Water-dissolution-resistant water-based flexographic printing ink for film printing and preparation method of water-dissolution-resistant water-based flexographic printing ink

By using water-based flexographic inks with combination materials such as self-crosslinked acrylic and polyurethane emulsions in film printing, the problems of slow drying speed and insufficient adhesion in film printing are solved, and rapid drying and strong adhesion are achieved. It reduces the risk of environmental pollution and is suitable for environmentally friendly film printing.

CN118931258APending Publication Date: 2024-11-12覃宏敏
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411226170.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In film printing, water-based inks have slow drying speed, poor overprinting effect, low printing efficiency and poor adhesion, resulting in limited application and promotion. At the same time, the use of solvent-based inks will lead to environmental pollution and health risks.

Method used

Using a combination of self-crosslinked acrylic emulsion, self-crosslinked polyurethane emulsion, polyethylene wax emulsion, crosslinking agent, color paste and defoaming agent, resin-free water-based color paste is prepared by high-speed dispersion and grinding, combining crosslinking agent. and wax emulsion to improve the water solubility, adhesion and wear resistance of ink.

Benefits of technology

It realizes rapid drying, strong adhesion and high printing efficiency of water-based flexographic inks, reduces VOC emissions, complies with environmental protection standards, and is suitable for film materials such as PE, OPP and PET.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a water-dissolution-resistant water-based flexible printing ink for film printing and a preparation method thereof, and the printing ink comprises the following components in percentage by mass: 23-25% of a self-crosslinking acrylic emulsion, 23-25% of a self-crosslinking polyurethane emulsion, 3-5% of a polyethylene wax emulsion, 1-2% of a crosslinking agent, 35-40% of color paste, 0.1-0.2% of a defoaming agent and the balance of purified water. The self-crosslinking acrylic emulsion comprises 18-22% of acrylic resin which is a protective colloid, 10-12% of a hard-segment monomer which is styrene, 12-15% of a soft-segment monomer which is 2-ethylhexyl acrylate, and the balance of a pH regulator, an initiator, a crosslinking monomer and purified water. The self-crosslinking polyurethane emulsion comprises the following components in percentage by weight: 15-18% of polyester polyol serving as a soft segment, 9-11% of isophorone diisocyanate serving as a hard segment, 0.5-1% of trimethylolpropane, a chain extender, a solvent, a catalyst, a neutralizer and a post-chain extender. The water-based flexible printing ink is good in water solubility, high in drying speed, good in overprinting effect, good in printing effect and high in adhesive force, and has the characteristic of water dissolution resistance after being dried.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-based flexographic ink, in particular to a water-soluble and water-resistant water-based flexographic ink for film printing and a preparation method thereof. Background Art

[0002] At present, due to the requirements for printing effect, ink adhesion, printing speed, etc., most domestic films (soft packaging) are printed mainly with gravure solvent inks, supplemented by solvent flexographic inks. When using gravure solvent inks or solvent flexographic inks, volatile organic solvents must be used. These toxic and harmful organic solvents not only seriously pollute the environment and seriously affect the physical and mental health of production workers, but also bring challenges to the safe production of enterprises; and organic solvents remain in printed products, which will produce a relatively large solvent residual odor, and cause pollution to packaged items, affecting people's physical and mental health. After the new VOCs emission standards are introduced, it is even more necessary to upgrade the industry to reduce or control the emission of VOCs.

[0003] Therefore, it is a trend to switch from solvent-based gravure to water-based gravure in film (flexible packaging) printing. In the field of paper printing, water-based ink currently occupies a dominant position, but in the field of film printing, due to the non-absorbent characteristics of the film, it can only be dried by surface evaporation, so the drying speed of water-based ink on film printing is very slow. In addition, there are also disadvantages such as poor overprinting effect, low printing efficiency and weak adhesion, which affect the application and promotion of water-based ink in film printing. Summary of the invention

[0004] In view of the above-mentioned problems, the object of the present invention is to provide a water-based flexographic ink for film printing, which has good water solubility, fast drying speed, good overprinting effect, good printing effect, strong adhesion, and the printed product has the characteristic of being insoluble in water after drying, which can promote the development of water-based flexographic printing ink in the field of flexible packaging.

[0005] To solve the above problems, the technical solution adopted by the present invention is as follows:

[0006] A water-soluble and water-resistant water-based flexographic ink for film printing, characterized in that: by mass ratio, it comprises 23-25% of self-crosslinking acrylic emulsion, 23-25% of self-crosslinking polyurethane emulsion, 3-5% of polyethylene wax emulsion, 1-2% of crosslinking agent, 35-40% of color paste, 0.1-0.2% of defoaming agent and the balance of purified water;

[0007] The self-crosslinking acrylic emulsion comprises, by mass ratio, acrylic resin as protective colloid: 18-22%, hard segment monomer as styrene: 10-12%, soft segment monomer as isooctyl acrylate: 12-15%, and pH regulator, initiator, crosslinking monomer and purified water: the balance;

[0008] The self-crosslinking polyurethane emulsion comprises, by mass ratio, 15-18% polyester polyol as a soft segment, 9-11% isophorone diisocyanate as a hard segment, 0.5-1% trimethylolpropane, a chain extender, a solvent, a catalyst, a neutralizer, a coupling agent and a post-chain extender.

[0009] Preferably, in terms of mass ratio, the pH regulator is 5-6% ammonia water; and the initiator is 0.4-0.5% potassium persulfate.

[0010] Preferably, the crosslinking monomer is a combination of diacetone acrylamide: 0.8-1%, methacrylamide ethyl ethylene urea: 0.3-0.6%, methacrylate: 0.3-0.6% and adipic acid dihydrazide: 0.5-0.8% by mass ratio.

[0011] Preferably, in terms of mass ratio, the chain extender is N,N-dimethylpropionamide: 1.5-2.5%; the solvent is: dimethylformamide: 12-14% and pure water: the balance; the neutralizer is triethylamine: 1-1.5%; and the coupling agent is Shin-Etsu KBM-303 epoxy silane coupling agent: 0.5-1%.

[0012] Preferably, in terms of mass ratio, the post-chain extender is isophorone diamine: 1.2-1.6%.

[0013] Preferably, the self-crosslinking acrylic emulsion MFT has a temperature of 5 to 10° C. and a solid content of 38 to 42%; the self-crosslinking polyurethane emulsion has a solid content of 34 to 36% and a pH value of 7.5 to 8.5.

[0014] Preferably, the polyethylene wax emulsion is an aqueous dispersion of anionic high-density polyethylene wax powder, with a solid content of 40-42% and a softening point of 125-130°C.

[0015] Preferably, the color paste is a resin-free water-based color paste, which comprises, by mass ratio, 40-60% pigment, 0.3-0.5% defoamer, 12-15% dispersant, and the balance of purified water.

[0016] Preferably, the dispersant is DISPERBYK190 from BYK.

[0017] A method for preparing a water-soluble and water-resistant aqueous flexographic ink for film printing comprises the following steps:

[0018] S1: Put the components of the color paste into the mixing tank, disperse the pigment at high speed for 60 minutes, and then grind to fineness

[0019] ≤10μm, then you get resin-free water-based color paste;

[0020] S2: Mix the other components with the resin-free water-based color paste, and disperse them uniformly at high speed using a disperser to obtain the ink of the present invention.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The resin-free color paste in the formula of the present invention uses a high-efficiency dispersant with a high pigment affinity group to disperse the pigment and grind the pigment into a color paste, which can improve the dispersibility and stability of the ground pigment. Since the resin-free color paste does not have a grinding resin, the defect of the grinding resin itself being easily soluble in water can be avoided. At the same time, since the color paste does not have a resin, the reactivity problem of the grinding resin and other resins in the formula system can be avoided, which is beneficial to improving the physical and chemical properties and storage stability of flexographic ink.

[0023] 2. The formula of the present invention uses a self-crosslinking soft film-forming water-based acrylic emulsion with a lower MFT and a polyester-type anionic water-based polyurethane resin liquid, and is matched with functional additives such as a crosslinking agent and a wax emulsion to improve the water solubility, adhesion, wear resistance, scratch resistance and rubbing resistance of the ink as a whole.

[0024] 3. The water-based flexographic ink of the present invention dries quickly and is suitable for high-speed printing; it has good film-forming properties and a smooth surface.

[0025] It is cool and has strong adhesion. It is not easy to produce adhesion after printing and the printed product has strong water solubility resistance after drying. It can achieve better printing transfer effect, adhesion, scratch resistance, wear resistance and water solubility resistance on PE, OPP, PET and other film substrates with surface corona treatment.

[0026] 4. The flexographic water-based ink of the present invention uses water as solvent, is safe and environmentally friendly, has extremely low VOC emissions, and meets the requirements of national VOC emission standards. The water-based flexographic printing method replaces the gravure solvent-based ink, and printing on films has a large market space. DETAILED DESCRIPTION

[0028] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0030] The present invention is further described below with specific embodiments:

[0031] It should be noted that, unless otherwise specified, the raw materials used in the technical solutions provided by the present invention are prepared by conventional means or purchased through commercial channels.

[0032] A water-soluble water-based flexographic ink for film printing, the components and mass percentages of which are shown in Table 1 below:

[0033]

[0034]

[0035] Self-crosslinking acrylic emulsion: 23-25%, self-crosslinking polyurethane emulsion: 23-25%, polyethylene wax emulsion: 3-5%, crosslinking agent: 1-2%, color paste: 35-40%, defoaming agent: 0.1-0.2% and pure water: the balance.

[0036] In the above formula, the self-crosslinking acrylic emulsion MFT is 5-10°C and has a solid content of 38-42%.

[0037] The solid content of the self-crosslinking polyurethane emulsion is 34-36%, and the pH value is 7.5-8.5.

[0038] The polyethylene wax emulsion is specifically an aqueous dispersion of anionic high-density polyethylene wax powder, with a solid content of 40-42% and a softening point of 125-130°C.

[0039] The crosslinking agent is an epoxysilane crosslinking agent, and the polyethylene wax is an anionic high-density polyethylene wax emulsion.

[0040] Purified water is purified water filtered through reverse osmosis, with a resistance value of >15MΩ.cm and a pH value of 6.5-7.5.

[0041] The color paste is a resin-free water-based color paste. The color paste components and mass percentages are shown in Table 2 below:

[0042]

[0043] The color paste of the present invention does not contain resin, and a high molecular weight block copolymer solution containing pigment affinity groups is used as a dispersant to grind the pigment into a color paste, which can improve the dispersibility and stability of the ground pigment. The dispersant of this embodiment is DISPERBYK190 produced by BYK Chemical.

[0044] Since there is no grinding resin in the resin-free color paste, the defect of the grinding resin itself being easily soluble in water can be avoided. At the same time, since the color paste is resin-free, the reactivity problem between the grinding resin and other resins in the formula system can be avoided, which is beneficial to improving the physical and chemical properties and storage stability of the present invention.

[0045] The components and mass percentages of the self-crosslinking acrylic emulsion are shown in Table 3 below:

[0046]

[0047] The self-crosslinking acrylic emulsion of this embodiment has acrylic resin as protective colloid: 18-22%, styrene as hard segment monomer: 10-12%, isooctyl acrylate as soft segment monomer: 12-15%, and pH regulator, initiator, crosslinking monomer and solvent are added.

[0048] The pH regulator is ammonia water: 5-6%;

[0049] The initiator is potassium persulfate: 0.4-0.5%;

[0050] The cross-linking monomer is a combination of 0.8-1% diacetone acrylamide, 0.3-0.6% methacrylamide ethyl ethylene urea, 0.3-0.6% methacrylate and 0.5-0.8% adipic acid dihydrazide;

[0051] The solvent is pure water: the balance.

[0052] The components and mass percentages of the self-crosslinking polyurethane emulsion are shown in Table 4 below:

[0053]

[0054] The self-crosslinking polyurethane emulsion of this embodiment has a soft segment of polyester polyol: 15-18%, a hard segment of isophorone diisocyanate: 9-11%, and is added with a chain extender, a solvent, a catalyst, a neutralizer, a crosslinker, a coupling agent and a post-chain extender.

[0055] The chain extender is N,N-dimethylpropionamide: 1.5-2.5%;

[0056] The solvent is: dimethylformamide: 12-14% and pure water: the balance;

[0057] The neutralizing agent is triethylamine: 1-1.5%;

[0058] The cross-linking agent is 0.5-1% trimethylolpropane;

[0059] The coupling agent is an epoxy silane coupling agent: 0.5-1%;

[0060] The post-chain extender is isophorone diamine: 1.2-1.6%.

[0061] In this embodiment, the epoxy silane coupling agent is Shin-Etsu KBM-303 from Japan. KBM-303 silane coupling agent is a compound composed of organic matter and silicon. Its molecules have two or more different reactive groups that can chemically combine with inorganic materials and organic materials, which improves the mechanical strength, water solubility and adhesion of the ink after film formation.

[0062] The preparation method of the present invention comprises the following steps:

[0063] (1) Put the components of the color paste into a mixing tank, disperse the pigment at high speed for 60 minutes, and then grind to a fineness of ≤10 μm to obtain a resin-free water-based color paste;

[0064] (2) The other components are mixed with the resin-free water-based color paste, and dispersed uniformly at high speed using a disperser to obtain the ink of the present invention.

[0065] The inks prepared in Examples 1 to 5 were tested, and the main performance indicators are shown in Table 5 below:

[0066]

[0067] For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all these changes and deformations should fall within the scope of protection of the claims of the present invention. For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all these changes and deformations should fall within the scope of protection of the claims of the present invention.

Claims

1. A water-resistant, water-based flexographic ink for film printing, Features: Calculated by mass ratio, it includes self-crosslinking acrylic emulsion: 23-25%, self-crosslinking polyurethane emulsion: 23-25%, polyethylene wax emulsion: 3-5%, crosslinking agent: 1-2%, color paste: 35-40%, defoaming agent: 0.1-0.2% and pure water: the balance; The self-crosslinking acrylic emulsion comprises acrylic resin as protective colloid in terms of mass ratio: 18-22%, hard segment monomer is styrene: 10-12%, soft segment monomer is isooctyl acrylate: 12-15%, and pH regulator, initiator, cross-linking monomer and purified water: balance; The self-crosslinking polyurethane emulsion comprises a polyester polyol in the soft segment, based on the mass ratio: The hard segment is isophorone diisocyanate: 9-11%, trimethylolpropane: 0.5-1%, as well as a chain extender, a solvent, a catalyst, a neutralizer, a coupling agent and a post-chain extender.

2. A water-resistant and water-soluble aqueous flexographic ink for film printing as claimed in claim 1, Features: In terms of mass ratio, the pH regulator is 5-6% ammonia water; the initiator is 0.4-0.5% potassium persulfate.

3. A water-resistant and water-soluble aqueous flexographic ink for film printing as claimed in claim 1, Features: In terms of mass ratio, the crosslinking monomers are diacetone acrylamide: 0.8-1%, methacrylamide ethyl ethylene urea: 0.3-0.6%, methacrylate: 0.3-0.6% and adipic acid dihydrazide: 0.5~0.8% combination.

4. A water-resistant and water-soluble aqueous flexographic ink for film printing as claimed in claim 1, Features: In terms of mass ratio, the chain extender is 1.5-2.5% N,N-dimethylpropionamide; the solvent is 12-14% dimethylformamide and the balance is pure water; the neutralizer is triethylamine: 1~1.5%; the coupling agent is Shin-Etsu KBM-303 epoxy silane coupling agent: 0.5~1%.

5. A water-resistant and water-soluble aqueous flexographic ink for film printing as claimed in claim 1, Features: In terms of mass ratio, the post-chain extender is isophorone diamine: 1.2-1.6%.

6. A water-resistant and water-soluble aqueous flexographic ink for film printing as claimed in claim 1, Features: The self-crosslinking acrylic emulsion MFT: 5-10°C, solid content of 38-42%; the self-crosslinking polyurethane emulsion solid content of 34-36%, pH value of 7.5-8.

5.

7. A water-resistant and water-soluble aqueous flexographic ink for film printing as claimed in claim 1, Features: The polyethylene wax emulsion is an aqueous dispersion of anionic high-density polyethylene wax powder, with a solid content of 40-42% and a softening point of 125-130°C.

8. The water-resistant and water-soluble aqueous flexographic ink for film printing according to claim 1, Features: The color paste is a resin-free water-based color paste, and the color paste includes the following pigments by mass ratio: 40~60%, defoamer: 0.3~0.5%, dispersant: 12~15%, pure water: balance.

9. A water-resistant and water-soluble aqueous flexographic ink for film printing as claimed in claim 8, Features: The dispersant is DISPERBYK 190 from BYK.

10. A method for preparing a water-resistant and water-soluble aqueous flexographic ink for film printing according to any one of claims 1 to 9, It is characterized in that The following steps are involved: S1: Put the components of the color paste into a mixing tank, disperse the pigment at high speed for 60 minutes, and then grind to a fineness of ≤10μm to obtain a resin-free water-based color paste; S2: Mix the other components with the resin-free water-based color paste, and disperse them uniformly at high speed using a disperser to obtain the ink of the present invention.

Citation Information

Cited By

  • Water-based paint for printing film as well as preparation method and application of water-based paint

    CN120737684A

  • White oil-resistant water-based ink for printing corona-free treatment woven bag and preparation method of white oil-resistant water-based ink

    CN121652635A