Fe3O4 coated porous carbon nanosphere as well as preparation method and application thereof

By using Fe3O4 to coat porous carbon nanospheres in zinc ion hybrid supercapacitors, the cyclic stability problem caused by the reduction of doping element content is solved, and the electrochemical window is expanded and the electrochemical performance is maintained, which is significantly improved. Improved capacity retention and electrochemical properties.

CN118942923APending Publication Date: 2024-11-12GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411261775.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

After long cycles of existing zinc ion hybrid supercapacitors, the decrease in doping element content leads to a decrease in cycling stability, and the common coating conductivity and electrochemical activity affect the electrochemical performance.

Method used

The porous carbon after ZIF-8 carbonization is used as the precursor, and hydrothermal reaction with ferric chloride in ethylene glycol solution is carried out to form a Fe3O4-covered core-shell structure, expanding the electrochemical window and maintaining electrochemical properties.

Benefits of technology

It achieves the maintenance of good cycle stability and electrochemical performance while expanding the electrochemical window, with a capacity retention rate of 82.5%, and is simple in process, low energy consumption and low pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942923A_ABST
    Figure CN118942923A_ABST
Patent Text Reader

Abstract

The invention discloses a Fe3O4 coated porous carbon nanosphere, which is a nanosphere formed by a Fe3O4 coated porous carbon structure, and Fe3O4 coated porous carbon is obtained by mixing ferric trichloride and porous carbon and then carrying out a hydrothermal reaction; the porous carbon is obtained by performing high-temperature calcination on ZIF-8; the ZIF-8 is obtained by chemical synthesis of zinc nitrate hexahydrate, 2-methylimidazole, methanol and ethanol. The ZIF-8 is of a regular dodecahedron structure, and the surface is smooth; the porous carbon is of a regular dodecahedron structure, and the surface is rough; the porous carbon nanospheres coated with Fe3O4 are of a core-shell nanosphere structure. The preparation method comprises the following steps: 1, preparing ZIF-8; 2, preparing porous carbon; and 3, preparation of the Fe3O4 coated porous carbon nanospheres. When the material is used as a supercapacitor electrode material, and the current density is 0.5 A g <-1 >, the charging and discharging voltage ranges are-1-0.5 V and 0-2.1 V; under the condition that the power density is 599.66 W kg <-1 >, the energy density is 24.12 Wh kg <-1 >; and under the condition that the current density is 10A g <-1 >, the cycle index is 10,000, and the capacity retention ratio is 82.5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of supercapacitors, and in particular to Fe3O4-coated porous carbon nanospheres and a preparation method and application thereof. Background Art

[0002] As a new type of energy storage device, zinc-ion hybrid supercapacitors combine the advantages of zinc-ion batteries and supercapacitors and have excellent energy density and power density. However, the decomposition voltage of water limits the operating voltage of the battery, thereby affecting the energy density and output, severely limiting the performance and life of zinc-ion hybrid supercapacitors and hindering their large-scale application.

[0003] In order to improve the energy density and cycle life of the capacitor, carbon materials with high conductivity, good chemical stability and large specific surface area can be used as the positive electrode material of zinc ion hybrid supercapacitors. For example, the existing document 1 (Coffee waste-derived porous carbon based flexible supercapacitors, Chemical Physics Letters, 2022, 809. DOI: 10.1016 / j.cplett.2022.140173) uses coffee grounds derived carbon as an electrode material. Under the condition of a current density of 5Ag-1, the number of cycles is 5000 times and the capacity retention rate is 90.5%. However, this technology has the problems of low voltage window and fast discharge time. The reason is that the biomass carbon material used in this technical solution has the structural characteristics of uneven structure and more surface defects, which leads to its poor electrochemical performance.

[0004] In order to expand the voltage window, the conductivity can be improved by doping non-metallic elements on the surface of the material. For example, the existing document 2 (2.6V aqueous symmetric supercapacitors based on phosphorus-doped TiO2 nanotube arrays, Dalton Transactions, 2020, 49 (6): 1785-1793. DOI: 10.1039 / c9dt04316k) uses a two-step combination method to prepare phosphorus-doped TiO2 nanotube arrays on Ti sheets, and realizes that the electrochemical window of the assembled aqueous symmetric supercapacitor can operate under an ultra-high voltage window of 2.6V. The basic principle of this technical solution is to achieve two technical effects at the same time by phosphorus doping: 1. Reducing the work function and band gap of TiO2; 2. Increasing the specific surface area of ​​the composite material, thereby increasing the conductivity of TiO2. Both of the above technical effects can improve the voltage window. However, this technical solution has the problem of poor cycle stability, specifically, only 63% of the initial capacitance is maintained after 10,000 cycles. The reason for the above problems is that during the cycle process, the surface doped phosphorus content is transferred by ions, resulting in reduced structural stability and a reduction in active sites.

[0005] In order to simultaneously expand the voltage window and improve the cycle stability, other materials can be coated on the surface of the material. For example, existing literature 3 (N-doped carbon-coated TiN exhibiting excellent electrochemical performance for supercapacitors, Electrochimica Acta, 2017, 257: 56-63. DOI: 10.1016 / j.electacta.2017.10.066) coated a layer of nitrogen-doped carbon on the outside of TiN nanoparticles to expand the voltage window to 1.6V, and at a current density of 1A g -1 Under the same conditions, the number of cycles is 5,000 and the capacity retention rate is 92%. However, this technology has the problems of fast discharge time, low energy density and power density. The reason is that while the nitrogen-doped carbon layer expands the voltage window of the electrode material, it also leads to uneven charge distribution and increased interface impedance due to its conductivity and electrochemical activity.

[0006] Therefore, based on the above-mentioned prior art solutions, it can be known that the prior art achieves the technical effect of expanding the voltage window by doping other elements on the surface of the material. However, this type of technical solution has the problem that after a long period of cycling, the content of the doped elements decreases due to ion transfer, resulting in reduced cycle stability. The current common solution is to improve the material surface by coating it again. Although this method can maintain cycle stability performance, it will produce new technical problems - the conductivity and electrochemical activity of the coating layer will directly affect the electrochemical properties of the electrode material. Summary of the invention

[0007] The purpose of the present invention is to provide a Fe3O4-coated porous carbon nanosphere and a preparation method and application thereof.

[0008] The present invention aims to solve the technical problems existing in the prior art by adopting the following methods:

[0009] 1. The porous carbon after carbonization of ZIF-8 is used as a precursor. The porous carbon has a uniform structure and a large specific surface area;

[0010] 2. Mix porous carbon with different masses of ferric chloride in ethylene glycol solution, then add a certain amount of anhydrous sodium citrate and anhydrous sodium acetate and stir. Finally, carry out hydrothermal reaction under certain conditions. Ferric chloride reacts with porous carbon to form Fe3O4-coated porous carbon nanospheres with a core-shell structure. This structure will not affect the electrochemical performance while expanding the electrochemical window of the material.

[0011] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:

[0012] A Fe3O4-coated porous carbon nanosphere, a nanosphere composed of a Fe3O4-coated porous carbon structure, wherein the Fe3O4-coated porous carbon is obtained by mixing ferric chloride and porous carbon and then subjecting the mixture to a hydrothermal reaction; the porous carbon is obtained by calcining ZIF-8 at a high temperature; the ZIF-8 is chemically synthesized from zinc nitrate hexahydrate, 2-methylimidazole, methanol and ethanol;

[0013] The microscopic morphology of the ZIF-8 is a regular dodecahedron structure with a smooth surface; the microscopic morphology of the porous carbon is a regular dodecahedron structure with a rough surface; the microscopic morphology of the Fe3O4-coated porous carbon nanospheres is a core-shell nanosphere structure.

[0014] A method for preparing Fe3O4-coated porous carbon nanospheres comprises the following steps:

[0015] Step 1, preparation of ZIF-8, first, weigh 2-methylimidazole and dissolve it in a mixed solvent to obtain a solution A, and at the same time, weigh zinc nitrate solid and dissolve it in a mixed solvent to obtain a solution B, then, at room temperature and under ultrasonic conditions, slowly pour the solution A into the solution B to obtain a solution C, then stir and mix, let stand, and finally, centrifuge and wash the obtained product and vacuum dry it to obtain ZIF-8 with a regular dodecahedral structure;

[0016] In the step 1, the mass ratio of 2-methylimidazole to zinc nitrate is (1-2):1; the mixed solvent is a mixed solution of methanol and ethanol, and the volume ratio of methanol to ethanol is 1:1;

[0017] In step 1, the centrifugal washing conditions are: the centrifugal speed is 8000 rpm, the centrifugal time is 5 min, the washing liquid is ethanol, and the number of centrifugal washings is 4-6 times;

[0018] In step 1, the vacuum drying conditions are as follows: the drying temperature is 60-80° C. and the drying time is 6-10 h;

[0019] Step 2, preparation of porous carbon, calcining the ZIF-8 obtained in step 1 under certain conditions to achieve carbonization, and grinding the obtained black product to obtain porous carbon with a regular dodecahedral structure;

[0020] In step 2, the calcination conditions are: the calcination temperature is 950° C. and the calcination time is 1-2 h;

[0021] Step 3, preparation of Fe3O4-coated porous carbon nanospheres, first, placing the porous carbon obtained in step 2, ferric chloride and anhydrous sodium citrate in an ethylene glycol solution to obtain a D solution, then stirring the D solution under certain conditions to obtain an E solution, then placing anhydrous sodium acetate in the E solution to obtain an F solution, then continuing to stir the F solution under certain conditions to obtain a reaction solution, finally, subjecting the reaction solution to a hydrothermal reaction under certain conditions, washing and drying the obtained product, and obtaining Fe3O4-coated porous carbon nanospheres;

[0022] In the step 3, the mass ratio of porous carbon, ferric chloride, anhydrous sodium citrate and anhydrous sodium acetate is 1:10:(3-4):20;

[0023] In step 3, the hydrothermal condition is 200° C. for 15-17 h;

[0024] In step 3, the drying conditions are as follows: the drying temperature is 60-80° C. and the drying time is 10-14 hours.

[0025] A Fe3O4-coated porous carbon nanosphere, when used as a supercapacitor electrode material, in a 6M potassium hydroxide electrolyte, when the current density is 0.5A g -1 When the charge and discharge voltage ranges from -1 to 0.5 V, in a 2M zinc sulfate electrolyte, when the current density is 0.5 A g -1 When the charge and discharge voltage ranges from 0 to 2.1 V, the power density is 599.66 W kg -1 Under these conditions, the energy density is 24.12Wh kg -1 ;

[0026] At a current density of 10A g -1 Under the same conditions, the number of cycles was 10,000 and the capacity retention rate was 82.5%.

[0027] The beneficial technical effects obtained by the present invention are known through testing:

[0028] XRD and EDS tests have shown that Fe-O / C is composed of three elements: Fe, C, and O, specifically including carbon and Fe3O4.

[0029] SEM and TEM tests have shown that the porous carbon obtained has a regular dodecahedral structure, a rough surface and a particle size of 60nm; after coating, Fe-O / C has a core-shell spherical structure, with Fe3O4 as a shell structure and C as a core structure.

[0030] The BET test showed that the specific surface area of ​​the porous carbon was 165-170 m 2 / g, and contains a large number of micropores and mesopores; the specific surface area of ​​Fe-O / C is 23-24m 2 / g, that is, Fe3O4 covers the micropores and mesopores of porous carbon, which proves that Fe3O4 is successfully coated on the surface of carbon material.

[0031] CV tests have shown that Fe-O / C exhibits both double-layer capacitance and pseudocapacitance behavior.

[0032] GCD tests have shown that Fe3O4 provides additional pseudocapacitance, expands the voltage window, and has good cycle stability.

[0033] Therefore, the present invention has the following advantages over the prior art:

[0034] 1. Porous carbon has the advantages of uniform structure and large specific surface area, which provides uniformity and dispersion for the load;

[0035] 2. The core-shell structure plays a supporting role, directly achieving the technical effect of improving cycle stability;

[0036] 3. Fe3O4, as a dielectric layer, polarizes under an external electric field to achieve the technical effect of storing electrical energy. At the same time, the electrochemical performance is not affected under the condition of expanding the electrochemical window;

[0037] 4. The synthesis process of the present invention is simple, the reaction cycle is short, and the reaction process is low in energy consumption and pollution.

[0038] Therefore, the present invention has better electrochemical performance than the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is the XRD pattern of ZIF-8 and C-8 in Example 1;

[0040] Figure 2 XRD diagrams of Fe-O / C-1 in Example 1, Ti-O / C in Comparative Example 1, and Fe-O / C-3 in Comparative Example 3;

[0041] Figure 3 XRD diagrams of ZIF-67 and Co-C in Comparative Example 2;

[0042] Figure 4 It is the SEM picture of ZIF-8 and C-8 in Example 1;

[0043] Figure 5 is the EDS diagram of Fe-O / C-1 in Example 1;

[0044] Figure 6 TEM image of Fe-O / C-1 in Example 1;

[0045] Figure 7 It is the BET diagram of Fe-O / C-1 and C-8 in Example 1;

[0046] Figure 8 GCD diagrams of Fe-O / C-1 and C-8 in Example 1, Ti-O / C in Comparative Example 1, Co-C in Comparative Example 2, and Fe-O / C-3 in Comparative Example 3;

[0047] Fig. 9 is the CV diagram of Fe-O / C-1 in Example 1;

[0048] Fig.10 It is the GCD diagram of Fe-O / C-1 and C-8 in Example 1 and Fe-O / C-3 in Comparative Example 3;

[0049] Fig.11 This is the cyclic stability performance diagram of Fe-O / C-1 in Example 1. DETAILED DESCRIPTION

[0050] The present invention is further described in detail through embodiments and in conjunction with the accompanying drawings, but the present invention is not limited thereto.

[0051] Example 1

[0052] A method for preparing Fe3O4-coated porous carbon nanospheres comprises the following steps:

[0053] Step 1, preparation of ZIF-8, first, weigh 6.92g of 2-methylimidazole and dissolve it in 480mL of mixed solvent to obtain solution A, and at the same time, weigh 6.27g of zinc nitrate solid and dissolve it in 480mL of mixed solvent to obtain solution B, then, at room temperature and under ultrasonic conditions, slowly pour solution A into solution B to obtain solution C, then, stir solution C for 10min, after stirring, let it stand for 24h, finally, centrifuge and wash the obtained product and vacuum dry it to obtain ZIF-8 with a regular dodecahedral structure;

[0054] In the step 1, the mixed solvent is a mixed solution of methanol and ethanol, and the volume ratio of methanol to ethanol is 1:1;

[0055] In step 1, the centrifugal washing conditions are: the centrifugal speed is 8000 rpm, the centrifugal time is 5 min, the washing liquid is ethanol, and the number of centrifugal washings is 4 times;

[0056] In step 1, the vacuum drying conditions are as follows: the drying temperature is 60° C. and the drying time is 8 h.

[0057] In order to prove the composition of ZIF-8 obtained in step 1, XRD test was performed. The test results are as follows Figure 1 As shown, the diffraction peak of the product prepared in step 1 is consistent with the characteristic peak of standard ZIF-8. The test results show that step 1 successfully prepares ZIF-8.

[0058] In order to verify the microstructure of ZIF-8, SEM test was performed. Figure 4 As shown, the ZIF-8 obtained in step 1 has a regular dodecahedral structure, a smooth surface and a particle size of 80 nm.

[0059] Step 2, preparation of porous carbon, calcining the ZIF-8 obtained in step 1 at a calcination temperature of 950° C. for 2 h to achieve carbonization, and grinding the obtained black product to obtain porous carbon with a regular dodecahedral structure, named C-8;

[0060] In order to verify the composition of the porous carbon obtained in step 2, an XRD test was performed. The test results are shown in Figure 1As shown, the diffraction peak of C-8 only has the characteristic peak of carbon, and does not have the characteristic peak of ZIF-8, that is, the original characteristic peak of ZIF-8 disappears. The test results show that step 2 achieves the carbonization of ZIF-8, that is, step 2 successfully prepares porous carbon.

[0061] In order to verify the microstructure of porous carbon, SEM test was performed. The test results are shown in Figure 4 As shown, the C-8 obtained in step 2 has a regular dodecahedral structure, a rough surface, and a particle size of 60nm. The test results are compared with those in step 1. It can be seen that the calcination and carbonization in step 2 changes the surface of the porous carbon from the smooth ZIF-8 to rough, and the calcination reduces the particle size. The reason is that during the calcination process, the volatilization of the Zn element causes the surface to become rough, and due to the volatilization of the central metal element Zn, the skeleton formed by the ligand shrinks inward, resulting in a reduction in particle size.

[0062] In order to further confirm the microscopic morphology of porous carbon, BET test was performed. The test results are shown in Figure 7 As shown, the specific surface area of ​​C-8 is 168.212 m 2 / g; It can be seen from the isotherm that the porous carbon contains a large number of micropores and mesopores.

[0063] The electrochemical tests were conducted using a three-electrode system and a two-electrode system.

[0064] In the three-electrode system, the material to be tested is used as the working electrode, the mercury oxide electrode is used as the reference electrode, the platinum electrode is used as the counter electrode, and the 6M KOH solution is used as the electrolyte. The specific preparation method of the working electrode is as follows: the mass ratio of the material to be tested, acetylene black and polytetrafluoroethylene powder is 8:1:1, 0.008g of the material to be tested, 0.001g of acetylene black, 0.001g of polytetrafluoroethylene powder and an appropriate amount of ethanol are weighed and mixed and ground; after grinding, it is dried under an infrared lamp to obtain a dry sample; finally, the dry sample is placed on a 2cm×4cm nickel foam current collector, the nickel foam is folded in half, and the nickel foam is pressed at a pressure of 5kPa to obtain a supercapacitor electrode, i.e., a working electrode.

[0065] In the dual-electrode system, the specific preparation method of the positive electrode is: the mass ratio of activated carbon, acetylene black and polytetrafluoroethylene powder is 8:1:1, 0.008g activated carbon, 0.001g acetylene black, 0.001g polytetrafluoroethylene powder and an appropriate amount of ethanol are weighed and mixed and ground; after grinding, it is dried under an infrared lamp to obtain a dry sample; finally, the dry sample is placed on a 2cm×4cm nickel foam current collector, the nickel foam is folded in half, and the nickel foam is pressed at a pressure of 5kPa to obtain the positive electrode. The negative electrode is the material to be tested. The preparation method is the same as the working electrode preparation method in the three-electrode system, and 2M ZnSO4 solution is used as the electrolyte.

[0066] In order to demonstrate the electrochemical performance of C-8, a constant current charge-discharge GCD test was performed. The test results are shown in Figure 8 As shown, at a current density of 0.5A g -1 When the charge and discharge voltage range is -1-0V, the discharge time is 360s;

[0067] In order to further quantify the electrochemical performance of C-8, electrochemical tests were performed in a two-electrode system. Fig.10 As shown, at a current density of 0.5A g -1 When the charge and discharge voltage ranges from 0 to 1.7 V, the discharge time is 102 s, that is, the power density is 425 W kg -1 Under these conditions, the energy density is 12.32Wh kg -1 .

[0068] Step 3, preparation of Fe3O4-coated porous carbon nanospheres, first, 0.06g of the porous carbon obtained in step 2, 0.6g of ferric chloride and 0.2g of anhydrous sodium citrate are placed in 20mL of ethylene glycol solution to obtain a D solution, then, the D solution is stirred for a stirring time of 1h to obtain an E solution, then, 1.2g of anhydrous sodium acetate is placed in the E solution to obtain a F solution, then, the F solution is continued to be stirred for a stirring time of 1h to obtain a reaction solution, finally, the reaction solution is subjected to a hydrothermal reaction at a hydrothermal temperature of 200°C and a hydrothermal time of 16h, and the obtained product is washed and dried to obtain Fe3O4-coated porous carbon nanospheres with a core-shell structure, referred to as Fe-O / C, and the Fe-O / C obtained in specific example 1 is named Fe-O / C-1;

[0069] In step 3, the drying conditions are as follows: the drying temperature is 60° C. and the drying time is 12 h.

[0070] In order to verify the composition and element distribution of Fe-O / C-1, EDS test was performed. The test results are as follows Figure 5 As shown, Fe-O / C-1 contains not only C element, but also Fe element and O element.

[0071] In order to further prove the composition of Fe-O / C-1 obtained in step 3, XRD test was performed. The test results are as follows Figure 2 As shown, Fe-O / C-1 has characteristic peaks of Fe3O4 in addition to carbon. The test results show that step 3 successfully prepared Fe3O4.

[0072] The combination of EDS test and XRD test can prove that Fe3O4 is successfully prepared on the porous carbon surface through step 3.

[0073] In order to verify the microstructure of Fe-O / C-1, TEM test was carried out. The test results are shown in Figure 6 As shown, Fe-O / C-1 presents a core-shell spherical structure, Fe3O4 is a shell structure, and C is a core structure.

[0074] In order to further confirm the microstructure of Fe-O / C-1, BET test was performed. The test results are as follows Figure 7 As shown, the specific surface area of ​​Fe-O / C-1 is 23.228m 2 / g; From the shape of the isotherm, it can be judged that Fe-O / C-1 contains fewer micropores and mesopores. Compared with step 2, it can be seen that coating Fe3O4 in step 3 reduces the specific surface area. This phenomenon shows that Fe3O4 covers micropores and mesopores, thereby reducing adsorption sites, which proves that Fe3O4 is successfully coated on the surface of carbon materials.

[0075] In order to prove the electrochemical performance of Fe-O / C-1, GCD test was carried out. The test results are shown in Figure 8 As shown, at a current density of 0.5A g -1 When the charge and discharge voltage ranges from -1 to 0.5 V, the discharge time is 327 s. Compared with the porous carbon obtained in step 2, although the Fe3O4 coating slightly reduces the discharge time, the charge and discharge voltage range is significantly increased by 0.5 V. The test results show that the voltage window can be significantly expanded by coating Fe3O4 to form a core-shell nanosphere structure.

[0076] In order to prove the electrochemical behavior of Fe-O / C-1, CV test was carried out. The test results are shown in Fig. 9 As shown, at a scan rate of 50 mv s -1 Under the same conditions, when the voltage window is in the range of -1-0 V, the CV curve is rectangular; when the voltage window is 0-0.5 V, the CV curve shows an obvious redox peak, which corresponds to Fe 3+ and Fe 2+ The test results show that Fe-O / C-1 exhibits double-layer capacitance behavior in the -1-0V voltage window range and pseudocapacitance behavior in the 0-0.5V voltage window range. The test results show that the Fe3O4 prepared in step 3 provides additional pseudocapacitance.

[0077] In order to further quantify the electrochemical performance of Fe-O / C-1, electrochemical tests were performed in a two-electrode system. Fig.10 As shown, at a current density of 0.5A g -1 When the charge and discharge voltage is in the range of 0-2.1V, the discharge time of the double electrodes is 150s, that is, when the power density is 599.66W kg -1Under these conditions, the energy density is 24.12Wh kg -1 .

[0078] In order to prove the cycling stability of Fe-O / C-1, cycling tests were carried out in a dual-electrode system. Fig.11 As shown, at a current density of 10A g -1 Under the same conditions, the number of cycles was 10,000 and the capacity retention rate was 82.5%.

[0079] In order to demonstrate the effect of Fe3O4 on the performance of coated porous carbon nanospheres, specifically the effect of Fe element, comparative example 1 is provided, which is based on TiO2 coated porous carbon nanospheres.

[0080] Comparative Example 1

[0081] A preparation method for TiO2-coated porous carbon nanospheres, wherein the steps not specifically described are the same as those in Example 1, except that in step 3, titanium sulfate is used instead of ferric chloride to obtain TiO2-coated porous carbon nanospheres, which are named Ti-O / C.

[0082] In order to prove the composition of the obtained Ti-O / C, XRD test was carried out. The test results are as follows Figure 2 As shown, in addition to the characteristic peaks of carbon, Ti-O / C also has characteristic peaks of TiO2. The test results show that the TiO2-coated porous carbon material was successfully prepared.

[0083] In order to prove the electrochemical performance of Ti-O / C, GCD test was carried out. The test results are shown in Figure 8 As shown, at a current density of 0.5A g -1 The charge and discharge voltage range is -1-0.3V, and the discharge time is 320s.

[0084] Compared with the porous carbon obtained in step 2 of Example 1, it can be seen that the effects of coating TiO2 and coating Fe3O4 are similar, that is, the discharge time is slightly reduced. However, the effect of coating TiO2 on increasing the charge and discharge voltage range is only 0.3V.

[0085] Further comparison with the Fe-O / C-1 obtained in step 3 of Example 1 shows that there is no significant difference in discharge time, but the charge and discharge voltage range of Fe-O / C-1 is 0.2 V higher than that of Ti-O / C.

[0086] The test results show that although coating with metal oxides will reduce the discharge time, it can increase the charge and discharge voltage range; and the effect of coating with Fe3O4 on improving the charge and discharge voltage range is much greater than that of coating with TiO2. That is to say, although both are fourth-period transition metal elements, there are significant differences in the effects of Fe and Ti on the charge and discharge voltage range.

[0087] In order to demonstrate the influence of the matrix on the performance, that is, the role of ZIF-8 in the technical solution, Comparative Example 2 is provided, which is based on carbonized porous carbon of ZIF-67.

[0088] Comparative Example 2

[0089] A preparation method of carbonized porous carbon based on ZIF-67, wherein the steps not otherwise specified are the same as those in Example 1, except that: in step 1, cobalt nitrate is used instead of zinc nitrate to obtain ZIF-67, and at the same time, the porous carbon obtained in step 2 is cobalt-doped porous carbon, named Co-C.

[0090] In order to prove the composition of the obtained ZIF-67, XRD test was performed. The test results are shown in Figure 3 As shown, the diffraction peaks of the prepared product are consistent with the characteristic peaks of standard ZIF-67. The test results show that ZIF-67 is successfully prepared.

[0091] In order to prove the composition of the obtained Co-C, XRD test was carried out. The test results are as follows Figure 3 As shown in the figure, the diffraction peak of Co-C has not only the characteristic peak of carbon, but also the characteristic peak of Co metal element. At the same time, there is no characteristic peak of ZIF-67, that is, the original characteristic peak of ZIF-67 disappears. The test results show that the carbonization of ZIF-67 is successful in preparing porous carbon.

[0092] Further comparison with the porous carbon obtained in step 2 of Example 1 shows that since the Zn element in ZIF-8 is volatile, the Zn element also volatilizes during the high-temperature carbonization of ZIF-8, that is, there is no metal element in the porous carbon after high-temperature carbonization, while the Co element in ZIF-67 is not volatile. Therefore, during the high-temperature carbonization of ZIF-67, the Co element cannot volatilize, that is, the Co element is still retained in the porous carbon after high-temperature carbonization to form a cobalt-carbon composite material.

[0093] In order to demonstrate the electrochemical performance of Co-C, GCD test was performed. The test results are shown in Figure 8 As shown, at a current density of 0.5A g -1 When the charge and discharge voltage ranges from -1 to 0 V, the discharge time is 15 s. Comparison of the porous carbon obtained in step 2 of Example 1 shows that the charge and discharge voltage ranges are the same, but the discharge time has significant differences.

[0094] Combining the XRD test results and GCD test results, it can be seen that during the high-temperature calcination process of ZIF-8, porous carbon is formed due to the volatilization of the central metal element Zn, while the central metal element of ZIF-67 is Co, which cannot volatilize at high temperatures and can only form Co-C. In addition, the pore structure of Co-C is much lower than that of porous carbon, which makes it impossible to effectively improve the rapid migration of electrolyte ions, thereby improving the charge and discharge rate and cycle stability.

[0095] In order to demonstrate the effect of Fe3O4 coating amount on performance, comparative example 3 is provided, in which the Fe3O4 coating amount is 10:3 for coating porous carbon nanospheres.

[0096] Comparative Example 3

[0097] A method for preparing porous carbon nanospheres coated with Fe3O4 in a coating amount of 10:3, wherein the steps not otherwise specified are the same as those in Example 1, except that in step 3, the mass ratio of ferric chloride to porous carbon is 10:3, and the Fe-O / C obtained in specific comparative example 3 is named Fe-O / C-3.

[0098] In order to prove the composition of Fe-O / C-3, XRD test was carried out. The test results are as follows Figure 2 As shown, Fe-O / C-3 has characteristic peaks of Fe3O4 in addition to the characteristic peaks of carbon. Comparing the test results with those of Example 1, it can be seen that increasing the amount of porous carbon added has no substantial effect on the composition of Fe-O / C-3.

[0099] In order to prove the electrochemical performance of Fe-O / C-3, GCD test was carried out. The test results are shown in Figure 8 As shown, at a current density of 0.5A g -1 When the charge and discharge voltage ranges from -1 to 0.3 V, the discharge time is 430 s. The test results are compared with those of Example 1, and it can be seen that although the discharge time is increased from 327 s to 430 s, the charge and discharge voltage range is reduced by 0.2 V.

[0100] In order to further quantify the electrochemical performance of Fe-O / C-3, electrochemical tests were carried out in a two-electrode system. Fig.10 As shown, at a current density of 0.5Ag -1 When the charge and discharge voltage ranges from 0 to 1.9 V, the discharge time is 178 s; that is, the power density is 475 W kg -1 Under these conditions, the energy density is 23.41Wh kg -1 .

[0101] The test results are compared with the Fe-O / C-1 in Example 1. It can be seen that although the discharge time is slightly reduced, the charge and discharge voltage range is expanded by 0.2V, and the improvement of the discharge voltage range is far better than the reduction of the discharge time. Therefore, the power density and energy density of Fe-O / C-1 are improved. The reason for obtaining this technical effect is that the introduction of excessive carbon material will lead to uneven Fe3O4 coating.

Claims

1. A kind of Fe 3 O 4 Coated with porous carbon nanospheres, Features: ByFe 3 O 4 Nanospheres composed of porous carbon structures, wherein the Fe 3 O 4 The coated porous carbon is obtained by mixing ferric chloride and porous carbon and then subjecting them to a hydrothermal reaction; the porous carbon is obtained by calcining ZIF-8 at a high temperature; and the ZIF-8 is obtained by chemical synthesis of zinc nitrate hexahydrate, 2-methylimidazole, methanol and ethanol.

2. Fe according to claim 1 3 O 4 Coated with porous carbon nanospheres, Features: The microstructure of the ZIF-8 is a regular dodecahedron structure with a smooth surface; the microstructure of the porous carbon is a regular dodecahedron structure with a rough surface; the Fe 3 O 4 The microscopic morphology of the coated porous carbon nanospheres is a core-shell nanosphere structure.

3. A kind of Fe 3 O 4 Preparation method of coated porous carbon nanospheres, Features The following steps are involved: Step 1, preparation of ZIF-8, first, weigh 2-methylimidazole and dissolve it in a mixed solvent to obtain a solution A, and at the same time, weigh zinc nitrate solid and dissolve it in a mixed solvent to obtain a solution B, then, at room temperature and under ultrasonic conditions, slowly pour the solution A into the solution B to obtain a solution C, then stir and mix, let stand, and finally, centrifuge and wash the obtained product and vacuum dry it to obtain ZIF-8 with a regular dodecahedral structure; Step 2, preparation of porous carbon, calcining the ZIF-8 obtained in step 1 under certain conditions to achieve carbonization, and grinding the obtained black product to obtain porous carbon with a regular dodecahedral structure; Step 3, Fe 3 O 4 Preparation of coated porous carbon nanospheres: first, the porous carbon obtained in step 2, ferric chloride and anhydrous sodium citrate are placed in an ethylene glycol solution to obtain a D solution, then the D solution is stirred under certain conditions to obtain an E solution, then anhydrous sodium acetate is placed in the E solution to obtain an F solution, then the F solution is continued to be stirred under certain conditions to obtain a reaction solution, and finally, the reaction solution is subjected to a hydrothermal reaction under certain conditions, and the obtained product is washed and dried to obtain Fe 3 O 4 Coated porous carbon nanospheres.

4. The preparation method according to claim 3, Features: In the step 1, the mass ratio of 2-methylimidazole to zinc nitrate is (1-2):1; the mixed solvent is a mixed solution of methanol and ethanol, and the volume ratio of methanol to ethanol is 1:1; In step 1, the centrifugal washing conditions are: the centrifugal speed is 8000 rpm, the centrifugal time is 5 min, the washing liquid is ethanol, and the number of centrifugal washings is 4-6 times; In step 1, the vacuum drying conditions are as follows: the drying temperature is 60-80° C. and the drying time is 6-10 h.

5. The preparation method according to claim 3, Features: In the step 2, the calcination conditions are: the calcination temperature is 950° C. and the calcination time is 1-2 hours.

6. The preparation method according to claim 3, Features: In the step 3, the mass ratio of porous carbon, ferric chloride, anhydrous sodium citrate and anhydrous sodium acetate is 1:10:(3-4):20; In step 3, the hydrothermal condition is 200° C. for 15-17 h; In step 3, the drying conditions are as follows: the drying temperature is 60-80° C. and the drying time is 10-14 hours.

7. A kind of Fe 3 O 4 Coated with porous carbon nanospheres, Features: When used as a supercapacitor electrode material, in a 6M potassium hydroxide electrolyte, when the current density is 0.5Ag -1 When the charge and discharge voltage ranges from -1 to 0.5V; In 2M zinc sulfate electrolyte, when the current density is 0.5Ag -1 When charging and discharging, the range of voltage is 0-2.1V; At a power density of 580-600W kg -1 Under these conditions, the energy density is 23-25Wh kg -1 .

8. A kind of Fe 3 O 4 Coated with porous carbon nanospheres, Features: When used as a supercapacitor electrode material, the current density is 10A. -1 Under the same conditions, the number of cycles was 10,000 and the capacity retention rate was 82.5%.

Citation Information

Cited By

  • Carbon aerogel loaded iron carbon nanospheres as well as preparation method and application thereof

    CN119811904A