Organic silicon block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating and preparation method thereof
The adhesion and electricality of existing coatings in high and low temperature and humidity environments are solved by solvent-free UV moisture dual-curing silicone block polyurethane acrylate resin for conformal coatings, combining polydimethylsiloxane and isocyanate monomers. The problem of insufficient performance achieves excellent adhesion and electrical insulation performance, is suitable for precision circuit board protection and meets environmental protection requirements.
Patent Information
- Application Number
- CN202411255869.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
AI Technical Summary
Existing electronic circuit board conformal coatings show insufficient adhesion, electrical properties and antistatic properties in high and low temperature and humidity environments, and most of them use organic solvents, which do not meet environmental protection requirements.
Silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coatings is used, and the weight fraction includes all UV cured silicone block polyurethane acrylate resin, all UV cured polyurethane acrylate resin and UV moisture dual-curing Cured polyurethane acrylate resin, combined with polydimethylsiloxane and isocyanate monomer, and the resin structure is designed by segmented excess grafting method to achieve good adhesion and electrical insulation properties.
It provides excellent adhesion, high and low temperature impact resistance and electrical insulation performance, meets the increasingly precise circuit board protection needs, meets environmental standards, and is suitable for rapid assembly line production.
Smart Images

Figure BDA0005034044680000021 
Figure BDA0005034044680000041 
Figure FDA0005034044660000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functionalized graft synthesis of organosilicon polymers and traditional polyurethane acrylate resins, and particularly relates to an organosilicon block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coatings and a preparation method thereof. Background Art
[0002] Electronic circuit boards are widely used in various electronic and electrical equipment, but they are easily damaged by moisture, static electricity, dust, high and low temperatures, etc. after long-term use, and there are risks such as copper rust, mildew, and short circuits. Conformal coatings are a coating material used to protect electronic circuit boards and improve their reliability and safety in long-term use. Conformal coatings currently mainly use systems such as acrylates, polyurethanes, and silicones. Each system has its own advantages and disadvantages, but the main problem with the various systems of conformal coatings currently used is that most of them are solvent-based conformal coatings with organic solvents as diluents, which do not meet the national environmental protection requirements. The electrical properties and high and low temperature impact resistance of acrylate and polyurethane conformal coatings in the three major systems are poor. Compared with silicone conformal coatings, they are also insufficient in insulation, flame retardancy, anti-static dust adhesion and other properties.
[0003] UV curing is a curing method that is more suitable for assembly line operations. It has 5E characteristics (Efficient, Enabling, Economical, Energy Saving, Environmental Friendly), especially in the field of thin coating. Although all-acrylate resin has the advantages of high gloss, high cross-linking, high sealing and waterproofness, it is insufficient in film toughness and adhesion to the substrate. It generally needs to be grafted with polyurethane. Although the toughness and adhesion performance of polyurethane grafted with acrylate are improved, it is still not enough to meet the needs of integrated circuit boards with increasingly precise specifications. Therefore, the market currently uses aliphatic polyester polyurethane acrylate to meet the balance of electronic circuit boards in terms of adhesion, toughness, cross-linking density, gloss, sealing, miscibility and other performance requirements. The shadow areas on the electronic circuit board that are not exposed to UV light due to the larger components of the electronic circuit board can also be coated with moisture-cured polyurethane through semi-enclosed polyurethane.
[0004] Another idea is to change the soft segment of polyurethane to replace aliphatic polyester, which also has the characteristics of yellowing resistance and flexibility. Reactive polydimethylsiloxane is one of them. Polydimethylsiloxane has good wettability with the laminated glass fiber material on the electronic circuit board, and has good air permeability from inside to outside, excellent high and low temperature impact resistance and electrical properties, but it also has the disadvantage that it cannot form intermolecular hydrogen bonds with the substrate. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coatings and a preparation method thereof, wherein the resin has excellent adhesion, good high and low temperature impact resistance and excellent electrical insulation properties.
[0006] The present invention provides a silicone block polyurethane acrylate resin for a solvent-free UV moisture dual-curing conformal coating, which comprises the following components in parts by weight:
[0007] 40 to 60 parts of a fully UV-curable silicone block polyurethane acrylate resin of structural formula I, 10 to 20 parts of a fully UV-curable polyurethane acrylate resin of structural formula II, 20 to 40 parts of a UV moisture dual-curable polyurethane acrylate resin of structural formula III, and 10 to 20 parts of a UV diluent monomer;
[0008]
[0009] Wherein, A in Formula I and Formula II is selected from 1≤x≤5;
[0010] In formula I and formula III, R' is selected from
[0011] In formula I, R" is selected from 10≤y≤30.
[0012] Preferably, the molecular weight of the fully UV-curable silicone block polyurethane acrylate resin is 1000-3000, the content of polydimethylsiloxane is 40-60wt%, and the main chain methyl polysiloxane provides rotational toughness by the helical structure of -Si-O-Si-;
[0013] The molecular weight of the UV moisture dual curing polyurethane acrylate resin is 300 to 1000;
[0014] The molecular weight of the fully UV-curable polyurethane acrylate resin is 500-2000.
[0015] Preferably, the UV diluent monomer is selected from one or more of 3,3,5-trimethylcyclohexyl acrylate, isobornyl acrylate, tetrahydrofurfuryl acrylate, cyclotrimethylolpropane formal acrylate and tricyclodecane dimethanol diacrylate.
[0016] The present invention provides a method for preparing a silicone block polyurethane acrylate resin for a solvent-free UV moisture dual-curing conformal coating as described in the above technical solution, comprising the following steps:
[0017] a) 2.2 to 2.5 parts of isocyanate, 1 part of hydroxyl-terminated polydimethylsiloxane, and part of the UV diluent monomer are vacuumed and stirred evenly in the absence of light radiation and at a temperature below 30° C. until there are no bubbles, then vacuuming is stopped, a catalyst and a polymerization inhibitor are added, and heating is performed for reaction to obtain a fully UV-curable silicone block polyurethane acrylate resin shown in structural formula I;
[0018] b) cooling to 28-33° C., adding 2.5-4.0 parts of terminal hydroxyl UV grafting monomer, controlling the system temperature to be below 40° C., performing reduced pressure evacuation, and stopping evacuation after confirming that there is no moisture in the system, adding catalyst and inhibitor, and heating for reaction to obtain a fully UV-curable polyurethane acrylate resin shown in structural formula II;
[0019] c) after the grafting of the main resin is completed, an isocyanate monomer is added to react with the residual terminal hydroxyl UV grafted monomer to obtain a UV moisture dual-curing polyurethane acrylate resin shown in structural formula III;
[0020] d) adding the remaining part of the UV dilution monomer to obtain a solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin.
[0021] Preferably, the average molecular weight of the hydroxy-terminated polydimethylsiloxane is between 500 and 2000;
[0022] The inhibitor is selected from phenolic inhibitors;
[0023] The isocyanate is selected from one or more of isophorone diisocyanate, hexamethylene diisocyanate, hexamethylene diisocyanate trimer, toluene diisocyanate, diphenylmethane diisocyanate and dicyclohexylmethane diisocyanate.
[0024] Preferably, the terminal hydroxyl UV grafting monomer is selected from one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate and hydroxyethyl acrylate polycaprolactone derivatives.
[0025] Preferably, when preparing the fully UV-curable organosilicon block polyurethane acrylate resin, the vacuum degree used is -80 kPa to -90 kPa.
[0026] Preferably, the heating reaction temperature in step a) is 50-80° C. and the time is 2-4 hours;
[0027] The heating reaction temperature in step b) is 50-80°C and the time is 2-4h;
[0028] The temperature of the reaction with the residual terminal hydroxyl UV grafting monomer in step c) is 60-80° C. and the time is 1-2 hours.
[0029] Preferably, the catalyst in step a) is selected from an organotin catalyst or an organobismuth catalyst.
[0030] The present invention provides a solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin, which comprises the following components by weight: 40 to 60 parts of a fully UV-curing silicone block polyurethane acrylate resin having a structure of formula I, 10 to 20 parts of a fully UV-curing polyurethane acrylate resin having a structure of formula II, 20 to 40 parts of a UV moisture dual-curing polyurethane acrylate resin having a structure of formula III, and 10 to 20 parts of a UV dilution monomer. The resin is embedded with flexible polydimethylsiloxane having good high and low temperature impact resistance and electrical properties, so it can meet the stringent requirements of circuit board protection with increasingly sophisticated integration in terms of stress resistance, flame retardancy and insulation performance; it has excellent adhesion to PCB boards; and it exhibits excellent thermal shock resistance within -45°C to 200°C. DETAILED DESCRIPTION
[0031] The present invention provides a silicone block polyurethane acrylate resin for a solvent-free UV moisture dual-curing conformal coating, which comprises the following components in parts by weight:
[0032] 40 to 60 parts of a fully UV-curable silicone block polyurethane acrylate resin of structural formula I, 10 to 20 parts of a fully UV-curable polyurethane acrylate resin of structural formula II, 20 to 40 parts of a UV moisture dual-curable polyurethane acrylate resin of structural formula III, and 10 to 20 parts of a UV diluent monomer;
[0033]
[0034] Wherein, A in Formula I and Formula II is selected from 1≤x≤5;
[0035] In formula I and formula III, R' is selected from
[0036] In formula I, R" is selected from 10≤y≤30.
[0037] The invention adopts a mixed use of organosilicon segments and aliphatic polyesters, adopts a monomer segmented excess addition grafting method to design a dual-curing resin structure, and utilizes the moisture curing characteristics of polyurethane to prepare a solvent-free UV moisture dual-curing conformal coating organosilicon block polyurethane acrylate resin.
[0038] In the present invention, the molecular weight of the fully UV-curable silicone segmented polyurethane acrylate resin is 1000-3000, the content of polydimethylsiloxane is 40-60wt%, the main chain methyl polysiloxane provides rotational toughness by the helical structure of -Si-O-Si-, and as anchoring positions, there are an average of more than four large conjugated π bonds of urethane and more than four ester bonds in contact with the substrate to generate intermolecular hydrogen bonds and ensure good adhesion, and the intervals of UV curing points are on average more than 20 C, N, O positions and provide good shrinkage resistance.
[0039] The molecular weight of the UV-moisture dual-curing polyurethane acrylate resin is 300-1000; as anchoring sites, it has an average of more than one large conjugated π bond of carbamate and more than two ester bonds in contact with the substrate to generate intermolecular hydrogen bonds. After the first step of UV curing, the UV-curing cross-linking point at one end of the structure forms a flat structure with other component resins, while the NCO at the other end protrudes out of the main chain and forms a urea bond with the NCO in other spatial structures through moisture curing, thereby providing excellent flexibility and adhesion protection properties for electronic circuit boards.
[0040] The molecular weight of the fully UV-curable polyurethane acrylate resin is 500-2000, and the main chain isocyanate adopts a hydrophobic organic phase with strong solubility and provides good substrate wettability and system miscibility. As anchoring sites, there are an average of more than two large conjugated π bonds of urethane and more than four ester bonds in contact with the substrate to generate intermolecular hydrogen bonds and ensure good adhesion. The intervals of the UV curing points are on average more than 10 C, N, O positions and provide good shrinkage resistance.
[0041] In the present invention, the UV diluent monomer is selected from one or more of 3,3,5-trimethylcyclohexyl acrylate, isobornyl acrylate, tetrahydrofurfuryl acrylate, cyclotrimethylolpropane formal acrylate and tricyclodecane dimethanol diacrylate.
[0042] The present invention provides a method for preparing a silicone block polyurethane acrylate resin for a solvent-free UV moisture dual-curing conformal coating as described in the above technical solution, comprising the following steps:
[0043] a) 2.2 to 2.5 parts of isocyanate, 1 part of hydroxyl-terminated polydimethylsiloxane, and part of the UV diluent monomer are vacuumed and stirred evenly in the absence of light radiation and at a temperature below 30° C. until there are no bubbles, then vacuuming is stopped, a catalyst and a polymerization inhibitor are added, and heating is performed for reaction to obtain a fully UV-curable silicone block polyurethane acrylate resin shown in structural formula I;
[0044] b) cooling to 28-33° C., adding 2.5-4.0 parts of terminal hydroxyl UV grafting monomer, controlling the system temperature to be below 40° C., performing reduced pressure evacuation, and stopping evacuation after confirming that there is no moisture in the system, adding catalyst and inhibitor, and heating for reaction to obtain a fully UV-curable polyurethane acrylate resin shown in structural formula II;
[0045] c) after the grafting of the main resin is completed, isocyanate is added to react with the residual terminal hydroxyl UV grafting monomer to obtain a UV moisture dual curing polyurethane acrylate resin shown in structural formula III;
[0046] d) adding the remaining part of the UV dilution monomer again to obtain a solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin.
[0047] The method provided by the invention adopts a one-pot process of segmented excess grafting, and the preparation process is safe and reliable, the operation is convenient, and the components in the mixed resin have good compatibility.
[0048] The present invention prepares 2.2 to 2.5 parts of isocyanate, 1 part of terminal hydroxyl polydimethylsiloxane and part of UV diluent monomer, vacuumizes and stirs evenly in the absence of light radiation and at a temperature below 30° C. until there are no bubbles, then stops vacuumizing, adds a catalyst and an inhibitor, and heats for reaction to obtain a fully UV-curable organic silicon segmented polyurethane acrylate resin.
[0049] In the present invention, the isocyanate is selected from one or more of isophorone diisocyanate, hexamethylene diisocyanate, hexamethylene diisocyanate trimer, toluene diisocyanate, diphenylmethane diisocyanate and dicyclohexylmethane diisocyanate.
[0050] In the present invention, the average molecular weight of the hydroxyl-terminated polydimethylsiloxane is 500 to 2000. The polymerization inhibitor is selected from phenolic polymerization inhibitors; the catalyst in step a) is selected from organic tin catalysts or organic bismuth catalysts. In step a), the polymerization inhibitor and the catalyst are preferably added in a metered manner, and the addition ratio of the polymerization inhibitor is preferably 1‰ to 2‰; the preferred ratio of the catalyst is 0.5‰ to 2‰.
[0051] In the present invention, the UV diluent monomer is selected from one or more of 3,3,5-trimethylcyclohexyl acrylate, isobornyl acrylate, tetrahydrofurfuryl acrylate, cyclotrimethylolpropane formal acrylate and tricyclodecane dimethanol diacrylate.
[0052] The temperature of the heating reaction in step a) of the present invention is 50-80°C, and the time is 2-4h. Specifically, after adding the catalyst and the inhibitor, the present invention heats to 50°C, observes the progress of the reaction, and the maximum reaction temperature does not exceed 80°C, and is ideally controlled at around 60°C. During the reaction, the change of the hydroxyl value in the system needs to be monitored in a timely manner until the hydroxyl groups in the system are completely reacted and consumed to obtain a fully UV-curable silicone block polyurethane acrylate resin having a structure of formula I, and some isocyanate remains in the system. In the process of monitoring the change of the hydroxyl value, the sampling time interval of the present invention is 1h, and the sampling is 2-6 times, preferably 2-4 times; the preferred reaction time is 2-4h.
[0053] When preparing the fully UV-curable organosilicon block polyurethane acrylate resin, the vacuum degree used is -80 kPa to -90 kPa, preferably -80 to -84 kPa.
[0054] After obtaining the fully UV-curable silicone segmented polyurethane acrylate resin, the system is cooled to 28-33° C., 2.5-4.0 parts of terminal hydroxyl UV grafting monomers are added, the system temperature is controlled below 40° C., and vacuuming is performed under reduced pressure. After confirming that there is no moisture in the system, vacuuming is stopped, and the reaction is heated to obtain a fully UV-curable polyurethane acrylate resin.
[0055] In the present invention, the terminal hydroxyl UV grafting monomer is selected from one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate and hydroxyethyl acrylate polycaprolactone derivatives.
[0056] The temperature of the heating reaction in step b) of the present invention is 50-80°C, and the time is 2-4 hours. Specifically, in this step, the reaction is heated to 50°C under stirring conditions, and the reaction is observed. The maximum reaction temperature does not exceed 80°C, and is ideally controlled at 60°C. During the reaction, the change of the NCO value in the system needs to be detected in a timely manner until the NCO in the reaction is completely consumed. The reaction time is 2-4 hours. After the reaction in this step, a fully UV-curable polyurethane acrylate resin is obtained in the system, and the structural formula is shown in Formula II, and some terminal hydroxyl UV grafting monomers remain in the system.
[0057] In step c) of the present invention, after the grafting of the main resin (resin of formula I and formula II) is completed, isocyanate monomer is added to react with the residual terminal hydroxyl UV grafted monomer to obtain UV moisture dual curing polyurethane acrylate resin, the structural formula of which is shown in formula III. The present invention adjusts the NCO content of the system to a suitable range by adding different amounts of isocyanate monomers, preferably the NCO content range is 4% to 10%, the reaction time is controlled at 1 to 2 hours, the reaction temperature is 60 to 80°C, and is ideally controlled at around 60°C. During the reaction, the change of NCO content in the system needs to be monitored in a timely manner.
[0058] Finally, the present invention adds the remaining part of the UV dilution monomer to adjust the viscosity of the system to obtain a silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating. The total amount of the part of the UV dilution monomer in step a) and the remaining part of the UV dilution monomer in step d) is 1 to 20 parts; the part of the UV dilution monomer accounts for 30 to 50% of the total amount of the UV dilution monomer. The present invention can adjust the viscosity and dispersing, wetting and defoaming properties of the system by adding a radiation-curing defoamer and a wetting and dispersing silicon auxiliary agent. After stirring evenly at 30°C, vacuum degassing is complete to obtain a silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating.
[0059] Compared with the prior art, the present invention provides a silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating and a preparation method thereof, which has the following beneficial effects:
[0060] 1) The method for preparing the solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin provided by the present invention is safe and reliable, easy to operate, and has no troublesome post-treatment of residual liquid.
[0061] 2) The main structure of the silicone block polyurethane acrylate resin for the solvent-free UV moisture dual-curing conformal coating provided by the present invention is a silicone segment, which has low surface tension and resistance to moisture, dust and corrosive gas adhesion, good antistatic insulation and flame retardant properties and excellent mechanical and electrical properties to meet the increasingly sophisticated circuit board component protection requirements.
[0062] 3) The solvent-free UV moisture dual-curing conformal coating provided by the present invention uses the moisture curing mechanism of aliphatic polyester polyurethane acrylate, and embeds aliphatic polyester and polydimethylsiloxane in the main chain. At the same time, in order to solve the problem of decreased adhesion to the substrate, an acrylate siloxane coupling agent can be added to meet the stringent requirements of electronic circuit boards in terms of high and low temperature impact resistance, electrical properties and excellent adhesion, as well as surface sealing hardness, gloss coating, transparency and other balanced performance, and the coating and curing of shadow areas that are not exposed to UV light are completed through the second step of moisture curing.
[0063] 4) The average molecular weight of the silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating provided by the present invention is moderate, which can better wet the semiconductor components soldered on the circuit board and form a protective coating with uniform distribution and consistent thickness, while meeting the national environmental protection policy and satisfying the fast assembly line production process.
[0064] The organic silicon segmented polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating provided by the present invention has good storage stability and flexible application formula, and can meet the requirements of different places and different application fields.
[0065] To further illustrate the present invention, a solvent-free UV moisture dual-curing conformal coating organic silicone block polyurethane acrylate resin and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0066] Example 1
[0067] 1) Take 50g of isophorone diisocyanate, 100g of hydroxyl-terminated polydimethylsiloxane (molecular weight 1000), and 30g of 3,3,5-trimethylcyclohexyl acrylate, evacuate and stir evenly without light radiation and below 30°C until there are no bubbles, then stop evacuating and add 8108 and 0.6g 2,6-di-tert-butyl-p-cresol, stir and heat to 50℃, observe the reaction progress, control the reaction temperature not to exceed 80℃, monitor the change of hydroxyl value in the system in time during the reaction, until the hydroxyl in the system is completely reacted and consumed, the reaction time is 2 hours;
[0068] 2) After the reaction is completed, the temperature is lowered to 30°C, 60g of hydroxyethyl acrylate caprolactone adduct is added, the system temperature is controlled below 40°C, the system is decompressed and vacuumed, and after confirming that there is no moisture in the system, the vacuuming is stopped and additional 8108, heated to 50°C with stirring, observed the reaction, controlled the reaction temperature not to exceed 80°C, and timely detected the change of NCO content in the system during the reaction until NCO was completely consumed in the reaction, and the reaction time was 2 hours;
[0069] 3) After the main resin is grafted, 20g of isophorone diisocyanate is added to react with the hydroxyethyl acrylate caprolactone adduct remaining in the system to prepare the UV moisture dual-curing component resin, and the NCO content of the system is adjusted to 8%wt, the reaction time is controlled at 1 to 2 hours, the maximum reaction temperature does not exceed 80°C, and the reaction temperature is controlled at about 60°C during the experiment. Finally, 10g of isobornyl acrylate and a small amount of radiation-curable defoaming, wetting and dispersing silicone additive are added to adjust the viscosity and dispersing, wetting and defoaming properties of the system respectively, and 0.3g of 2,6-di-tert-butyl-p-cresol is added as needed. After stirring evenly at 30°C, vacuum is evacuated until the degassing is complete, and the desired solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin is obtained.
[0070] 4) The prepared solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin is in a colorless, transparent, viscous liquid state; the viscosity is 212.8 cP.
[0071] Example 2
[0072] 1) Take 50g of isophorone diisocyanate, 100g of hydroxyl-terminated polydimethylsiloxane (molecular weight 1000), and 20g of 3,3,5-trimethylcyclohexyl acrylate, evacuate and stir evenly without light radiation and below 30°C until there are no bubbles, then stop evacuating and add 8108 and 0.6g 2,6-di-tert-butyl-p-cresol, stir and heat to 50℃, observe the reaction, control the reaction temperature not to exceed 80℃, and control the reaction temperature at around 60℃ during the experiment. During the reaction, the change of hydroxyl value in the system should be monitored in time until the hydroxyl in the system is completely reacted and consumed. The reaction time is 2 hours;
[0073] 2) After the reaction is completed, the temperature is lowered to about 30°C, 32g of hydroxypropyl acrylate is added, the system temperature is controlled to be below 40°C, and the system is vacuumed under reduced pressure. After confirming that there is no moisture in the system, the vacuuming is stopped and the addition of 8108, stir and heat to about 50℃, observe the reaction, control the reaction temperature not to exceed 80℃, and control the reaction temperature at about 60℃ during the experiment. During the reaction, the change of NCO value in the system should be detected in time until NCO in the reaction is completely consumed. The reaction time is 2 hours;
[0074] 3) After the main resin is grafted, 20g of isophorone diisocyanate is added to react with the hydroxypropyl acrylate adduct remaining in the system to prepare a UV moisture dual-curing component resin, and the NCO content of the system is adjusted to 8%wt. The reaction time is controlled at 1 to 2 hours, and the maximum reaction temperature does not exceed 80°C. During the reaction, the change of the NCO value in the system needs to be monitored in time. Finally, 20g of isobornyl acrylate and part of the radiation-curable defoaming, wetting and dispersing silicone additives are added to adjust the viscosity and dispersing, wetting and defoaming properties of the system respectively, and 0.3g of 2,6-di-tert-butyl-p-cresol is added as needed. After stirring evenly at 30°C, vacuum degassing is performed completely to obtain a solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin.
[0075] 4) The prepared solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin is in a colorless, transparent, viscous liquid state; the viscosity is 269 cP.
[0076] Embodiment 3:
[0077] 1) Take 60g of dicyclohexylmethane diisocyanate, 100g of hydroxyl-terminated polydimethylsiloxane (molecular weight 2000), and 20g of 3,3,5-trimethylcyclohexyl acrylate, evacuate and stir evenly without light radiation and below 30°C until there are no bubbles, then stop evacuating and add 8108 and 0.6g 2,6-di-tert-butyl-p-cresol, stir and heat to 50℃, observe the reaction, control the reaction temperature not to exceed 80℃, and control the reaction temperature at around 60℃ during the experiment. During the reaction, the change of hydroxyl value in the system should be monitored in time until the hydroxyl in the system is completely reacted and consumed. The reaction time is 2 hours;
[0078] 2) After the reaction is completed, the temperature is lowered to about 30°C, 32g of hydroxypropyl acrylate is added, the system temperature is controlled to be below 40°C, and the system is vacuumed under reduced pressure. After confirming that there is no moisture in the system, the vacuuming is stopped and the addition of 8108, heated to about 50°C with stirring, observed the reaction, controlled the reaction temperature not to exceed 80°C, and controlled the reaction temperature at about 60°C during the experiment. The change of NCO value in the system should be detected in due time during the reaction until NCO in the reaction is completely consumed. The reaction time is 2 hours;
[0079] 3) After the main resin is grafted, 20g of dicyclohexylmethane diisocyanate is added to react with the hydroxypropyl acrylate remaining in the system to prepare a UV moisture dual-curing component resin, and the NCO content of the system is adjusted to 8%wt. The reaction time is controlled at 1 to 2 hours, the maximum reaction temperature does not exceed 80°C, and the reaction temperature is controlled at about 60°C during the experiment. During the reaction, the change of the NCO value in the system needs to be monitored in time. Finally, 20g of isobornyl acrylate and part of the radiation-curable defoaming, wetting and dispersing silicone additives are added to adjust the viscosity and dispersing, wetting and defoaming properties of the system respectively, and 0.3g of 2,6-di-tert-butyl-p-cresol is added as needed. After stirring evenly at 30°C, vacuum degassing is performed to obtain a solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin.
[0080] 4) The prepared solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin is in a colorless, transparent, viscous liquid state; the viscosity is 311 cP.
[0081] Application performance testing:
[0082] The solvent-free UV moisture dual-curing conformal coating prepared in Example 1 was prepared with silicone block polyurethane acrylate resin and applied to a PCB circuit board for performance testing.
[0083] Coating configuration: add diluent monomers such as isobornyl acrylate, trimethylol cyclohexyl acrylate, and mixture 2 parts (mass ratio is 1:1) in sequence; additives such as BYK 141, BYK 3500, Digo 2300, Digo 270, and Shin-Etsu KBM-5103 mixture 1 part (mass ratio is 2:1:2:1:4); inhibitor BHT 0.01 part; photoinitiator 2-hydroxy-2-methyl benzophenone, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 2-benzoyl methyl benzoate, 2-isopropylthioxanthone mixture 1 part (mass ratio is 2:1:2:1); then stir and disperse completely, add 10 parts of solvent-free UV moisture dual-curing silicone block polyurethane acrylate resin prepared in Example 1, stir in vacuum and avoid light until there are no obvious bubbles and the liquid is in a uniform phase, filter through a 100-mesh filter and can it. Apply it on the surface of the PCB circuit board by spraying.
[0084] Test after coating curing: After the sprayed coating is cured by UV and moisture dual curing on the PCB surface, the coating shows excellent adhesion on the PCB surface after curing. According to the coating adhesion cross-cut test (GB / T9286-88), it reaches 5B grade, that is, the cut edge is smooth and there is no peeling at the grid edge; the Shore hardness test is 56A; the coating has excellent electrical insulation performance, and there is no leakage current when powered on for 1 minute at a voltage of 1500VAC; the surface resistance test is 0.57*10 13 Ω; In the temperature range of -45℃~200℃, stay at each temperature for 30min, and conduct 80 cycles of hot and cold shock test. The coating has no obvious cracking and passes the hot and cold shock test.
[0085] Similarly, the solvent-free UV moisture dual-curing conformal coatings prepared in Example 2 and Example 3 were formulated with silicone block polyurethane acrylate resin and applied to PCB circuit boards for performance testing.
[0086] Example 2 Coating configuration: add 2 parts of the mixture of diluent monomers isobornyl acrylate and trimethylol cyclohexyl acrylate (mass ratio is 1:1); 1 part of the mixture of additives Bick 141, Bick 3500, Digo 2300, Digo 270, Shin-Etsu KBM-5103 (mass ratio is 2:1:1:1:4); 0.01 part of the polymerization inhibitor BHT; 1 part of the mixture of photoinitiator 2-hydroxy-2-methyl benzophenone, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 2-benzoyl methyl benzoate, 2-isopropylthioxanthone (mass ratio is 2:1:2:1); then stir and disperse completely, add 10 parts of the solvent-free UV moisture dual-curing silicone block polyurethane acrylate resin prepared in Example 2, stir in vacuum and avoid light until there are no obvious bubbles and the liquid is in a uniform phase, filter through a 100-mesh filter and can it. Apply it on the surface of the PCB circuit board by spraying.
[0087] Test after coating curing: After the sprayed coating is cured by UV and moisture dual curing on the PCB surface, the coating shows excellent adhesion on the PCB surface after curing. According to the coating adhesion cross-cut test (GB / T9286-88), it reaches 5B grade, that is, the cut edge is smooth and there is no peeling at the grid edge; the Shore hardness test is 60A; the coating has excellent electrical insulation performance, and there is no leakage current when powered on for 1 minute at a voltage of 1500VAC; the surface resistance test is 0.61*10 13 Ω; In the temperature range of -45℃~200℃, stay at each temperature for 30min, and conduct 80 cycles of hot and cold shock test. The coating has no obvious cracking and passes the hot and cold shock test.
[0088] Example 3 coating configuration: add 2 parts of the mixture of diluent monomers isobornyl acrylate and trimethylol cyclohexyl acrylate (mass ratio is 1:1); 1 part of the mixture of additives Bick 141, Bick 3500, Digo 2300, Digo 270, Shin-Etsu KBM-5103 (mass ratio is 2:1:2:1:4); 0.01 parts of the polymerization inhibitor BHT; 1.2 parts of the mixture of photoinitiator 2-hydroxy-2-methyl benzophenone, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 2-benzoyl benzoic acid methyl ester, 2-isopropylthioxanthone (mass ratio is 2:1:2:1); then stir and disperse completely, add 10 parts of the solvent-free UV moisture dual-curing silicone block polyurethane acrylate resin prepared in Example 3, stir in vacuum and avoid light until there are no obvious bubbles and the liquid is in a uniform phase, filter through a 100-mesh filter and can it. Apply it on the surface of the PCB circuit board by spraying.
[0089] Test after coating curing: After the sprayed coating is cured by UV and moisture dual curing on the PCB surface, the coating shows excellent adhesion on the PCB surface after curing. According to the coating adhesion cross-cutting test (GB / T9286-88), it reaches 5B grade, that is, the cut edge is smooth and there is no peeling at the grid edge; the Shore hardness test is 62A; the coating has excellent electrical insulation performance, and there is no leakage current when powered on for 1 minute at a voltage of 1500VAC; the surface resistance test is 0.62*10 13 Ω; In the temperature range of -45℃~200℃, stay at each temperature for 30min, and conduct 80 cycles of hot and cold shock test. The coating has no obvious cracking and passes the hot and cold shock test.
[0090] As can be seen from the above embodiments, the viscosity of the resin provided by the present invention is adjustable to meet the needs of different climatic regions, is environmentally friendly and solvent-free, and is easy to apply. In the area of the circuit board components that can be irradiated by UV, the curing speed is fast, which can meet the automated assembly line process. The shadow areas generated by the high and low positions on the sides of the components that cannot be irradiated by UV light can also be completely coated and protected by two-step moisture curing. Since the resin is embedded with flexible polydimethylsiloxane with good high and low temperature impact resistance and electrical properties, it can meet the stringent requirements of circuit board protection with increasingly sophisticated integration in terms of stress resistance and flame retardant insulation. At the same time, the organosilicon itself has good wetting between the glass fiber laminated circuit board material, low surface tension and excellent heat dissipation and air permeability from the inside to the outside. With the automatic spraying equipment that can control the film thickness and the high crosslinking density after UV curing, the coated circuit board can have excellent comprehensive protection performance. As for the defects of organosilicon such as low adhesion to the circuit board and low gloss and low hardness of the coating surface, they can also be solved by embedding aliphatic polyester in the main resin and using silane coupling agents such as KH-570 and high gloss and high glass transition temperature UV dilution monomers. The preparation process of the present invention is safe and reliable, and can be applied to circuit board protection fields such as high-end PCB industrial electronics, automotive electronics, consumer electronics, aerospace electronics and military electronics.
[0091] The experimental results show that the solvent-free UV moisture dual curing conformal coating is made of silicone block polyurethane acrylate resin and then cured on the surface of the PCB board by UV moisture dual curing. The coating has a Shore hardness of 56A~60A; the coating has excellent electrical insulation performance. Under a voltage of 1500VAC, there is no leakage current phenomenon when powered on for 1 minute; the surface resistance test is 0.57*10 13 Ω~0.61*10 13 Ω; In the temperature range of -45℃~200℃, stay at each temperature for 30min, and conduct 80 cycles of hot and cold shock test. The coating has no obvious cracking and passes the hot and cold shock test.
[0092] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating, comprising the following components in parts by weight: 40 to 60 parts of a fully UV-curable silicone block polyurethane acrylate resin of structural formula I, 10 to 20 parts of a fully UV-curable polyurethane acrylate resin of structural formula II, 20 to 40 parts of a UV moisture dual-curable polyurethane acrylate resin of structural formula III, and 10 to 20 parts of a UV diluent monomer; in, In formula I and formula II, A is selected from 1≤x≤5; In formula I and formula III, R' is selected from In formula I, R" is selected from 10≤y≤30.
2. The organic silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating according to claim 1, characterized in that: The molecular weight of the fully UV-curable silicone block polyurethane acrylate resin is 1000-3000, the content of polydimethylsiloxane is 40-60wt%, and the main chain methyl polysiloxane provides rotational toughness by the helical structure of -Si-O-Si-; The molecular weight of the UV moisture dual curing polyurethane acrylate resin is 300 to 1000; The molecular weight of the fully UV-curable polyurethane acrylate resin is 500-2000.
3. The organic silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating according to claim 1, characterized in that: The UV diluent monomer is selected from one or more of 3,3,5-trimethylcyclohexyl acrylate, isobornyl acrylate, tetrahydrofurfuryl acrylate, cyclotrimethylolpropane formal acrylate and tricyclodecane dimethanol diacrylate.
4. A method for preparing the silicone block polyurethane acrylate resin for solvent-free UV moisture dual-curing conformal coating according to claim 1, comprising the following steps: a) 2.2 to 2.5 parts of isocyanate, 1 part of hydroxyl-terminated polydimethylsiloxane, and part of the UV diluent monomer are vacuumed and stirred evenly in the absence of light radiation and at a temperature below 30° C. until there are no bubbles, then vacuuming is stopped, a catalyst and a polymerization inhibitor are added, and heating is performed for reaction to obtain a fully UV-curable silicone block polyurethane acrylate resin shown in structural formula I; b) cooling to 28-33° C., adding 2.5-4.0 parts of terminal hydroxyl UV grafting monomer, controlling the system temperature to be below 40° C., performing reduced pressure evacuation, and stopping evacuation after confirming that there is no moisture in the system, adding catalyst and inhibitor, and heating for reaction to obtain a fully UV-curable polyurethane acrylate resin shown in structural formula II; c) after the grafting of the main resin is completed, an isocyanate monomer is added to react with the residual terminal hydroxyl UV grafted monomer to obtain a UV moisture dual-curing polyurethane acrylate resin shown in structural formula III; d) adding the remaining part of the UV dilution monomer to obtain a solvent-free UV moisture dual-curing conformal coating silicone block polyurethane acrylate resin.
5. The method according to claim 4, characterized in that The average molecular weight of the hydroxy-terminated polydimethylsiloxane is between 500 and 2000; The inhibitor is selected from phenolic inhibitors; The isocyanate is selected from one or more of isophorone diisocyanate, hexamethylene diisocyanate, hexamethylene diisocyanate trimer, toluene diisocyanate, diphenylmethane diisocyanate and dicyclohexylmethane diisocyanate.
6. The method according to claim 4, characterized in that The terminal hydroxyl UV grafting monomer is selected from one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate and hydroxyethyl acrylate polycaprolactone derivatives.
7. The method according to claim 4, characterized in that When preparing the fully UV-curable organosilicon block polyurethane acrylate resin, the vacuum degree used is -80 kPa to -90 kPa.
8. The method according to claim 4, characterized in that The heating reaction temperature in step a) is 50-80°C and the time is 2-4h; The heating reaction temperature in step b) is 50-80°C and the time is 2-4h; The temperature of the reaction with the residual terminal hydroxyl UV grafting monomer in step c) is 60-80° C. and the time is 1-2 hours.
9. The method according to claim 4, characterized in that The catalyst in step a) is selected from an organic tin catalyst or an organic bismuth catalyst.
Citation Information
Patent Citations
UV light-cured organic silicon polyurethane acrylate monomer and preparation method thereof
CN109265686A
Preparation method of UV-cured organic silicon modified hyperbranched polyurethane material
CN111393608A
Acrylate modified organic silicon resin and application thereof in ultraviolet (UV) / moisture dual-curing organic silicon conformal coating
CN114409905A
Resin for solvent-free UV moisture dual-curing organic silicon conformal coating as well as preparation method and application thereof
CN118271620A
Cited By
Silane modified polyurethane acrylate resin, preparation method thereof and anticorrosive paint
CN120965967A
Single coating type UV and heat dual-curing laser anti-counterfeiting coating and UV mold pressing microstructure copying process
CN121930733A