adjusted to 10.5 with a 22% sodium hydroxide solution by mass, and then the mixture is heated to 52° C. and stirred for reaction for 35 min, and then heated to 165° C. and stirred for reaction for 11 h, and after the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged, and the precipitate is washed twice with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 62° C. for 2.5 h to obtain nano zinc oxide;
[0047] Step S2: 5 g of nano zinc oxide and 110 mL of deionized water are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 12 min at a temperature of 28° C. and a stirring rate of 350 r / min, and then 12 mL of a 7% silver nitrate solution is added dropwise while stirring, and the dropping rate is controlled to be 1 drop / s. After the addition is completed, the mixture is stirred for reaction for 1.2 h, and then the pH is adjusted to 8.5 with a 22% sodium hydroxide solution, and then the mixture is stirred for reaction for 4.5 h at a temperature of 82° C. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed twice with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 62° C. for 2.5 h to obtain doped zinc oxide;
[0048] Step S3: 5 g of chitosan and 90 mL of 1.5% acetic acid solution are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 35 min at a temperature of 28° C. and a stirring rate of 350 r / min, and then the pH is adjusted to 7 with a 22% sodium hydroxide solution, and then 40 mL of isopropanol is added to continue stirring for reaction for 25 min, and then 12 mL of 0.7 g / mL trimethylammonium chloride solution of glycidyl chloride is added dropwise while heating to 82° C., and the dropping rate is controlled to be 1 drop / s. After the addition is completed, the reaction is continued to stir for 2.5 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to anhydrous ethanol, and then allowed to stand for precipitation, and then vacuum filtered, and the filter cake is placed in a vacuum drying oven, and dried at a temperature of 52° C. for 2.5 h to obtain modified chitosan;
[0049] Step S4: 10 mmol glycerol, 30 mmol (3-chloropropyl) triethoxysilane, 38 mmol anhydrous potassium carbonate, 0.4 g potassium iodide and 110 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen inlet tube, and nitrogen protection is introduced. The mixture is stirred at a temperature of -3°C and a stirring rate of 350 r / min for 40 min, and then the mixture is heated to 82°C and stirred for 22 h. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent, and then placed in a vacuum drying oven and dried at a temperature of 52°C for 2.5 h to obtain a multi-group siloxane;
[0050] Step S5: 10g of polylactic acid 4032d, 0.1g of doped zinc oxide, 0.6g of modified chitosan and 110mL of N,N-dimethylformamide were added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and stirred for reaction for 35min at a temperature of 28°C and a stirring rate of 350r / min, and then the temperature was raised to 82°C and the stirring reaction was continued for 2.5h, and then 11mL of a multi-group siloxane solution prepared by mixing deionized water and anhydrous ethanol in a mass ratio of 3g:90mL:12mL was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the dropwise addition was completed, the stirring reaction was continued for 2.5h. After the reaction was completed, the reaction product was cooled to room temperature, and then placed in a vacuum drying oven and dried at a temperature of 52°C for 4.5h to obtain an antibacterial substrate;
[0051] Step S6: Weigh 40 parts of antibacterial substrate, 10 parts of plasticizer, 8 parts of talcum powder, 4 parts of titanium dioxide, 3.5 parts of compatibilizer, 2 parts of antioxidant and 2 parts of ultraviolet absorber according to weight parts for later use; the plasticizer is butyl benzyl phthalate; the compatibilizer is ABS-g-MAH; the antioxidant is antioxidant 1076; the ultraviolet absorber is ultraviolet absorber UV-O;
[0052] Step S7: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0053] Step S8: melt-extrude the mixture through an extruder, and then granulate and pelletize to obtain a bio-based antibacterial packaging material.
[0054] Embodiment 3:
[0055] This embodiment is a method for preparing a bio-based antibacterial packaging material, comprising the following steps:
[0056] Step S1: 5.5 g of zinc acetate and 50 mL of deionized water are added to a three-necked flask equipped with a thermometer and a stirrer, and the mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, and then the pH is adjusted to 11 with a 25% mass fraction sodium hydroxide solution, and then the mixture is heated to 55° C. and stirred for reaction for 40 min, and then heated to 170° C. and stirred for reaction for 12 h. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed three times with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain nano zinc oxide;
[0057] Step S2: 5 g of nano zinc oxide and 120 mL of deionized water are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 15 min at a temperature of 30° C. and a stirring rate of 400 r / min, and then 15 mL of a 9% silver nitrate solution is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the addition is completed, the mixture is stirred for reaction for 1.5 h, and then the pH is adjusted to 9 with a 25% sodium hydroxide solution, and then the mixture is stirred for reaction for 5 h at a temperature of 85° C. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed three times with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain doped zinc oxide;
[0058] Step S3: 5g chitosan and 100mL of acetic acid solution with a mass fraction of 2% are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and stirred for 40min at a temperature of 30°C and a stirring rate of 400r / min, and then the pH is adjusted to 7 with a sodium hydroxide solution with a mass fraction of 25%, and then 50mL of isopropanol is added to continue stirring for 30min, and then 15mL of trimethylammonium chloride solution with a mass concentration of 0.9g / mL is added dropwise under the condition of heating to 85°C, and the dropping rate is controlled to 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 3h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to anhydrous ethanol, and then allowed to stand for precipitation, and then vacuum filtered, and the filter cake is placed in a vacuum drying oven, and dried at a temperature of 55°C for 3h to obtain modified chitosan;
[0059] Step S4: 10 mmol glycerol, 30 mmol (3-chloropropyl) triethoxysilane, 40 mmol anhydrous potassium carbonate, 0.6 g potassium iodide and 120 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen inlet tube, and nitrogen protection is introduced. The mixture is stirred for reaction at 0° C. and a stirring rate of 400 r / min for 50 min, and then the mixture is heated to 85° C. and stirred for reaction for 25 h. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent, and then placed in a vacuum drying oven and dried at 55° C. for 3 h to obtain a multi-group siloxane;
[0060] Step S5: 10g of polylactic acid 4032d, 0.15g of doped zinc oxide, 0.8g of modified chitosan and 120mL of N,N-dimethylformamide are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 40min at a temperature of 30°C and a stirring rate of 400r / min, and then the mixture is heated to 85°C and stirred for reaction for 3h, and then 12mL of a multi-group siloxane solution prepared by mixing multi-group siloxane, deionized water and anhydrous ethanol in a mass ratio of 5g:95mL:15mL is added dropwise while stirring, and the dropping rate is controlled to 2 drops / s. After the addition is completed, the mixture is stirred for reaction for 3h. After the reaction is completed, the reaction product is cooled to room temperature, and then placed in a vacuum drying oven and dried for 5h at a temperature of 55°C to obtain an antibacterial substrate;
[0061] Step S6: Weigh 45 parts of antibacterial substrate, 14 parts of plasticizer, 11 parts of talc, 6 parts of titanium dioxide, 5.5 parts of compatibilizer, 3 parts of antioxidant and 3 parts of ultraviolet absorber according to weight parts for later use; the plasticizer is diisononyl phthalate; the compatibilizer is PE-g-MAH; the antioxidant is antioxidant 1330; the ultraviolet absorber is ultraviolet absorber UV-9;
[0062] Step S7: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0063] Step S8: melt-extrude the mixture through an extruder, and then granulate and pelletize to obtain a bio-based antibacterial packaging material.
[0064] Comparative Example 1:
[0065] This comparative example is a method for preparing a bio-based antibacterial packaging material, comprising the following steps:
[0066] Step S1: weigh 35 parts of polylactic acid, 7 parts of plasticizer, 5 parts of talc, 2 parts of titanium dioxide, 1.5 parts of compatibilizer, 1 part of antioxidant and 1 part of ultraviolet absorber according to weight parts, and set aside; the plasticizer is dioctyl phthalate; the compatibilizer is PP-g-ST; the antioxidant is antioxidant 1024; the ultraviolet absorber is ultraviolet absorber UV-P;
[0067] Step S2: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0068] Step S3: melt-extrude the mixture through an extruder, and then granulate and pelletize to obtain a bio-based antibacterial packaging material.
[0069] Comparative Example 2:
[0070] This comparative example is a method for preparing a bio-based antibacterial packaging material, comprising the following steps:
[0071] Step S1: 5.5 g of zinc acetate and 50 mL of deionized water are added to a three-necked flask equipped with a thermometer and a stirrer, and the mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, and then the pH is adjusted to 11 with a 25% mass fraction sodium hydroxide solution, and then the mixture is heated to 55° C. and stirred for reaction for 40 min, and then heated to 170° C. and stirred for reaction for 12 h. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed three times with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain nano zinc oxide;
[0072] Step S2: 5 g of nano zinc oxide and 120 mL of deionized water are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 15 min at a temperature of 30° C. and a stirring rate of 400 r / min, and then 15 mL of a 9% silver nitrate solution is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the addition is completed, the mixture is stirred for reaction for 1.5 h, and then the pH is adjusted to 9 with a 25% sodium hydroxide solution, and then the mixture is stirred for reaction for 5 h at a temperature of 85° C. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed three times with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain doped zinc oxide;
[0073] Step S3: 5g chitosan and 100mL of acetic acid solution with a mass fraction of 2% are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and stirred for 40min at a temperature of 30°C and a stirring rate of 400r / min, and then the pH is adjusted to 7 with a sodium hydroxide solution with a mass fraction of 25%, and then 50mL of isopropanol is added to continue stirring for 30min, and then 15mL of trimethylammonium chloride solution with a mass concentration of 0.9g / mL is added dropwise under the condition of heating to 85°C, and the dropping rate is controlled to 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 3h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to anhydrous ethanol, and then allowed to stand for precipitation, and then vacuum filtered, and the filter cake is placed in a vacuum drying oven, and dried at a temperature of 55°C for 3h to obtain modified chitosan;
[0074] Step S4: 10 g of polylactic acid 4032d, 0.15 g of doped zinc oxide, 0.8 g of modified chitosan and 120 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and stirred for reaction at a temperature of 30°C and a stirring rate of 400 r / min for 40 min, then heated to 85°C and continued to stir for reaction for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then placed in a vacuum drying oven and dried at a temperature of 55°C for 5 h to obtain an antibacterial substrate;
[0075] Step S5: Weigh 45 parts of antibacterial substrate, 14 parts of plasticizer, 11 parts of talc, 6 parts of titanium dioxide, 5.5 parts of compatibilizer, 3 parts of antioxidant and 3 parts of ultraviolet absorber according to weight parts for later use; the plasticizer is diisononyl phthalate; the compatibilizer is PE-g-MAH; the antioxidant is antioxidant 1330; the ultraviolet absorber is ultraviolet absorber UV-9;
[0076] Step S6: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0077] Step S7: melt-extrude the mixture through an extruder, and then granulate and pelletize to obtain a bio-based antibacterial packaging material.
[0078] Comparative Example 3:
[0079] This comparative example is a method for preparing a bio-based antibacterial packaging material, comprising the following steps:
[0080] Step S1: 5.5 g of zinc acetate and 50 mL of deionized water are added to a three-necked flask equipped with a thermometer and a stirrer, and the mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 15 min, and then the pH is adjusted to 11 with a 25% mass fraction sodium hydroxide solution, and then the mixture is heated to 55° C. and stirred for reaction for 40 min, and then heated to 170° C. and stirred for reaction for 12 h. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed three times with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain nano zinc oxide;
[0081] Step S2: 5 g of nano zinc oxide and 120 mL of deionized water are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 15 min at a temperature of 30° C. and a stirring rate of 400 r / min, and then 15 mL of a 9% silver nitrate solution is added dropwise while stirring, and the dropping rate is controlled to be 2 drops / s. After the addition is completed, the mixture is stirred for reaction for 1.5 h, and then the pH is adjusted to 9 with a 25% sodium hydroxide solution, and then the mixture is stirred for reaction for 5 h at a temperature of 85° C. After the reaction is completed, the reaction product is cooled to room temperature, and then centrifuged. The precipitate is washed three times with distilled water and anhydrous ethanol in sequence, and then placed in a vacuum drying oven and dried at a temperature of 65° C. for 3 h to obtain doped zinc oxide;
[0082] Step S3: 10 mmol glycerol, 30 mmol (3-chloropropyl) triethoxysilane, 40 mmol anhydrous potassium carbonate, 0.6 g potassium iodide and 120 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen inlet tube, and nitrogen protection is introduced. The mixture is stirred for reaction at 0°C and a stirring rate of 400 r / min for 50 min, and then the mixture is heated to 85°C and stirred for reaction for 25 h. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent, and then placed in a vacuum drying oven and dried at 55°C for 3 h to obtain a multi-group siloxane;
[0083] Step S4: 10 g of polylactic acid 4032d, 0.15 g of doped zinc oxide and 120 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture was stirred for reaction at a temperature of 30°C and a stirring rate of 400 r / min for 40 min, and then the mixture was heated to 85°C and continued to stir for reaction for 3 h, and then 12 mL of a multi-group siloxane solution prepared by mixing multi-group siloxane, deionized water and anhydrous ethanol in a mass ratio of 5 g: 95 mL: 15 mL was added dropwise while stirring, and the dropping rate was controlled to 2 drops / s. After the addition was completed, the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then placed in a vacuum drying oven and dried at a temperature of 55°C for 5 h to obtain an antibacterial substrate;
[0084] Step S5: Weigh 45 parts of antibacterial substrate, 14 parts of plasticizer, 11 parts of talc, 6 parts of titanium dioxide, 5.5 parts of compatibilizer, 3 parts of antioxidant and 3 parts of ultraviolet absorber according to weight parts for later use; the plasticizer is diisononyl phthalate; the compatibilizer is PE-g-MAH; the antioxidant is antioxidant 1330; the ultraviolet absorber is ultraviolet absorber UV-9;
[0085] Step S6: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0086] Step S7: melt-extrude the mixture through an extruder, and then granulate and pelletize to obtain a bio-based antibacterial packaging material.
[0087] Comparative Example 4:
[0088] This comparative example is a method for preparing a bio-based antibacterial packaging material, comprising the following steps:
[0089] Step S1: 5g chitosan and 100mL of acetic acid solution with a mass fraction of 2% are added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and stirred for 40min at a temperature of 30°C and a stirring rate of 400r / min, and then the pH is adjusted to 7 with a sodium hydroxide solution with a mass fraction of 25%, and then 50mL of isopropanol is added to continue stirring for 30min, and then 15mL of trimethylammonium chloride solution with a mass concentration of 0.9g / mL is added dropwise under the condition of heating to 85°C, and the dropping rate is controlled to 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 3h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to anhydrous ethanol, and then allowed to stand for precipitation, and then vacuum filtered, and the filter cake is placed in a vacuum drying oven, and dried at a temperature of 55°C for 3h to obtain modified chitosan;
[0090] Step S2: 10 mmol glycerol, 30 mmol (3-chloropropyl) triethoxysilane, 40 mmol anhydrous potassium carbonate, 0.6 g potassium iodide and 120 mL anhydrous toluene are added to a three-necked flask equipped with a stirrer, a thermometer and a nitrogen inlet tube, and nitrogen protection is introduced. The mixture is stirred at 0° C. and a stirring rate of 400 r / min for 50 min, and then the mixture is heated to 85° C. and the stirring reaction is continued for 25 h. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. The filtrate is rotary evaporated to remove the solvent, and then placed in a vacuum drying oven and dried at 55° C. for 3 h to obtain a multi-group siloxane;
[0091] Step S3: 10g of polylactic acid 4032d, 0.8g of modified chitosan and 120mL of N,N-dimethylformamide were added to a three-necked flask equipped with a thermometer, a stirrer and a constant pressure dropping funnel, and the mixture was stirred for reaction for 40min at a temperature of 30°C and a stirring rate of 400r / min, and then the mixture was heated to 85°C and stirred for reaction for 3h, and then 12mL of a multi-group siloxane solution prepared by mixing multi-group siloxane, deionized water and anhydrous ethanol in a mass ratio of 5g:95mL:15mL was added dropwise while stirring, and the dropping rate was controlled to 2 drops / s. After the addition was completed, the mixture was stirred for reaction for 3h. After the reaction was completed, the reaction product was cooled to room temperature, and then placed in a vacuum drying oven and dried for 5h at a temperature of 55°C to obtain an antibacterial substrate;
[0092] Step S4: Weigh 45 parts of antibacterial substrate, 14 parts of plasticizer, 11 parts of talc, 6 parts of titanium dioxide, 5.5 parts of compatibilizer, 3 parts of antioxidant and 3 parts of ultraviolet absorber according to weight parts for later use; the plasticizer is diisononyl phthalate; the compatibilizer is PE-g-MAH; the antioxidant is antioxidant 1330; the ultraviolet absorber is ultraviolet absorber UV-9;
[0093] Step S5: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture;
[0094] Step S6: melt-extrude the mixture through an extruder, and then granulate and pelletize to obtain a bio-based antibacterial packaging material.
[0095] The performance of the bio-based antibacterial packaging materials of Examples 1-3 and Comparative Examples 1-4 was tested, and the test results are as follows:
[0096]
[0097] Referring to the data in the above table, according to the comparison between Examples 1-3 and Comparative Examples 1-4, it can be seen that the addition of doped zinc oxide and modified chitosan can greatly improve the antibacterial properties of the bio-based antibacterial packaging material, and the addition of multi-group siloxane can further improve its antibacterial properties, so that the prepared bio-based antibacterial packaging material has excellent antibacterial properties.
[0098] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0099] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A bio-based antibacterial packaging material, characterized in that: It includes the following components by weight: 35-45 parts of antibacterial base material, 7-14 parts of plasticizer, 5-11 parts of talc, 2-6 parts of titanium dioxide, 1.5-5.5 parts of compatibilizer, 1-3 parts of antioxidant and 1-3 parts of ultraviolet absorber; Wherein, the antibacterial substrate is prepared by the following steps: Step s1: stirring zinc acetate and deionized water for reaction, and then adjusting the pH with sodium hydroxide solution. After the reaction is completed, the reaction product is cooled, centrifuged, and the precipitate is washed and dried to obtain nano zinc oxide; Step s2: stirring the nano zinc oxide and deionized water for reaction, then adding the silver nitrate solution dropwise while stirring, continuing the stirring reaction after the addition is complete, then adjusting the pH with a sodium hydroxide solution, cooling the reaction product after the reaction is complete, then centrifuging, washing and drying the precipitate to obtain doped zinc oxide; Step s3: stirring the chitosan and acetic acid solution to react, then adjusting the pH with a sodium hydroxide solution, then adding isopropanol and continuing to stir the reaction, then adding the glycidyl trimethylammonium chloride solution dropwise while stirring, and continuing to stir the reaction after the dropwise addition is completed. After the reaction is completed, the reaction product is cooled, then added to anhydrous ethanol, then allowed to stand and precipitate, then vacuum filtered, and the filter cake is dried to obtain modified chitosan; Step s4: stirring glycerol, (3-chloropropyl)triethoxysilane, anhydrous potassium carbonate, potassium iodide and anhydrous toluene for reaction, cooling the reaction product after the reaction is completed, then vacuum filtering, rotary evaporating the filtrate, and then drying to obtain multi-group siloxane; Step s5: Stirring polylactic acid, doped zinc oxide, modified chitosan and N,N-dimethylformamide for reaction, then adding the multi-group siloxane solution dropwise while stirring, and continuing to stir the reaction after the addition is completed. After the reaction is completed, the reaction product is cooled and then dried to obtain an antibacterial substrate.
2. The bio-based antibacterial packaging material according to claim 1, characterized in that: The dosage ratio of the zinc acetate and deionized water in step s1 is 4.5-5.5 g:50 mL; the mass fraction of the sodium hydroxide solution in step s1 is 20-25%.
3. The bio-based antibacterial packaging material according to claim 1, characterized in that: The dosage ratio of the nano zinc oxide, deionized water and silver nitrate solution in step s2 is 5g:100-120mL:10-15mL; the mass fraction of the silver nitrate solution in step s2 is 5-9%, and the mass fraction of the sodium hydroxide solution is 20-25%.
4. The bio-based antibacterial packaging material according to claim 1, characterized in that: The amount ratio of the chitosan, acetic acid solution, isopropanol and glycidyl trimethylammonium chloride solution in step s3 is 5g:80-100mL:30-50mL:10-15mL; the mass fraction of the sodium hydroxide solution in step s3 is 20-25%, the mass fraction of the acetic acid solution is 1-2%, and the mass concentration of the glycidyl trimethylammonium chloride solution is 0.5-0.9g / mL.
5. The bio-based antibacterial packaging material according to claim 1, characterized in that: The usage ratio of the glycerol, (3-chloropropyl)triethoxysilane, anhydrous potassium carbonate, potassium iodide and anhydrous toluene in step s4 is 10mmol:30mmol:35-40mmol:0.2-0.6g:100-120mL.
6. The bio-based antibacterial packaging material according to claim 1, characterized in that: The amount ratio of the polylactic acid, doped zinc oxide, modified chitosan, N,N-dimethylformamide and multi-group siloxane solution in step s5 is 10g: 0.05-0.15g: 0.4-0.8g: 100-120mL: 10-12mL; the polylactic acid in step s5 is 4032d polylactic acid, and the multi-group siloxane solution is a mixture of multi-group siloxane, deionized water and anhydrous ethanol in a mass ratio of 1-5g: 85-95mL: 10-15mL.
7. A method for preparing a bio-based antibacterial packaging material, characterized in that: The following steps are involved: Step 1: Weigh 35-45 parts of antibacterial substrate, 7-14 parts of plasticizer, 5-11 parts of talcum powder, 2-6 parts of titanium dioxide, 1.5-5.5 parts of compatibilizer, 1-3 parts of antioxidant and 1-3 parts of ultraviolet absorber according to weight parts, and set aside; Step 2: adding the antibacterial substrate, plasticizer, talcum powder, titanium dioxide, compatibilizer, antioxidant and ultraviolet absorber into a mixer, stirring and mixing to obtain a mixture; Step 3: The mixed material is melt-extruded through an extruder, and then granulated and pelletized to obtain a bio-based antibacterial packaging material.
8. The method for preparing a bio-based antibacterial packaging material according to claim 7, characterized in that: The plasticizer is one of dioctyl phthalate, butyl benzyl phthalate and diisononyl phthalate; the compatibilizer is one of PP-g-ST, ABS-g-MAH and PE-g-MAH.
9. The method for preparing a bio-based antibacterial packaging material according to claim 7, characterized in that: The antioxidant is one of antioxidant 1024, antioxidant 1076 and antioxidant 1330; the ultraviolet absorber is one of ultraviolet absorber UV-P, ultraviolet absorber UV-O and ultraviolet absorber UV-9.
Citation Information
Patent Citations
Weather-resistant degradable plastic bottle and preparation method
CN108948703A
Antibacterial TiO2-carbon nanotube modified polylactic acid material and preparation method thereof
CN111499841A
Medical polymer bandage convenient to biodegrade and preparation method thereof
CN117618624A
Antibacterial modified plastic
WO2022022544A1
Cited By
Manufacturing process of degradable material for syringe production
CN119639242A
Plastic material for antibacterial and anti-adhesion medical pipe fitting and preparation method of plastic material
CN121203304A
Biodegradable polylactic acid composite material and preparation method thereof
CN121379082A
A biodegradable polylactic acid composite material and its preparation method