Supported PtFe diatomic catalyst as well as preparation method and application thereof
By using ALD technology to deposit Pt single atoms on FeNC/AC support, the problems of slow deposition rate and difficult control in the preparation of PtFe bimetallic catalysts are solved, and efficient catalysts with low Pt loading are achieved, which significantly improves the catalysis of hydrogen fuel cells Performance and reduce production costs.
Patent Information
- Application Number
- CN202411012827.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-26
AI Technical Summary
In the prior art, the Pt deposition rate during the preparation of PtFe bimetallic catalyst is slow, and the stable PtFe diatomic catalyst cannot be accurately controlled, which limits the catalytic efficiency and cost-effectiveness of hydrogen fuel cells.
After mixing FeNC with ammonium chloride, atomic layer deposition (ALD) method is used to uniformly deposit low-load Pt single atoms on the surface of FeNC/AC support, and a loaded low-PtFe diatom catalyst is prepared to achieve PtFe biatomic Accurate and controllable synthesis of atomic morphology.
The catalytic efficiency of the catalyst in the hydrogen oxidation reaction of the anode of the fuel cell is significantly improved, the Pt loading and production cost are reduced, and a high activity, high stability and low cost catalyst system is provided.
Smart Images

Figure CN118943396A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cell electrocatalysis, and in particular to a method for preparing a supported PtFe diatomic catalyst and application of the supported PtFe diatomic catalyst in anode hydrogen oxidation of a fuel cell. Background Art
[0002] Hydrogen fuel cells (PEMFCs) are energy conversion devices that convert hydrogen energy directly into electrical energy. Compared with thermal power generation and heat engine power generation, they are clean, efficient, low-carbon and environmentally friendly. They are a major strategic direction for the world's energy and power transformation. Electrode catalysts are used to reduce the reaction activation energy barrier and increase the reaction rate, and are considered to be the key core materials of PEMFCs. The most effective catalyst for PEMFC is mainly platinum-carbon (Pt / C), but the high cost of precious metal Pt, limited reserves, aggregation deactivation and poor stability under battery operating conditions have seriously restricted the commercialization process of PEMFC. Therefore, the development of new catalysts with high activity, low Pt loading and high stability is of great significance to breaking through the main bottlenecks of PEMFC.
[0003] The prior art discloses a hybrid electrocatalyst composed of atomically dispersed Pt single atoms and Fe single atoms and Pt-Fe alloy nanoparticles, wherein Pt acetylacetonate is dispersed in a solvent, a nitrogen source and Fe-doped ZIF-8 are added to prepare a suspension, and after drying, Fe-ZIF-8 with Pt and N source distributed therein is obtained by ball milling, and finally high-temperature treatment is performed to remove Zn to obtain a Pt-Fe-NC catalyst, wherein the Pt loading is 1.7%. However, the Pt deposition rate is slow during the preparation process, and it is impossible to synthesize precisely controlled PtFe nanoparticles and clusters, and it is impossible to precisely control a stable PtFe diatomic catalyst. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of slow Pt deposition rate and inability to accurately control stable PtFe diatoms in the preparation process of PtFe bimetallic catalysts in the prior art, thereby providing a supported PtFe diatomic catalyst for hydrogen fuel cell applications and a preparation method thereof. The supported low Pt diatomic catalyst PtFeNC / AC is prepared by pyrolyzing a mixture of FeNC and ammonium chloride and then using an atomic layer deposition (ALD) method to uniformly deposit low-loaded Pt single atoms on the FeNC / AC surface. The deposition of Pt single atoms can be controlled at the atomic scale, which is conducive to the precise and controllable synthesis of PtFe diatomic catalysts. The catalytic efficiency of the catalyst in hydrogen oxidation at the anode of the fuel cell can be significantly improved while greatly reducing the Pt loading, while effectively reducing the production and preparation costs.
[0005] In order to solve the above technical problems, the present invention is implemented through the following technical solutions.
[0006] The first aspect of the present invention provides a method for preparing a supported PtFe diatomic catalyst, comprising the following steps:
[0007] (1) dissolving zinc salt and iron salt in an organic solvent and mixing them evenly, adding 2-methylimidazole solution, and stirring them together at room temperature for reaction; then centrifuging, washing, and drying to obtain Fe-ZIF-8;
[0008] (2) Fe-ZIF-8 is carbonized at high temperature under an inert gas atmosphere to obtain Fe-NC containing single Fe atoms;
[0009] (3) Fe-NC and NH4Cl are mixed and pyrolyzed at high temperature under an inert gas atmosphere to obtain a Fe-NC / AC carrier with a mesoporous structure;
[0010] (4) ALD was used to deposit single Pt atoms on the surface of the Fe-NC / AC support.
[0011] Preferably, the zinc salt in step (1) is selected from one or more of zinc chloride, zinc bromide, zinc nitrate, zinc sulfate, zinc acetate, and hydrates thereof.
[0012] Preferably, the iron salt in step (1) is selected from one or more of ferric chloride, ferric bromide, ferric nitrate, ferric sulfate and ferric acetate.
[0013] Preferably, the mass ratio of the zinc salt to the iron salt in step (1) is 10-30:1; more preferably, the mass ratio of the zinc salt to the iron salt is 20-25:1.
[0014] Preferably, in step (1), the mass ratio of the zinc salt to the 2-methylimidazole in the 2-methylimidazole solution is 0.5-1:1; more preferably, the mass ratio of the zinc salt to the 2-methylimidazole in the 2-methylimidazole solution is 0.7-0.9:1.
[0015] Preferably, the organic solvent in step (1) is selected from one or more of methanol, ethanol, isopropanol, acetone, chloroform and tetrahydrofuran.
[0016] Preferably, the solvent of the 2-methylimidazole solution in step (1) is selected from one or more of methanol, ethanol, isopropanol, acetone, chloroform and tetrahydrofuran.
[0017] Preferably, the stirring reaction time in step (1) is 12-48 h; more preferably, the stirring reaction time is 18-30 h.
[0018] Preferably, the drying in step (1) is vacuum drying.
[0019] Preferably, the high temperature carbonization in step (2) is carried out at a temperature of 800-1200° C. for a time of 1-5 h; more preferably, the high temperature carbonization is carried out at a temperature of 900-1100° C. for a time of 1.5-3 h.
[0020] Preferably, the inert gas in step (2) is selected from one or more of nitrogen, helium, argon, etc.
[0021] Preferably, in step (3), the mass ratio of Fe-NC to NH4Cl is 1:2-5; more preferably, the mass ratio of Fe-NC to NH4Cl is 1:2.5-4.
[0022] Preferably, the high temperature pyrolysis in step (3) is carried out at a temperature of 500-900°C for a period of 20-120 min; more preferably, the high temperature pyrolysis is carried out at a temperature of 600-800°C for a period of 40-80 min.
[0023] Preferably, the inert gas in step (3) is selected from one or more of nitrogen, helium, argon, etc.
[0024] Preferably, the specific parameters of the ALD in step (4) are: performing 2 to 8 cycles (2c-8c) of ALD to deposit Pt; most preferably, the specific parameters of the ALD are: performing 2 cycles (2c) of ALD to deposit Pt.
[0025] The second aspect of the present invention provides a supported PtFe diatomic catalyst prepared according to the above preparation method.
[0026] Preferably, in the supported PtFe diatomic catalyst, Pt and Fe are dispersed in the carrier in the structure of diatomic pairs.
[0027] Preferably, the average distance between PtFe diatoms in the supported PtFe diatomic catalyst is 0.33-0.35 nm.
[0028] The third aspect of the present invention provides the use of the supported PtFe diatomic catalyst prepared according to the above preparation method in the anode of a fuel cell.
[0029] Preferably, the application is specifically an anode hydrogen oxidation reaction and / or a cathode oxygen reduction reaction.
[0030] Compared with the prior art, the present invention has the following technical effects:
[0031] Through extensive research, the present invention prepares a loaded low Pt diatomic catalyst 2cPtFeNC / AC by mixing FeNC and ammonium chloride for pyrolysis and then using a specific atomic layer deposition method to uniformly deposit low-loaded Pt single atoms on the FeNC / AC surface, wherein the Pt loading is 0.4wt%, the Fe loading is 0.37wt%, and the Pt loading is significantly lower than the prior art level. Due to the high exposed surface, gradient porous structure and stable metal loading sites, FeNC / AC provides an ideal carrier for the successful construction of diatomic catalysts. Based on its self-saturation limitation and selective deposition characteristics, ALD technology can control the deposition of Pt single atoms at the atomic scale, which is conducive to the precise and controllable synthesis of PtFe diatomic catalysts. By regulating the coordination environment of the active sites of Pt atoms, the multifunctional synergistic catalysis of low Pt diatomic catalysts in fuel cells is achieved, and the catalytic efficiency of the catalyst in hydrogen oxidation at the anode of the fuel cell can be significantly improved while greatly reducing the Pt loading. In order to obtain a catalyst in diatomic form, strict restrictions are imposed on ALD deposition parameters. The present invention found that when the number of ALD deposition cycles is too large, a mixed form of single atoms and atomic clusters will be formed, which seriously affects the catalytic performance of the catalyst. When two cycles (2c) of ALD deposition of Pt are performed, a PtFe diatomic catalyst with uniform structure and optimal performance can be obtained. The 2cPtFeNC / AC diatomic catalyst of the present invention exhibits excellent unit mass activity (10.5Amg Pt -1 ) is a commercial nanoparticle Pt / C (0.2A mg Pt -1 ) catalyst mass activity is 48.5 times higher than that of the catalyst. At the same time, the significant reduction in Pt loading can also effectively reduce the production and preparation costs. The present invention helps to achieve the precise construction of low-Pt diatomic catalysts and provide a high-activity, high-stability and low-cost excellent catalyst system for hydrogen fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a low-magnification transmission electron microscopy image of the supported low-Pt diatomic catalyst 2cPtFeNC / AC obtained in Example 1.
[0033] Figure 2 This is a high-magnification transmission electron microscopy image of the supported low-Pt diatomic catalyst 2cPtFeNC / AC obtained in Example 1.
[0034] Figure 3 This is the spherical aberration corrected transmission electron microscopy AC-HAADF-STEM image of the supported low Pt diatomic catalyst 2cPtFeNC / AC obtained in Example 1.
[0035] Figure 4This is the Pt-Fe diatomic distance distribution diagram of the supported low Pt diatomic catalyst 2cPtFeNC / AC obtained in Example 1.
[0036] Figure 5 This is the energy spectrum distribution diagram of C, N, Fe, and Pt elements in the supported low-Pt diatomic catalyst 2cPtFeNC / AC obtained in Example 1.
[0037] Figure 6 This is the morphology of the ALD 10cPtFeNC / AC catalyst obtained in Comparative Example 1.
[0038] Figure 7 Pt obtained in Comparative Example 2 NP Morphology of FeNC / AC catalyst.
[0039] Figure 8 This is the morphology of the ALD 2cPtNC / AC single atom catalyst obtained in Comparative Example 3.
[0040] Fig. 9 This is the current-voltage performance curve of different catalysts in the hydrogen oxidation reaction.
[0041] Fig.10 Schematic diagram of the unit mass activity results of different catalysts in the hydrogen oxidation reaction.
[0042] Fig.11 Schematic diagram of the H2-O2 fuel cell performance polarization curve results. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0044] Example 1
[0045] A supported low-Pt diatomic catalyst, the preparation method of which specifically comprises the following steps:
[0046] (1) 6.74 g Zn(NO3)2·6H2O and 0.326 g Fe(NO3)3·9H2O were stirred and dissolved in 1000 mL methanol, and 1000 mL 2-methylimidazole methanol solution (containing 7.88 g 2-methylimidazole) was added and stirred at room temperature for 24 h; then, Fe-ZIF-8 was obtained by centrifugation, washing and vacuum drying.
[0047] (2) Fe-ZIF-8 was heated to 1000°C in a nitrogen atmosphere for high temperature carbonization for 2 h to obtain Fe-NC containing single Fe atoms.
[0048] (3) Fe-NC and NH4Cl were uniformly mixed in a mass ratio of 1:3, heated to 700°C in a nitrogen atmosphere for high-temperature pyrolysis for 1 h to obtain a Fe-NC / AC carrier with a mesoporous structure.
[0049] (4) With Fe-NC / AC as the substrate material, ALD was performed with two cycles of Pt source pulses under vacuum conditions to deposit Pt single atoms on the carrier surface, thus obtaining 2cPtFeNC / AC diatomic material.
[0050] Example 2
[0051] A supported low-Pt diatomic catalyst, the preparation method of which specifically comprises the following steps:
[0052] (1) 6.74 g Zn(NO3)2·6H2O and 0.326 g Fe(NO3)3·9H2O were stirred and dissolved in 1000 mL methanol, and 1000 mL 2-methylimidazole methanol solution (containing 7.88 g 2-methylimidazole) was added and stirred at room temperature for 24 h; then, Fe-ZIF-8 was obtained by centrifugation, washing and vacuum drying.
[0053] (2) Fe-ZIF-8 was heated to 900 °C in a nitrogen atmosphere for high temperature carbonization for 3 h to obtain Fe-NC containing single Fe atoms.
[0054] (3) Fe-NC and NH4Cl were uniformly mixed in a mass ratio of 1:3, heated to 600°C in a nitrogen atmosphere for high-temperature pyrolysis for 80 min, and a Fe-NC / AC carrier with a mesoporous structure was obtained.
[0055] (4) With Fe-NC / AC as the substrate material, ALD was performed with two cycles of Pt source pulses under vacuum conditions to deposit Pt single atoms on the carrier surface, thus obtaining 2cPtFeNC / AC diatomic material.
[0056] Example 3
[0057] A supported low-Pt diatomic catalyst, the preparation method of which specifically comprises the following steps:
[0058] (1) 6.74 g Zn(NO3)2·6H2O and 0.326 g Fe(NO3)3·9H2O were stirred and dissolved in 1000 mL methanol, and 1000 mL 2-methylimidazole methanol solution (containing 7.88 g 2-methylimidazole) was added and stirred at room temperature for 24 h; then, Fe-ZIF-8 was obtained by centrifugation, washing and vacuum drying.
[0059] (2) Fe-ZIF-8 was heated to 1100°C in a nitrogen atmosphere for high temperature carbonization for 1.5 h to obtain Fe-NC containing single Fe atoms.
[0060] (3) Fe-NC and NH4Cl were uniformly mixed in a mass ratio of 1:3, heated to 800°C in a nitrogen atmosphere for high-temperature pyrolysis for 40 min, and a Fe-NC / AC carrier with a mesoporous structure was obtained.
[0061] (4) With Fe-NC / AC as the substrate material, ALD was performed with two cycles of Pt source pulses under vacuum conditions to deposit Pt single atoms on the carrier surface, thus obtaining 2cPtFeNC / AC diatomic material.
[0062] Comparative Example 1
[0063] A supported low-Pt catalyst, the preparation method of which specifically comprises the following steps:
[0064] (1) 6.74 g Zn(NO3)2·6H2O and 0.326 g Fe(NO3)3·9H2O were stirred and dissolved in 1000 mL methanol, and 1000 mL 2-methylimidazole methanol solution (containing 7.88 g 2-methylimidazole) was added and stirred at room temperature for 24 h; then, Fe-ZIF-8 was obtained by centrifugation, washing and vacuum drying.
[0065] (2) Fe-ZIF-8 was heated to 1000°C in a nitrogen atmosphere for high temperature carbonization for 2 h to obtain Fe-NC containing single Fe atoms.
[0066] (3) Fe-NC and NH4Cl were uniformly mixed in a mass ratio of 1:3, heated to 700°C in a nitrogen atmosphere for high-temperature pyrolysis for 1 h to obtain a Fe-NC / AC carrier with a mesoporous structure.
[0067] (4) Using Fe-NC / AC as the substrate material, ALD was performed under vacuum conditions with 10 cycles of Pt source pulses to obtain a mixture of Pt single atoms and atomic clusters on the carrier surface, namely, 10cPtFeNC / AC cluster catalyst material.
[0068] Comparative Example 2
[0069] A supported nanoparticle Pt NP The FeNC / AC catalyst, the preparation method thereof specifically comprises the following steps:
[0070] (1) 6.74 g Zn(NO3)2·6H2O and 0.326 g Fe(NO3)3·9H2O were stirred and dissolved in 1000 mL methanol, and 1000 mL 2-methylimidazole methanol solution (containing 7.88 g 2-methylimidazole) was added and stirred at room temperature for 24 h; then, Fe-ZIF-8 was obtained by centrifugation, washing and vacuum drying.
[0071] (2) Fe-ZIF-8 was heated to 1000°C in a nitrogen atmosphere for high temperature carbonization for 2 h to obtain Fe-NC containing single Fe atoms.
[0072] (3) Fe-NC and NH4Cl were uniformly mixed in a mass ratio of 1:3, heated to 700°C in a nitrogen atmosphere for high-temperature pyrolysis for 1 h to obtain a Fe-NC / AC carrier with a mesoporous structure.
[0073] (4) Weigh 20 mg of Fe-NC / AC and disperse it in ethylene glycol (EG) by ultrasonic. Add an appropriate amount of H2Pt / Cl6·6H2O to the Fe-NC / AC dispersion. Add NaOH to the mixed solution to adjust the pH to 11. Heat the mixed solution to boiling and then cool it to room temperature. Wash it with ultrapure water for 5 times to obtain nanoparticles of Pt NP FeNC / AC catalyst.
[0074] Comparative Example 3
[0075] A supported low Pt atom catalyst, the preparation method of which specifically comprises the following steps:
[0076] (1) 6.74 g Zn(NO3)2·6H2O was dissolved in 1000 mL methanol by stirring, and 1000 mL 2-methylimidazole methanol solution (containing 7.88 g 2-methylimidazole) was added, and the mixture was stirred and reacted at room temperature for 24 h; then, the mixture was centrifuged, washed, and vacuum dried to obtain ZIF-8.
[0077] (2) ZIF-8 was heated to 1000 °C in a nitrogen atmosphere for high temperature carbonization for 2 h to obtain metal-free NC.
[0078] (3) NC and NH4Cl were uniformly mixed in a mass ratio of 1:3, and heated to 700°C for high-temperature pyrolysis for 1 h under a nitrogen atmosphere to obtain a NC / AC carrier with a mesoporous structure;
[0079] (4) Using NC / AC as the substrate material, ALD was performed with two cycles of Pt source pulses under vacuum conditions to deposit Pt on the surface of the carrier to obtain 2cPtNC / AC catalyst material.
[0080] Verification Example 1
[0081] First, the morphology of the supported low-Pt diatomic catalyst 2cPtFeNC / AC prepared in Example 1 of the present invention was detected. Figure 1 This is a low-magnification transmission electron microscopy image. Figure 2 This is a high-magnification transmission electron microscopy image. Figure 3 This is the ACHAADFSTEM image of the spherical aberration corrected transmission electron microscope. Figure 4 is the Pt-Fe diatomic distance statistics diagram, Figure 5 The energy spectrum distribution diagram of C, N, Fe, and Pt elements in the diatomic catalyst. The results show that Pt and Fe representing the metal sites appear in pairs in the form of diatoms, the average distance between PtFe diatoms is 0.33-0.35nm, and each element is evenly dispersed on the carrier. The above results show that the ALD technology regulated by specific parameters in this embodiment successfully prepared the supported 2cPtFeNC / AC diatomic catalyst, and Pt and Fe are evenly dispersed in the carrier in the form of diatomic pairs, where the Pt loading is about 0.4wt% and the Fe loading is about 0.37wt%.
[0082] Secondly, the morphology of the catalysts prepared in Comparative Examples 1-3 of the present invention was tested. Figure 2 The transmission electron microscopy and spherical aberration electron microscopy images shown in the figure show that the morphology of the ALD 10cPtFeNC / AC catalyst prepared in Comparative Example 1 is as follows: Figure 6 As shown, Figure 6 (a) is a low-magnification transmission electron microscopy image. Figure 6 (b) is a high-magnification transmission electron microscope image. Figure 6 (c) is a spherical aberration corrected transmission electron microscopy image. The results show that there are no obvious Pt nanoparticles on the surface of the ALD 10cPtFeNC / AC catalyst, and Pt is distributed on the surface of the carrier in the form of single atoms and atomic clusters; the inductively coupled plasma emission spectrum shows that the Pt loading in the 10cPtFeNC / AC catalyst is 1.0wt% and the Fe loading is 0.37wt%. Comparative Example 2 Pt containing only Pt particles dispersed on the surface of the FeNC / AC carrier was prepared by chemically assisted microwave reduction. NP The morphology of FeNC / AC catalyst is shown in Figure 7 As shown, Figure 7 (a) is a low-magnification transmission electron microscopy image. Figure 7 (b) is a high-magnification transmission electron microscopy image. The results show that in Pt NP In the FeNC / AC catalyst, Pt is dispersed on the surface of the support in the form of nanoparticles with a particle size of 3-5 nm. Inductively coupled plasma emission spectroscopy shows that Pt NP The Pt loading in FeNC / AC is 2.5 wt %. In addition, in Comparative Example 3, 2 circles of Pt were deposited on the NC substrate by ALD to prepare a 2cPtNC / AC catalyst, the morphology of which is shown in FIG. Figure 8 As shown, Figure 8 (a) is a low-magnification transmission electron microscopy image. Figure 8 (b) is a high-magnification transmission electron microscopy image. The results show that the ALD 2c PtNC / AC has uneven dispersion of Pt atoms and clusters. Inductively coupled plasma emission spectroscopy shows that the Pt loading is 0.9wt%, indicating that the Fe single atom in the carrier material plays an important role in anchoring Pt atoms.
[0083] Subsequently, the catalysts prepared in Example 1, Comparative Examples 1-3, and commercial Pt / C catalysts were respectively used to test the hydrogen oxidation performance of the fuel cell anode. The test conditions were as follows: electrochemical workstation: French Bio Logic electrochemical workstation; counter electrode: Pt sheet electrode; reference electrode: reversible hydrogen electrode; electrolyte: 0.1M HClO4 solution; the hydrogen oxidation performance in the three-electrode and single-cell test results is as follows Figure 9-11 The results show that by constructing PtFe diatomic active sites, the ALD 2c PtFeNC / AC supported diatomic catalyst prepared in Example 1 of the present invention has a limiting diffusion current density of 2.5 mA cm at 0.05 V in a challenging acidic electrolyte. -2 , compared with the ALD deposited 10c PtFeNC / AC catalyst (2.1mAcm -2 ), ALD 2c Pt-NC / AC single atom catalyst in Comparative Example 3 (1.9 mA cm -2 ) and the nanoparticles Pt in Comparative Example 2 NP FeNC / AC catalyst (1.8 mA cm -2 ), its catalytic performance has obvious advantages (such as Fig. 9 More importantly, the ALD 2c PtFe-NC diatomic catalyst prepared in Example 1 of the present invention exhibits an extremely high unit mass activity, and its mass activity is 10.6 mA·mg at a potential of 0.05 V. Pt -1 , much higher than the ALD 10c PtFeNC / AC (4.8 mA·mg Pt -1 ) catalyst, Pt in Comparative Example 2 NP FeNC / AC(4.7mA·mg Pt -1 ) catalyst, 2cPt-NC / AC single atom in Comparative Example 3 (2.5mA·mg Pt -1 ) catalyst and commercial Pt / C (0.2 mA·mg Pt -1) catalyst, which is 48.5 times more active than the commercial nanoparticle Pt / C catalyst (see Fig.10 ). In the anode application of hydrogen and oxygen fuel cells, the ALD 2cPtFeNC / AC supported diatomic catalyst prepared in Example 1 of the present invention has a very low Pt loading of 0.02 mg. Pt cm -2 Under the condition of 0.4 mg / cm2, it can show superiority over commercial nanoparticle Pt / C catalyst (0.4 mg / cm2). Pt cm -2 ) of the battery discharge performance (see Fig.11 ).
[0084] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.
Claims
1. A method for preparing a supported PtFe diatomic catalyst, characterized in that: The steps include: (1) dissolving zinc salt and iron salt in an organic solvent and mixing them evenly, adding 2-methylimidazole solution, and stirring them together at room temperature for reaction; then centrifuging, washing, and drying to obtain Fe-ZIF-8; (2) Fe-ZIF-8 is carbonized at high temperature under an inert gas atmosphere to obtain Fe-NC containing single Fe atoms; (3) Fe-NC and NH4Cl are mixed and pyrolyzed at high temperature under an inert gas atmosphere to obtain a Fe-NC / AC carrier with a mesoporous structure; (4) ALD was used to deposit single Pt atoms on the surface of the Fe-NC / AC support to obtain the diatomic catalyst PtFeNC / AC.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the zinc salt to the iron salt in step (1) is 10-30:
1.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the zinc salt in step (1) to the 2-methylimidazole in the 2-methylimidazole solution is 0.5-1:
1.
4. The preparation method according to claim 1, characterized in that: The high temperature carbonization temperature in step (2) is 800-1200° C. and the time is 1-5 hours.
5. The preparation method according to claim 1, characterized in that: The mass ratio of Fe-NC to NH4Cl in step (3) is 1:2-5.
6. The preparation method according to claim 1, characterized in that: The high temperature pyrolysis in step (3) is carried out at a temperature of 500-900°C and for a time of 20-120 minutes.
7. The preparation method according to claim 1, characterized in that: The specific parameters of the ALD in step (4) are: performing 2 to 8 cycles of ALD to deposit Pt.
8. The supported PtFe diatomic catalyst prepared according to the preparation method according to any one of claims 1 to 7.
9. The supported PtFe diatomic catalyst according to claim 8, characterized in that: In the supported PtFe diatomic catalyst, Pt and Fe are dispersed in the carrier in the structure of diatomic pairs.
10. The supported PtFe diatomic catalyst according to claim 8, characterized in that: The average distance between two PtFe atoms in the supported PtFe diatomic catalyst is 0.33-0.35 nm.
Citation Information
Patent Citations
Metal monatomic catalyst and preparation method thereof
CN111420691A
Iron-doped magnesium aluminate spinel loaded noble metal catalyst as well as preparation and application thereof
CN113996312A
Hierarchical pore defect carbon loaded monatomic oxygen reduction electrocatalyst and preparation method thereof
CN117613288A
Double monatomic doped carbon coupled Pt3Zn intermetallic compound as well as preparation method and application thereof
CN118136867A
KR20240093022A
Cited By
Ru-based electrolyzed water catalyst composite material as well as preparation method and application thereof