Modified antibacterial foamed silica gel and preparation method thereof

By surface modification of nanotitanium dioxide, grafting diphenyl etherified haloamine triazine group, and evenly dispersing it in silica gel, the problem of foamed silica gel lacks antibacterial properties is solved, and the stable dispersion of nanotitanium dioxide in silica gel is achieved and Effective antibacterial effect improves the comprehensive performance of foamed silicone.

CN118931191APending Publication Date: 2024-11-12SHENZHEN HUAYI FEIHU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411227314.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional foamed silicone lacks antibacterial properties, and nanotitanium dioxide is prone to agglomeration in polymer matrix, making it difficult to form a stable dispersion system, making it difficult to improve the mechanical and antibacterial properties of the polymer.

Method used

By modifying nanotitanium dioxide, diphenyl etherified haloamine triazine group is grafted on the surface to reduce its hydrophilicity and disperse evenly in the silica gel matrix, combining photocatalytic and bioinactivation mechanisms to improve antibacterial performance.

Benefits of technology

The uniform dispersion and effective antibacterial effect of nanotitanium dioxide in silica gel are achieved, which significantly improves the antibacterial properties of foamed silica gel and enhances its application potential in the field of electronic information technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931191A_ABST
    Figure CN118931191A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of foamed silica gel, and discloses a TiO2 modified foamed silica gel containing diphenyl etherified halamine triazinyl, epoxy titanium dioxide reacts with 2-chloro-4, 6-diamino-1, 3, 5-triazine under the action of triethylamine to generate 2-chloro-4-amino-1, 3, 5-triazinyl titanium dioxide, and the 2-chloro-4-amino-1, 3, 5-triazinyl titanium dioxide reacts with 2, 4, 5-triazinyl to generate 2-chloro-4-amino-1, 3, 5-triazinyl titanium dioxide. According to the present invention, diphenyl etherified halamine triazinyl titanium dioxide is obtained by reacting 4, 4 '-trichloro-2'-hydroxydiphenyl ether and chloridizing, the diphenyl etherified halamine triazinyl titanium dioxide and the foaming silica gel have good interface affinity, and when the diphenyl etherified halamine triazinyl titanium dioxide is irradiated by ultraviolet rays, the titanium dioxide generates photo-induced electrons and holes, and reacts with water to generate superoxide and hydroxyl free radicals, such that the superoxide and hydroxyl free radicals are formed; microbial bacteria are oxidized, halogen positive ions and halogenated diphenyl ether groups can inhibit physiological functions of bacterial cell walls and destroy metabolism of bacteria, and the antibacterial performance of the foamed silica gel is improved by combining photocatalytic antibacterial performance of titanium dioxide and biological inactivation antibacterial performance of diphenyl etherified halamine triazinyl.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foamed silica gel, in particular to a modified antibacterial foamed silica gel and a preparation method thereof. Background Art

[0002] Silicone is a synthetic rubber composed of silicon atoms and oxygen atoms. Ordinary silicone is mainly composed of silicon-oxygen chain segments containing a small amount of methyl and vinyl groups. It has good low-temperature resistance, high-temperature resistance, air permeability and physiological inertness. It is widely used in electrical insulation materials, protective layers, and biomedicine. Foamed silicone used in the field of electronic information technology does not have antibacterial properties, so traditional foamed silicone needs to be modified. Filling modification is an efficient and economical modification method, which is often used in the modification of polymer materials. Inorganic nanomaterials such as graphene and titanium dioxide with excellent performance are filled into polymer rubbers such as nitrile rubber and room temperature vulcanized rubber. By integrating the excellent mechanical, thermodynamic, antibacterial and other properties of inorganic nanomaterials into polymer rubber materials, the comprehensive properties of polymer rubber materials such as mechanics and antibacterial can be improved.

[0003] Nano-titanium dioxide is a white powdery benign oxide with properties such as non-toxicity, opacity, and high whiteness. It is considered to be the best white pigment in the world today. It is widely used in coatings, plastics, papermaking, chemical fibers, rubber, photocatalytic antibacterial and other fields. Because of this, nano-titanium dioxide is also often used in functional reinforcing fillers. However, the traditional nano-titanium dioxide has a small specific surface area and low absorption efficiency of ultraviolet light, making it difficult to achieve the ideal photocatalytic antibacterial effect. In addition, as a functional reinforcing filler, the biggest problem of nano-titanium dioxide is that it is easy to agglomerate in the polymer matrix and cannot form a stable dispersion system. Therefore, it is difficult to achieve the effect of improving the comprehensive properties of polymer mechanics, antibacterial and other comprehensive properties in practical applications. Based on this, we need to modify the traditional nano-titanium dioxide. Since the surface of nano-titanium dioxide contains a large number of hydroxyl groups and exhibits hydrophilicity, it can be chemically reacted with the hydroxyl groups on its surface and grafted with some antibacterial functional groups to reduce its surface hydrophilicity. At the same time, it can also combine the advantages of antibacterial functional groups to further enhance the practical value of nano-titanium dioxide.

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a modified antibacterial foamed silica gel and a preparation method thereof, which solves the problem that the foamed silica gel does not have antibacterial properties.

[0006] (II) Technical solution

[0007] To achieve the above object, the present invention provides the following technical scheme: a modified antibacterial foamed silica gel, wherein the modified foamed silica gel is a TiO2 modified foamed silica gel containing diphenyl ether halogenamine triazine groups, wherein the TiO2 with diphenyl ether halogenamine triazine groups grafted on the surface is uniformly dispersed in a silica gel matrix, and the preparation method of the TiO2 modified foamed silica gel containing diphenyl ether halogenamine triazine groups comprises the following steps:

[0008] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0009] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide into a three-necked flask, disperse uniformly by ultrasonication, fill with nitrogen to remove oxygen, transfer to an oil bath, continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring conditions to carry out a ring-opening reaction, and after cooling the product, distill under reduced pressure to remove the solvent, wash and dry to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0010] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix well, transfer the system to an ice water bath, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, adjust the solution pH to 7-8 with sodium carbonate, carry out substitution reaction in a nitrogen atmosphere, centrifuge, wash and dry the product to obtain diphenyl ether triazine titanium dioxide;

[0011] (4) adding a sodium hypochlorite solution with a concentration of 0.5-1% and diphenyl ether triazine-based titanium dioxide to a three-necked flask, and after uniform ultrasonic dispersion, adjusting the solution pH to 6-8 with dilute sulfuric acid, and chlorinating. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine-based titanium dioxide;

[0012] (5) Add vulcanized silica gel, catalyst dibutyltin dioctoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, then continue to add diphenyl ether halogenamine triazine titanium dioxide, use a plastic mixing knife to evenly stir for 10-20 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.1-0.3 MPa for 10-30 minutes, and then cure at 15-35°C for 70-80 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine groups. The TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine groups is used in the field of antibacterial foaming silica gel.

[0013] Preferably, in step (2), the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:60-100:10-20.

[0014] Preferably, the temperature of the ring-opening reaction in step (2) is raised to 90-110° C., and the reaction is stirred in a nitrogen atmosphere for 10-20 hours.

[0015] Preferably, in step (3), the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 100-120:100.

[0016] Preferably, during the substitution reaction in step (3), the reaction is first carried out at 0-5° C. in a nitrogen atmosphere for 1-3 h, and then the temperature is raised to 40-60° C. and the reaction is continued for 2-6 h.

[0017] Preferably, the temperature during chlorination in step (4) is 15-35° C. and the time is 40-80 min.

[0018] Preferably, in step (5), the mass ratio of the foamed silica gel, the catalyst dibutyltin dioctoate, the reinforcing agent white carbon black, the additive calcium carbonate and the diphenylether halogenamine triazine-based titanium dioxide is 100:20-40:10-20:4-8:2-6.

[0019] (III) Beneficial technical effects

[0020] Compared with the prior art, the present invention has the following beneficial technical effects:

[0021] The TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine group has a large number of epoxy groups on the surface of nano titanium dioxide modified by 3-(2,3-epoxypropoxy)propyltrimethoxysilane. Under the action of catalyst triethylamine, it can undergo a ring-opening reaction with part of the amino groups in 2-chloro-4,6-diamino-1,3,5-triazine to generate 2-chloro-4-amino-1,3,5-triazine titanium dioxide. In an alkaline environment, 2-chloro-4-amino-1,3,5- Triazine titanium dioxide can undergo a substitution reaction with the hydroxyl group in 2,4,4'-trichloro-2'-hydroxydiphenyl ether, and then be chlorinated with a sodium hypochlorite solution to obtain diphenyl ether halamine triazine titanium dioxide. Special organic functional groups such as epoxy, triazine, and halamine are connected to the surface of nano-titanium dioxide through chemical bond connection, which consumes a large number of hydroxyl groups on the surface of nano-titanium dioxide, reduces the hydrophilicity of nano-titanium dioxide, and is beneficial to the dispersibility of nano-titanium dioxide in oily matrices.

[0022] The TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine groups is prepared by adding diphenyl ether halogenamine triazine titanium dioxide into a vulcanized silica gel matrix to finally obtain the TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine groups. The titanium dioxide grafted with diphenyl ether halogenamine triazine groups on the surface has good interface affinity with the foaming silica gel and can be evenly dispersed in the foaming silica gel matrix, thus avoiding the agglomeration of nano-titanium dioxide to a certain extent. When the composite foaming silica gel is irradiated with ultraviolet rays, the nano-titanium dioxide generates photogenerated electrons and holes, which can react with water to generate highly oxidizing superoxide free radicals and hydroxyl free radicals, thereby oxidizing Staphylococcus aureus, Escherichia coli and other microorganisms and bacteria. The organic matter is oxidized into titanium dioxide and water, thereby achieving the effect of photocatalytic antibacterial. In addition, the halamine in the diphenyl ether halamine triazine group on the surface of nano-titanium dioxide can generate halogen cations and directly act on bacterial receptors, thereby inhibiting or even destroying the metabolism of bacterial cells, and ultimately leading to the death of bacteria. The halogenated diphenyl ether group in the diphenyl ether halamine triazine group can inhibit the physiological function of the bacterial cell wall, reduce the cell's absorption of required amino acids, and then inactivate the bacterial cells. By combining the photocatalytic antibacterial of nano-titanium dioxide and the biological inactivation antibacterial of the diphenyl ether halamine triazine group, the antibacterial properties of the composite foaming silica gel are greatly improved, and the application field of the foaming silica gel is further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the synthesis principle diagram of 2-chloro-4-amino-1,3,5-triazine titanium dioxide.

[0024] Figure 2 This is the synthesis principle diagram of diphenyl ether triazine titanium dioxide.

[0025] Figure 3 This is the synthesis principle diagram of diphenyl etherified halogenamine triazine titanium dioxide. DETAILED DESCRIPTION

[0026] To achieve the above object, the present invention provides the following specific implementation methods and examples: A TiO2-modified foamed silica gel containing diphenyl etherified halogenamine triazine groups, the preparation method of which comprises the following steps:

[0027] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0028] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide to a three-necked flask, and after ultrasonic dispersion, fill with nitrogen to remove oxygen, transfer to an oil bath, and continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring conditions, wherein the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:60-100:10-20, and stir in a nitrogen atmosphere at 90-110° C. for 10-20 hours to carry out a ring-opening reaction. After the product is cooled, the solvent is removed by distillation under reduced pressure, washed and dried to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0029] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix evenly, transfer the system to an ice water bath environment, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, wherein the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 100-120:100, adjust the solution pH to 7-8 with sodium carbonate, react at 0-5°C for 1-3h in a nitrogen atmosphere, and then heat to 40-60°C after the reaction, continue to react for 2-6h, centrifuge, wash and dry the product to obtain diphenyl ether triazine titanium dioxide;

[0030] (4) adding a sodium hypochlorite solution with a concentration of 0.5-1% and diphenyl ether triazine-based titanium dioxide to a three-necked flask, uniformly dispersing by ultrasonication, adjusting the solution pH to 6-8 with dilute sulfuric acid, and chlorinating at 15-35° C. for 40-80 min. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine-based titanium dioxide;

[0031] (5) Add vulcanized silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, and then continue to add diphenyl ether halamine triazine titanium dioxide, wherein the mass ratio of foaming silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black, additive calcium carbonate and diphenyl ether halamine triazine titanium dioxide is 100:20-40:10-20:4-8:2-6, use a plastic mixing knife to mix evenly for 10-20 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.1-0.3 MPa for 10-30 minutes, and then cure at 15-35°C for 70-80 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halamine triazine.

[0032] Example 1

[0033] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0034] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide to a three-necked flask, and after ultrasonic dispersion, fill with nitrogen to remove oxygen, transfer to an oil bath, and continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring conditions, wherein the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:60:10, and stir at 90° C. in a nitrogen atmosphere for a ring-opening reaction for 10 hours. After the product is cooled, the solvent is distilled off under reduced pressure, washed and dried to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0035] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix evenly, transfer the system to an ice water bath environment, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, wherein the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 100:100, adjust the solution pH to 7 with sodium carbonate, react at 0°C in a nitrogen atmosphere for 1h, then heat to 40°C, continue to react for 2h, centrifuge, wash and dry the product to obtain diphenyl ether triazine titanium dioxide;

[0036] (4) adding a 0.5% sodium hypochlorite solution and diphenyl ether triazine titanium dioxide to a three-necked flask, and uniformly dispersing by ultrasonication, adjusting the solution pH to 6 with dilute sulfuric acid, and chlorinating at 15° C. for 40 min. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine titanium dioxide;

[0037] (5) Add vulcanized silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, and then continue to add diphenyl ether halamine triazine titanium dioxide, wherein the mass ratio of foaming silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black, additive calcium carbonate and diphenyl ether halamine triazine titanium dioxide is 100:20:10:4:2, use a plastic mixing knife to mix evenly for 10 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.1 MPa for 10 minutes, and then cure at 15°C for 70 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halamine triazine.

[0038] Example 2

[0039] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0040] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide to a three-necked flask, and after ultrasonic dispersion, fill with nitrogen to remove oxygen, transfer to an oil bath, and continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring conditions, wherein the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:70:12.5, and stir at 95° C. in a nitrogen atmosphere for a ring-opening reaction for 12 hours. After the product is cooled, the solvent is distilled off under reduced pressure, washed and dried to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0041] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix evenly, transfer the system to an ice water bath environment, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, wherein the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 105:100, adjust the solution pH to 7 with sodium carbonate, react at 2°C in a nitrogen atmosphere for 1.5h, then heat to 45°C after completion, continue to react for 3h, centrifuge, wash and dry the product to obtain diphenyl ether triazine titanium dioxide;

[0042] (4) adding a 0.6% sodium hypochlorite solution and diphenyl ether triazine titanium dioxide to a three-necked flask, and uniformly dispersing them by ultrasonication. Then adjusting the pH of the solution to 7 with dilute sulfuric acid, and chlorinating at 20° C. for 50 min. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine titanium dioxide;

[0043] (5) Add vulcanized silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, then continue to add diphenyl ether halamine triazine titanium dioxide, wherein the mass ratio of foaming silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black, additive calcium carbonate and diphenyl ether halamine triazine titanium dioxide is 100:25:12.5:5:3, use a plastic mixing knife to mix evenly for 12 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.2 MPa for 15 minutes, and then cure at 20°C for 72 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halamine triazine.

[0044] Example 3

[0045] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0046] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide to a three-necked flask, and after ultrasonic dispersion, fill with nitrogen to remove oxygen, transfer to an oil bath, and continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring conditions, wherein the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:80:15, and stir at 100° C. in a nitrogen atmosphere for a ring-opening reaction for 15 hours. After the product is cooled, the solvent is distilled off under reduced pressure, washed and dried to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0047] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix evenly, transfer the system to an ice water bath environment, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, wherein the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 110:100, adjust the solution pH to 7 with sodium carbonate, react at 3°C ​​for 2h in a nitrogen atmosphere, and then heat to 50°C after the reaction, continue to react for 4h, centrifuge, wash and dry the product to obtain diphenyl ether triazine titanium dioxide;

[0048] (4) adding a 0.7% sodium hypochlorite solution and diphenyl ether triazine titanium dioxide to a three-necked flask, and uniformly dispersing them by ultrasonication, adjusting the pH of the solution to 7 with dilute sulfuric acid, and chlorinating at 25° C. for 60 min. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine titanium dioxide;

[0049] (5) Add vulcanized silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, then continue to add diphenyl ether halogenamine triazine titanium dioxide, wherein the mass ratio of foaming silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black, additive calcium carbonate and diphenyl ether halogenamine triazine titanium dioxide is 100:30:15:6:4, use a plastic mixing knife to mix evenly for 15 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.2 MPa for 20 minutes, and then cure at 25°C for 75 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine.

[0050] Example 4

[0051] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0052] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide to a three-necked flask, and after ultrasonic dispersion, fill with nitrogen to remove oxygen, transfer to an oil bath, and continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring conditions, wherein the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:90:17.5, and stir at 105° C. in a nitrogen atmosphere for 18 hours to carry out a ring-opening reaction. After the product is cooled, the solvent is distilled off under reduced pressure, washed and dried to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0053] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix evenly, transfer the system to an ice water bath environment, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, wherein the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 115:100, adjust the solution pH to 8 with sodium carbonate, react at 4°C for 2h in a nitrogen atmosphere, heat to 55°C after completion, continue to react for 5h, centrifuge, wash and dry the product to obtain diphenyl ether triazine titanium dioxide;

[0054] (4) adding a 0.8% sodium hypochlorite solution and diphenyl ether triazine titanium dioxide to a three-necked flask, and uniformly dispersing them by ultrasonication, adjusting the pH of the solution to 7 with dilute sulfuric acid, and chlorinating at 30° C. for 70 min. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine titanium dioxide;

[0055] (5) Add vulcanized silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, then continue to add diphenyl ether halamine triazine titanium dioxide, wherein the mass ratio of foaming silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black, additive calcium carbonate and diphenyl ether halamine triazine titanium dioxide is 100:35:17.5:7:5, use a plastic mixing knife to mix evenly for 18 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.2 MPa for 25 minutes, and then cure at 30°C for 78 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halamine triazine.

[0056] Example 5

[0057] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0058] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide to a three-necked flask, and after ultrasonic dispersion, fill with nitrogen to remove oxygen, transfer to an oil bath, and continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring, wherein the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:100:20, and stir at 110° C. in a nitrogen atmosphere for a ring-opening reaction for 20 hours. After the product is cooled, the solvent is distilled off under reduced pressure, washed and dried to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0059] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix evenly, transfer the system to an ice water bath environment, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, wherein the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 120:100, adjust the solution pH to 8 with sodium carbonate, react at 5°C for 3h in a nitrogen atmosphere, and then heat to 60°C after the reaction, continue to react for 6h, centrifuge, wash and dry the product to obtain diphenyl ether triazine titanium dioxide;

[0060] (4) adding a 1% sodium hypochlorite solution and diphenyl ether triazine titanium dioxide to a three-necked flask, and after ultrasonic dispersion, adjusting the solution pH to 8 with dilute sulfuric acid, and chlorinating at 35° C. for 80 min. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine titanium dioxide;

[0061] (5) Add vulcanized silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, then continue to add diphenyl ether halamine triazine titanium dioxide, wherein the mass ratio of foaming silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black, additive calcium carbonate and diphenyl ether halamine triazine titanium dioxide is 100:40:20:8:6, use a plastic mixing knife to mix evenly for 20 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.3 MPa for 30 minutes, and then cure at 35°C for 80 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halamine triazine.

[0062] Comparative Example 1

[0063] (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide;

[0064] (2) Add N,N-dimethylformamide solvent and epoxidized nano-titanium dioxide to a three-necked flask, and after ultrasonic dispersion, fill with nitrogen to remove oxygen, transfer to an oil bath, and continue to add 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine under stirring conditions, wherein the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:50:7.5, and stir at 90° C. in a nitrogen atmosphere for a ring-opening reaction for 5 hours. After the product is cooled, the solvent is distilled off under reduced pressure, washed and dried to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide;

[0065] (3) Add 1,4-dioxane solvent and 2,4,4'-trichloro-2'-hydroxydiphenyl ether to a three-necked flask, stir and mix evenly, transfer the system to an ice water bath environment, continue to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, wherein the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 95:100, adjust the solution pH to 7 with sodium carbonate, react at 0°C for 0.5h in a nitrogen atmosphere, and then heat to 40°C after the reaction, continue to react for 1h, centrifuge the product, wash and dry to obtain diphenyl ether triazine titanium dioxide;

[0066] (4) adding a 0.4% sodium hypochlorite solution and diphenyl ether triazine-based titanium dioxide to a three-necked flask, and uniformly dispersing by ultrasonication, adjusting the solution pH to 6 with dilute sulfuric acid, and chlorinating at 15° C. for 20 min. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl ether halamine triazine-based titanium dioxide;

[0067] (5) Add vulcanized silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, then continue to add diphenyl ether halogenamine triazine titanium dioxide, wherein the mass ratio of foaming silica gel, catalyst dibutyl tin dioctanoate, reinforcing agent white carbon black, additive calcium carbonate and diphenyl ether halogenamine triazine titanium dioxide is 100:15:7.5:3:1, use a plastic mixing knife to mix evenly for 5 minutes, transfer to a plexiglass mold, put into a vacuum pump, maintain at a pressure of 0.1 MPa for 5 minutes, and then cure at 15°C for 60 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine.

[0068] The TiO2-modified foamed silica gel containing diphenylether halogenamine triazine groups was cut into circular samples with a diameter of 10 mm and a thickness of 5 mm. After being washed, they were immersed in a Staphylococcus aureus suspension obtained in 10 mL of tryptic soy broth medium, and cultured in an incubator at 37°C in a dark environment for 30 hours. The bacterial suspension without the TiO2-modified foamed silica gel containing diphenylether halogenamine triazine groups was used as a blank control test. The colony count in the bacterial suspension was observed, and the sterilization rate was calculated.

[0069]

[0070] The TiO2-modified foamed silica gel containing diphenylether halogenamine triazine groups was cut into circular samples with a diameter of 10 mm and a thickness of 5 mm. After being washed, they were immersed in a Staphylococcus aureus suspension obtained in 10 mL of tryptic soy broth medium. The suspension was irradiated with ultraviolet light and cultured in an incubator at 37°C for 30 hours. The bacterial suspension without the TiO2-modified foamed silica gel containing diphenylether halogenamine triazine groups was used as a blank control test. The number of colonies in the bacterial suspension was observed and the sterilization rate was calculated.

[0071]

Claims

1. A modified antibacterial foamed silica gel, characterized in that: The modified antibacterial foamed silica gel is a modified foamed silica gel containing TiO2 with diphenyl ether halogenamine triazine groups, and the TiO2 with diphenyl ether halogenamine triazine groups grafted on the surface is uniformly dispersed in the silica gel matrix.

2. A method for preparing the modified antibacterial foamed silica gel according to claim 1, characterized in that the method for preparing the modified foamed silica gel containing diphenyl etherified halogenamine triazine group TiO2 comprises the following steps: (1) reacting nano titanium dioxide with 3-(2,3-epoxypropoxy)propyltrimethoxysilane to obtain epoxidized nano titanium dioxide; (2) adding epoxidized nano-titanium dioxide to N,N-dimethylformamide solvent, uniformly dispersing by ultrasonication, filling with nitrogen to remove oxygen, transferring to an oil bath, adding 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine to carry out a ring-opening reaction, and distilling the product under reduced pressure after cooling, washing and drying to obtain 2-chloro-4-amino-1,3,5-triazine titanium dioxide; (3) adding 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 1,4-dioxane solvent, stirring and mixing, transferring the system to an ice water bath, continuing to add 2-chloro-4-amino-1,3,5-triazine titanium dioxide, adjusting the solution pH to 7-8 with sodium carbonate, carrying out substitution reaction in a nitrogen atmosphere, centrifuging, washing and drying the product to obtain diphenyl ether triazine titanium dioxide; (4) adding diphenyl etherified triazine-based titanium dioxide to a sodium hypochlorite solution having a concentration of 0.5-1%, and uniformly dispersing the solution by ultrasonication, adjusting the pH of the solution to 6-8 with dilute sulfuric acid, and chlorinating the solution. After the chlorination is completed, the product is filtered, washed with deionized water, and dried to obtain diphenyl etherified halamine triazine-based titanium dioxide; (5) Add vulcanized silica gel, catalyst dibutyltin dioctoate, reinforcing agent white carbon black and additive calcium carbonate into the reactor, stir and mix evenly, then continue to add diphenyl ether halogenamine triazine titanium dioxide, use a plastic mixing knife to evenly stir for 10-20 minutes, transfer to a plexiglass mold, put in a vacuum pump, maintain at a pressure of 0.1-0.3 MPa for 10-30 minutes, and then cure at 15-35°C for 70-80 hours to obtain TiO2 modified foaming silica gel containing diphenyl ether halogenamine triazine.

3. The method for preparing the modified antibacterial foamed silica gel according to claim 2, characterized in that: In the step (2), the mass ratio of epoxidized nano-titanium dioxide, 2-chloro-4,6-diamino-1,3,5-triazine and triethylamine is 100:60-100:10-20.

4. The method for preparing the modified antibacterial foamed silica gel according to claim 2, characterized in that: The temperature of the ring-opening reaction in step (2) is raised to 90-110° C., and the reaction is stirred in a nitrogen atmosphere for 10-20 hours.

5. The method for preparing the modified antibacterial foamed silica gel according to claim 2, characterized in that: In the step (3), the mass ratio of 2,4,4'-trichloro-2'-hydroxydiphenyl ether to 2-chloro-4-amino-1,3,5-triazine titanium dioxide is 100-120:

100.

6. The method for preparing the modified antibacterial foamed silica gel according to claim 2, characterized in that: During the substitution reaction in step (3), the reaction is first carried out at 0-5° C. in a nitrogen atmosphere for 1-3 h, and then the temperature is raised to 40-60° C. and the reaction is continued for 2-6 h.

7. The method for preparing the modified antibacterial foamed silica gel according to claim 2, characterized in that: The temperature during chlorination in step (4) is 15-35° C. and the time is 40-80 min.

8. The method for preparing the modified antibacterial foamed silica gel according to claim 2, characterized in that: In the step (5), the mass ratio of the foamed silica gel, the catalyst dibutyltin dioctoate, the reinforcing agent white carbon black, the additive calcium carbonate and the diphenylether halogenamine triazine-based titanium dioxide is 100:20-40:10-20:4-8:2-6.

9. The method for preparing the modified antibacterial foamed silica gel according to claim 2, characterized in that: The TiO2-modified foamed silica gel containing diphenyl etherified halogenamine triazine groups in step (5) is used in the field of antibacterial foamed silica gel.