Method for inhibiting needle-like platinum metal precipitation in high-level liquid waste glass curing process
By controlling the particle size of the base glass and the Na2O/RuO2 mass ratio, the precipitation morphology of platinum group metals during the glass curing process of high-level radioactive waste liquid is regulated, solving the furnace operation problem caused by the precipitation of platinum group metals in the existing technology, and improving the stability and safety of the glass curing body.
Patent Information
- Application Number
- CN202410981499.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing high-level radioactive waste glass curing process, the morphology control methods for platinum group metal precipitates can reduce the chemical stability of the glass-cured body and may lead to furnace operation accidents, such as abnormal resistivity and viscosity. The chemical reagents introduced by the existing technology cause additional problems.
By controlling the particle size and distribution of the base glass and the Na2O/RuO2 mass ratio, the precipitation morphology of platinum group metals during the glass curing process of high-level radioactive waste liquid is regulated to avoid the formation of needle-like crystals. A method that does not change the chemical composition of the glass is adopted, using a base glass composed of SiO2, B2O3, Al2O3, CaO, Li2O, Na2O, etc., mixed with high-level radioactive waste liquid to control the RuO2 precipitates to be in particulate form.
It effectively suppresses the precipitation of needle-shaped platinum group metals, reduces their impact on the electrical conductivity and viscosity of the glass melt, ensures the safe operation of the furnace, and does not change the chemical composition of the glass solidified body. It is suitable for high-level radioactive waste liquids with different chemical compositions and is easy to operate.
Smart Images

Figure CN118942759A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of radioactive nuclear waste solidification treatment, and in particular to a method for inhibiting the precipitation of needle-shaped platinum group metals during the glass solidification process of high-level waste liquid. Background Art
[0002] The spent fuel reprocessing process inevitably produces high-level liquid waste, which has extremely strong biological toxicity and radioactivity, and is extremely harmful to the ecological environment. It usually needs to be solidified by glass and then disposed of in deep geology to isolate it from the biosphere to the greatest extent. Vitrification refers to the technology of evaporating, calcining, melting and casting high-level liquid waste with a glass substrate at high temperature to form a stable glass solid. The glass solid is resistant to leaching, radiation, and has a wide tolerance for elements. Its production is easy to control remotely. It is currently the only high-level liquid waste treatment technology for engineering applications in the world. However, the platinum group metals ruthenium (Ru), rhodium (Rh), and palladium (Pd) in high-level liquid waste have extremely low solubility in borosilicate glass (generally less than 100ppm) and high melting point (>2000℃) and stable chemical properties, so they are often suspended in the glass melt as individual particles. The density of platinum group metals and their oxides (7-13g / cm 3 ) is much higher than the density of glass melt (2.4-2.9g / cm 3 ), during the long-term continuous operation of the furnace, the particles of platinum metals and their oxides gradually grow larger, settle and accumulate at the bottom of the molten pool, and form a "sludge" glass melt rich in platinum metals. When the platinum metal content in the "sludge" exceeds 15wt%, its resistivity is more than 20 times lower than that of normal glass melt, which can easily cause excessive local current density at the bottom of the furnace, leading to operation interruption; and its viscosity is generally nearly 10 times higher than that of the melt, which can easily cause faults such as poor discharge and blockage of the discharge port.
[0003] Ru in the platinum group metals accounts for the highest proportion in high-level radioactive waste (generally greater than 7wt%), and its precipitates have the greatest impact on the properties of glass melts. During the glass solidification process, Ru is mainly present in the form of needle-shaped RuO 2 Studies have shown that in RuO 2 When the precipitate content is the same, the needle-shaped RuO 2 The conductivity and viscosity of the crystals are much higher than those of granular RuO 2 The main reason is that the needle-shaped crystal particles are easy to form a network structure and increase the conductivity and viscosity, thus causing furnace operation accidents.
[0004] Regarding the method for controlling the morphology of platinum metal precipitates during the glass solidification process of high-level radioactive waste, the existing patent 202211408096.6 discloses a glass solidification body and a preparation method thereof for improving the deposition of precious metals, which is to introduce a small amount of P into borosilicate glass. 2 O 5 and Fe2 O 3 , making RuO 2 The precipitate is in granular form, which improves the viscosity and conductivity of the glass melt, thereby extending the life of the glass solidification furnace. However, the additional P and Fe elements introduced by this technical solution change the chemical composition of the final glass solidification body, which brings challenges to its practical application. For example, the introduction of P is likely to cause phase separation of borosilicate glass and reduce the chemical stability of the glass solidification body; and the introduction of Fe will cause it to form refractory spinel phase precipitates with elements such as Mg, Ni, and Cr in high-level radioactive waste during the glass solidification process, blocking the discharge port and bringing new challenges. Summary of the invention
[0005] In view of this, the present invention proposes a method for inhibiting the precipitation of needle-shaped platinum group metals during the glass solidification process of high-level radioactive waste liquid, so as to solve the problem that the existing method for improving the precipitation of precious metals during the glass solidification process of high-level radioactive waste liquid will reduce the chemical stability of the glass solidification body and form more difficult to melt precipitates.
[0006] The technical solution of the present invention is achieved in this way:
[0007] In a first aspect, the present invention provides a method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste, comprising the following steps:
[0008] S1, mixing glass raw materials, heating and melting them, and then crushing and grinding them to obtain basic glass, wherein the basic glass is in a granular form, and the particle size of the basic glass is 0.050-0.900 mm;
[0009] S2. The base glass is mixed with high-level radioactive waste liquid, heated and melted, and then cooled and annealed to obtain a glass solidification sample.
[0010] Specifically, the present invention controls the particle size and particle size distribution of the basic glass and the Na content in the high-energy glass solid body without changing the chemical composition of the glass solid body. 2 O and RuO 2 When the base glass particle size is larger than 1 mm, due to its small surface area and slow melting rate, a large amount of continuous glass liquid is formed late, which makes it easy for the base glass particles to form cavities with the waste, making RuO 2 The precipitate tends to grow along the cavity direction to form needle-shaped crystals. When the base glass particle size is less than 1 mm, its surface area is large and it is easy to melt at high temperature. The cavity between the base glass particles and the waste is reduced, making RuO 2 The precipitates are growth-restricted and form granules rather than needles.
[0011] More preferably, the basic glass particle size range is 0.075-0.800 mm; further preferably, the basic glass particle size range is 0.125-0.750 mm. The basic glass particle size range of 0.125-0.750 mm is the best implementation. The lower limit of 0.125 mm avoids the problem of excessive reaction and volatilization loss caused by too small particle size, and the upper limit of 0.750 mm avoids the problem of cavity caused by too large particle size and affecting the uniformity of reaction. At the same time, within the range of 0.125-0.750 mm, it is easier to form a continuous glass liquid phase between the glass particles and the waste, and this continuous glass phase helps to limit the RuO 2 Oriented growth of crystals, inhibiting the formation of needle-shaped crystals.
[0012] On the basis of the above technical solution, preferably, the standard deviation of the basic glass particle size distribution is less than 0.250 mm.
[0013] The number or mass of particles contained in different particle size ranges is called particle size distribution. Standard deviation is often used to describe the distribution of particle size. Standard deviation is used to measure the degree to which the particle size data set deviates from the average particle size. The smaller the standard deviation, the less the overall value deviates from the average value. Preferably, the standard deviation of the base glass particle size distribution is less than 0.180 mm. When the standard deviation is greater than 0.250 mm, the uniformity is poor, and more needle-shaped RuO is easily precipitated during high-temperature melting. 2 Crystal.
[0014] On the basis of the above technical solution, preferably, the basic glass chemical composition (in terms of oxide) includes SiO 2 , B 2 O 3 、Al 2 O 3 、CaO、Li 2 O and Na 2 Multiple types in O.
[0015] On the basis of the above technical solution, preferably, in terms of mass percentage, SiO 2 The content of B is 40wt% to 65wt%, 2 O 3 The content of Al is 13wt% to 25wt%, 2 O 3 The content of is 2wt% to 10wt%, the content of CaO is 3wt% to 15wt%, and the content of Li 2 The content of O is 0wt% to 5wt%, Na 2 The content of O is 6wt% to 17wt%.
[0016] In the present invention, SiO 2It is the main network former of glass, and its content determines the stability of glass structure; B 2 O 3 As a glass network former, Al can reduce the expansion coefficient of glass and improve the thermal and chemical stability of glass. 2 O 3 It can improve the acid resistance and temperature resistance of glass and enhance the chemical stability of glass; CaO, as an alkaline earth metal oxide, can improve the water resistance and chemical corrosion resistance of glass; Li 2 O and Na 2 O two alkali metal oxides are beneficial to improving the meltability and processability of glass.
[0017] On the basis of the above technical solution, preferably, the chemical composition of the high-level waste liquid (in terms of oxides) includes RuO 2 、Na 2 O, ZrO 2 、Nd 2 O 3 、MoO 3 、CeO 2 , Cs 2 O, BaO, Fe 2 O 3 ,La 2 O 3 , Pr 2 O 3 、Sm 2 O 3 , SrO, Y 2 O 3 Cr 2 O 3 , Rb 2 O, NiO, Gd 2 O 3 、Eu 2 O 3 and SnO 2 In a variety of.
[0018] On the basis of the above technical solution, preferably, in terms of mass percentage, RuO 2 The content of Na is 2wt% to 12wt%, 2 The content of O is 15wt% to 30wt%, ZrO 2 The content of MoO is 5wt% to 18wt%, the content of rare earth element oxide is 6wt% to 37wt%, 3 The content of is 6wt% to 13wt%, and the contents of other components are greater than 0.
[0019] On the basis of the above technical solution, preferably, the Na 2O and RuO 2 The mass ratio is 8:1-20:1.
[0020] Specifically, Na 2 O, as an alkaline oxide, can destroy the glass network structure and improve the solubility of the glass. 2 O can affect the viscosity and surface tension of the glass melt, thereby affecting the nucleation and growth dynamics of the crystal; RuO 2 As a platinum metal oxide, it is easy to precipitate and crystallize in high-level radioactive waste glass melt. 2 O / RuO 2 When the ratio is in the range of 8-20 and the base glass particle size is in the range of 0.125-0.750 mm, the fine base glass particle size provides more heterogeneous nucleation sites, and the appropriate Na 2 The O content regulates the melt properties. 2 The diffusion rate in the glass melt is adjusted to a moderate level, and then the synergistic effect of the two can promote RuO 2 It exists in the glass matrix in the form of fine and evenly dispersed particles.
[0021] On the basis of the above technical solution, preferably, in terms of mass percentage, SiO 2 The content is 38wt%~50wt%, B 2 O 3 The content of Al is 8wt% to 20wt%, 2 O 3 The content of is 2wt% to 6wt%, the content of CaO is 2wt% to 10wt%, and the content of Li 2 The content of O is 0wt% to 4wt%, Na 2 The content of O is 5wt% to 20wt%, RuO 2 The content of ZrO is 0.7wt%~2wt%, 2 The content of MoO is 1wt% to 5wt%, the content of rare earth element oxide is 1wt% to 7.5wt%, 3 The content of is 1wt% to 3wt%, and the contents of other components are greater than 0.
[0022] Based on the above technical solution, preferably, the rare earth element oxide can be Nd 2 O 3 、CeO 2 ,La 2 O 3 , Pr 2 O 3 、Sm 2 O 3 , Y 2 O3 , Gd 2 O 3 and Eu 2 One or more of O.
[0023] Based on the above technical solution, preferably, in steps S1 and S2, the temperature of heating and melting is 1100-1350° C., and in step S2, the temperature of annealing is 300-550° C. More preferably, in steps S1 and S2, the temperature of heating and melting is 1200-1300° C.
[0024] In a second aspect, the present invention provides a glass solidified body of high-level radioactive liquid waste, wherein the glass solidified body is prepared by any of the methods described above.
[0025] The method of suppressing the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste of the present invention has the following beneficial effects compared with the prior art:
[0026] (1) By adjusting the base glass particle size and Na 2 O / RuO 2 The mass ratio inhibits the formation of needle-shaped platinum metal precipitates, causing the platinum metals to exist in the glass matrix in the form of fine and evenly dispersed particles, thereby reducing the impact of the precipitates on the conductivity and viscosity of the glass melt, ensuring the safe operation of the glass solidification furnace;
[0027] (2) The method provided by the present invention does not add any chemical reagents to the base glass or high-level radioactive waste liquid, does not change the chemical composition and properties of the high-level radioactive glass solid body, and has wide applicability to high-level radioactive waste liquids with different chemical compositions. In addition, the operating process of the present invention is simple and easy to implement, and has good engineering application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a SEM image of the high-level radioactive liquid waste glass solidified body prepared in Example 1 of the present invention;
[0030] Figure 2 This is a SEM image of the high-level radioactive liquid waste glass solidified body prepared in Example 2 of the present invention;
[0031] Figure 3 This is a SEM image of the high-level radioactive liquid waste glass solidified body prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] This embodiment provides a method for inhibiting the precipitation of needle-shaped platinum metals during the vitrification process of high-level radioactive waste liquid, and prepares a simulated Ru-containing high-level radioactive waste vitrified body, the design composition of which is shown in Table 1, and the specific steps are as follows:
[0035] (1) Weigh borosilicate glass raw materials and mix them evenly, wherein SiO 2 , B 2 O 3 、Al 2 O 3 、ZrO 2 Introduced in the form of oxides, CaO, Na 2 O. Li 2 O is introduced as carbonate;
[0036] (2) placing 60 g of the mixed raw materials in a corundum crucible, heating and melting in a muffle furnace at 1200° C. for 1 h, then taking out the glass liquid and cooling it naturally on a copper plate, and then crushing it to obtain a borosilicate base glass with a particle size of 0.325±0.180 mm;
[0037] (3) The basic glass particles were mixed with Ru-containing simulated high-level waste according to the calculated ratio, 10 g of the mixture was placed in a corundum crucible and heated in a muffle furnace at 1200° C. for 1 h, and then the sample was taken out and placed in an annealing furnace at 400° C. for 2 h to finally obtain a Ru-containing simulated glass solidified body sample, wherein Na 2 O and RuO 2 The mass ratio is 9:1.
[0038] Table 1 Design composition of Ru-containing simulated high-radiation glass solidification body (wt%)
[0039]
[0040] Example 2
[0041] This embodiment provides a method for inhibiting the precipitation of needle-shaped platinum metals during the vitrification process of high-level radioactive waste liquid, and prepares a simulated Ru-containing high-level radioactive waste vitrified body, the design composition of which is shown in Table 2, and the specific steps are as follows:
[0042] (1) Weigh borosilicate glass raw materials and mix them evenly, wherein SiO 2 , B 2 O 3 、Al 2 O 3 、ZrO 2 Introduced in the form of oxides, CaO, Na 2 O. Li 2 O is introduced as carbonate;
[0043] (2) placing 60 g of the mixed raw materials in a corundum crucible, heating and melting in a muffle furnace at 1200° C. for 1 h, then taking out the glass liquid and cooling it naturally on a copper plate, and then crushing it to obtain a borosilicate base glass with a particle size of 0.325±0.180 mm;
[0044] (3) The basic glass particles were mixed with simulated Ru-containing high-level waste according to the calculated ratio, 10 g of the mixture was placed in a corundum crucible and heated in a muffle furnace at 1200° C. for 1 h, and then the sample was taken out and placed in an annealing furnace at 400° C. for 2 h to finally obtain a Ru-containing simulated glass solidified body sample, Na 2 O and RuO 2 The mass ratio is 19:1.
[0045] Table 2 Design composition of Ru-containing simulated high-radiation glass solidification body (wt%)
[0046]
[0047]
[0048] Example 3
[0049] This embodiment provides a method for inhibiting the precipitation of needle-shaped platinum metals during the vitrification process of high-level radioactive waste liquid, and prepares a simulated Ru-containing high-level radioactive waste vitrified body, the design composition of which is shown in Table 3, and the specific steps are as follows:
[0050] (1) Weigh borosilicate glass raw materials and mix them evenly, wherein SiO 2 , B 2 O 3 、Al 2 O 3 、ZrO 2 Introduced in the form of oxides, CaO, Na 2 O. Li 2 O is introduced as carbonate;
[0051] (2) placing 60 g of the mixed raw materials in a corundum crucible, heating and melting in a muffle furnace at 1300° C. for 0.8 h, then taking out the glass liquid and cooling it naturally on a copper plate, and then crushing and grinding to obtain a borosilicate base glass with a particle size of 0.050±0.230 mm;
[0052] (3) The basic glass particles were mixed with simulated Ru-containing high-level waste according to the calculated ratio, 10 g of the mixture was placed in a corundum crucible and heated in a muffle furnace at 1200° C. for 0.8 h, and then the sample was taken out and placed in an annealing furnace at 300° C. for 1.5 h to finally obtain a Ru-containing simulated glass solidified body sample, wherein Na 2 O and RuO 2 The mass ratio is 13:1.
[0053] Table 3 Design composition of Ru-containing simulated high-radiation glass solidification body (wt%)
[0054]
[0055]
[0056] Example 4
[0057] This embodiment provides a method for inhibiting the precipitation of needle-shaped platinum metals during the vitrification process of high-level radioactive waste to prepare a simulated Ru-containing high-level radioactive waste vitrified body, the design composition of which is shown in Table 4, and the specific steps are as follows:
[0058] (1) Weigh borosilicate glass raw materials and mix them evenly, wherein SiO 2 , B 2 O 3 、Al 2 O 3 、ZrO 2 Introduced in the form of oxides, CaO, Na 2 O. Li 2 O is introduced as carbonate;
[0059] (2) placing 60 g of the mixed raw materials in a corundum crucible, heating and melting in a muffle furnace at 1250° C. for 1.2 h, then taking out the glass liquid and cooling it naturally on a copper plate, and then crushing it to obtain a borosilicate base glass with a particle size of 0.72±0.180 mm;
[0060] (3) The basic glass particles were mixed with simulated Ru-containing high-level waste according to the calculated ratio, 10 g of the mixture was placed in a corundum crucible and heated in a muffle furnace at 1200° C. for 1.2 h, and then the sample was taken out and placed in an annealing furnace at 500° C. for 2.5 h to finally obtain a Ru-containing simulated glass solidified body sample, wherein Na 2 O and RuO 2The mass ratio is 19:1.
[0061] Table 4 Design composition of Ru-containing simulated high-radiation glass solidification body (wt%)
[0062]
[0063]
[0064] Comparative Example 1
[0065] This embodiment provides a method for inhibiting the precipitation of needle-shaped platinum group metals during the solidification of high-level radioactive liquid waste glass. The specific operation is the same as that of Example 2, except that: in step (1), the borosilicate base glass with a particle size of 0.325±0.30 mm is crushed.
[0066] Comparative Example 2
[0067] This embodiment provides a method for inhibiting the precipitation of needle-shaped platinum metals during the glass solidification process of high-level waste liquid. The specific operation is the same as that of Example 2, except that: Na 2 O and RuO 2 The mass ratio of 25:1 was used to prepare a glass solidified body of simulated Ru-containing high-level waste. The designed composition is shown in Table 5, namely
[0068] Table 5 Design composition of Ru-containing simulated high-radiation glass solidification body (wt%)
[0069]
[0070]
[0071] Comparative Example 3
[0072] This comparative example provides a method for inhibiting the precipitation of needle-shaped platinum group metals during the glass solidification process of high-level radioactive waste. The specific operating steps are the same as those of Example 1, except that: in step (1), the borosilicate base glass with a particle size of 1.2±0.180 mm is obtained by crushing.
[0073] Performance Testing
[0074] The resistivity (1150° C.) of the high-level radioactive liquid waste glass solidified bodies prepared in the examples and comparative examples was tested. The test results are shown in Table 6.
[0075] Table 6
[0076]
[0077]
[0078] Figure 1The SEM image of the Ru-containing simulated high-level waste glass solidified body prepared in Example 1 shows that when the base glass particle size is 0.325±0.180 mm, the RuO precipitated in the glass 2 , mainly in granular form.
[0079] Figure 2 The SEM image of the Ru-containing simulated high-level waste glass solidified body prepared in Example 2 shows that when the base glass particle size is 0.325±0.180 mm, the RuO precipitated in the glass 2 , mainly in granular form.
[0080] Figure 3 The SEM image of the Ru-containing simulated high-level waste glass solidified body prepared in Comparative Example 3 shows that when the base glass particle size is 1.2±0.180 mm, the RuO precipitated in the glass is 2 , mainly in needle shape.
[0081] As shown in Table 1, by comparing Examples 1-4, it can be seen that the technical solution of the present invention can better suppress the precipitation of needle-shaped platinum metals in the HFL glass solid body, thereby reducing the influence of platinum metal precipitates on the resistivity and viscosity of the HFL glass melt. By comparing Example 2 with Comparative Example 1, it can be seen that when the particle size standard deviation is greater than 0.25 mm, the uniformity is poor, and more needle-shaped RuO is easily precipitated during the high-temperature melting process. 2 Crystals, the resistivity of the glass melt is reduced by nearly 3 times. 2 O and RuO 2 When the mass ratio of is 8-20:1, it can better cooperate with the base glass particle size to inhibit the precipitation of needle-shaped platinum metals. Comparing Example 1 with Comparative Example 3, it can be seen that when the base glass particle size is greater than 1 mm, platinum metals are prone to form needle-shaped crystals and precipitate, reducing the resistivity of the glass melt by nearly 3 times.
[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive waste, characterized in that: The following steps are involved: S1. Mixing glass raw materials, heating and melting them, and then crushing them to obtain basic glass, wherein the basic glass is in a granular form and the particle size of the basic glass is 0.050-0.900 mm; S2. Mix 70-90 wt% of base glass and 10-30 wt% of high-level radioactive waste liquid (calculated as oxides), heat and melt, then cool and anneal to obtain a glass solidification sample.
2. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 1, characterized in that: The standard deviation of the base glass particle size distribution is less than 0.250 mm.
3. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 1, characterized in that: Calculated as oxides, basic glass chemistry includes various ones of SiO2, B2O3, Al2O3, CaO, Li2O and Na2O.
4. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 3, characterized in that: In terms of mass percentage, the content of SiO2 in the base glass is 40wt% to 65wt%, the content of B2O3 is 13wt% to 25wt%, the content of Al2O3 is 2wt% to 10wt%, the content of CaO is 3wt% to 15wt%, the content of Li2O is 0wt% to 5wt%, and the content of Na2O is 6wt% to 17wt%.
5. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 1, characterized in that: The chemical composition of the high-level radioactive waste (in terms of oxides) includes multiple elements selected from RuO2, Na2O, ZrO2, Nd2O3, MoO3, CeO2, Cs2O, BaO, Fe2O3, La2O3, Pr2O3, Sm2O3, SrO, Y2O3, Cr2O3, Rb2O, NiO, Gd2O3, Eu2O3 and SnO2.
6. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 5, characterized in that: Calculated by mass percentage, the content of RuO2 in the high-level radioactive waste is 2wt% to 12wt%, the content of Na2O is 15wt% to 30wt%, the content of ZrO2 is 5wt% to 18wt%, the content of rare earth element oxides is 6wt% to 37wt%, the content of MoO3 is 6wt% to 13wt%, and the contents of other components are all greater than 0.
7. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 1, characterized in that: The mass ratio of Na2O to RuO2 in the high-level radioactive liquid waste glass solidification body is 8:1-20:
1.
8. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 7, characterized in that: Calculated by mass percentage, the content of SiO2 in the high-level radioactive liquid waste glass solidification body is 38wt%~50wt%, the content of B2O3 is 8wt%~20wt%, the content of Al2O3 is 2wt%~6wt%, the content of CaO is 2wt%~10wt%, the content of Li2O is 0wt%~4wt%, the content of Na2O is 5wt%~20wt%, the content of RuO2 is 0.7wt%~2wt%, the content of ZrO2 is 1wt%~5wt%, the content of rare earth element oxide is 1wt%~7.5wt%, the content of MoO3 is 1wt%~3wt%, and the contents of other components are all greater than 0.
9. The method for inhibiting the precipitation of needle-shaped platinum group metals during the vitrification process of high-level radioactive liquid waste according to claim 1, characterized in that: In steps S1 and S2, the temperature of heating and melting is 1100-1350°C; in step S2, the temperature of annealing treatment is 300-550°C.
10. A high-level radioactive liquid waste glass solidification body, characterized in that: The glass solidified body is prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Waste leady CRT glass and high-level waste liquid coprocessing method
CN108417287A
Preparation method for high-sulfur, high-sodium and high-level-liquid-waste glass-ceramic solidifier
CN109273130A
High-sulfur and high-sodium waste liquid cured glass as well as preparation method and application thereof
CN115359943A
Method for preparing high-sulfur high-level liquid waste borosilicate glass solidified body
CN115806386A
Base glass for curing high-level liquid waste, preparation method and application thereof, and curing method of high-level liquid waste
CN117658460A
Cited By
Method for inhibiting crystallization of high-level waste glass solidified body
CN120117837A
Prediction method for leaching resistance of high-level borosilicate glass and application
CN120183543A
Method for restraining variable valence metal precipitation problem in power stack high-level liquid waste glass curing process and application
CN120261010A
A method and application for suppressing the precipitation of variable valence metals during vitrification of high-level radioactive waste in power reactors
CN120261010B
Method for controlling morphology of ruthenium oxide precipitate in high-level liquid waste glass curing process
CN121905602A