Preparation method of sodium ion battery bacterial cellulose diaphragm
The preparation of sodium ion battery separators through the treatment of bacterial cellulose hydrogels has solved the problem of sodium dendrite and dead sodium deposition in sodium metal batteries, improved the cycle life and Coulomb efficiency, and achieved protection of the metal sodium negative electrode. Materials are safe and easy to obtain.
Patent Information
- Application Number
- CN202411285526.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the circulation process, sodium dendrite and dead sodium are formed due to uneven deposition of sodium ions, resulting in electrolyte consumption, reduced Coulomb efficiency and safety problems, and the existing diaphragm cannot effectively inhibit these side reactions.
Using bacterial cellulose hydrogel as raw material, it replaces water molecules by soaking in anhydrous ethanol solution to form an ethanol gel film, and then drying in a vacuum oven and then soaking into the sodium ion battery electrolyte to prepare a kind of inhibitory effect. Sodium dendrite growth and dead sodium deposition of sodium separators.
It significantly improves the cycle life and Coulomb efficiency of sodium ion batteries, realizes the protection of the sodium metal negative electrode, and the material is non-toxic and simple and easy to obtain.
Smart Images

Figure CN118943646A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a method for preparing a bacterial cellulose diaphragm for a sodium ion battery. Background Art
[0002] At a time when energy crisis and environmental pollution are serious, new energy is developing rapidly and the demand for electric vehicles is increasing. Developing large-scale energy storage with high energy / power density and high energy conversion efficiency is an effective strategy to ensure the efficient and stable use of new energy electricity.
[0003] Among various electrochemical energy storage devices, sodium metal battery raw materials are abundant, with large theoretical capacity, low potential and broad application prospects. However, its sodium metal negative electrode has high activity. During the battery cycle, the current density and uneven deposition of sodium ions will form sodium dendrites and dead sodium. It is also easy to react with the electrolyte to form an uneven and unstable SEI layer, resulting in continuous consumption of electrolyte, reduced battery coulomb efficiency, reduced battery cycle stability, and possible safety issues.
[0004] As an indispensable part of the battery composition, the diaphragm has the functions of isolating the positive and negative electrodes and transmitting ions in the battery. The quality of the diaphragm directly affects the interface stability of the battery, the battery capacity, and the long-term safe and stable operation of the battery. By designing a diaphragm for sodium metal batteries, the occurrence of sodium dendrites and dead sodium deposition can be effectively inhibited, and the cycle life and coulomb efficiency of sodium ion batteries can be improved. Bacterial cellulose (BC) is a cellulose produced by bacteria and is a typical biomass material. Cellulose is the most abundant natural polymer on earth. It is a linear natural polymer glucose anhydride with the characteristics of high crystallinity, fibrous and insoluble. It has the characteristics of 3D mesh structure, high tensile strength, etc., and the material is cheap, abundant in source, non-toxic and harmless, and has outstanding advantages in diaphragm materials. Based on the above characteristics, the present invention adopts bacterial cellulose hydrogel as raw material, and through simple processing, invents a method for preparing a sodium metal battery diaphragm. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a bacterial cellulose membrane for a sodium ion battery, wherein the membrane can inhibit side reactions such as sodium dendrite growth and dead sodium deposition of a sodium metal battery, and can greatly improve the cycle life and coulombic efficiency of the sodium ion battery.
[0006] The technical solution adopted by the present invention is a method for preparing a bacterial cellulose membrane for a sodium ion battery, which is specifically implemented according to the following steps:
[0007] Step 1, soaking the bacterial cellulose hydrogel in an ethanol solution to obtain a replaced bacterial cellulose ethanol gel film;
[0008] Step 2, sandwiching the bacterial cellulose ethanol gel membrane obtained in step 1 between two filter papers and drying them to obtain a solid bacterial cellulose membrane;
[0009] Step 3: Infiltrate the dried bacterial cellulose membrane obtained in step 2 into a sodium ion battery electrolyte to obtain a sodium ion battery bacterial cellulose membrane.
[0010] The present invention is also characterized in that:
[0011] In step 1, the bacterial cellulose hydrogel is immersed in the ethanol solution for three times, and each immersion time is 5 to 8 hours.
[0012] The ethanol solution in step 1 is anhydrous ethanol.
[0013] In step 2, drying is performed in a vacuum oven, the temperature of the vacuum oven is 60 to 80° C., and the drying time is 3 to 5 hours.
[0014] In step 3, the sodium ion battery electrolyte is 1M NaClO4 / PC.
[0015] The soaking time in step 3 is 12h-24h.
[0016] The beneficial effect of the present invention is that the preparation method of the bacterial cellulose membrane for sodium ion battery can inhibit the growth of sodium ion battery dendrites and the occurrence of electrode interface and electrolyte side reactions compared with the existing sodium ion battery membrane, and the prepared sodium ion battery has a longer cycle life and higher coulomb efficiency, thereby achieving the purpose of protecting the metallic sodium negative electrode. The preparation method of the bacterial cellulose membrane for sodium ion battery of the present invention is simple, and the raw materials are non-toxic and harmless and easy to obtain. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is the cycle time curve of the battery assembled in Example 1. DETAILED DESCRIPTION
[0018] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0019] The method for preparing the bacterial cellulose membrane for sodium ion batteries of the present invention is specifically implemented according to the following steps:
[0020] Step 1, soaking the bacterial cellulose hydrogel in an ethanol solution to obtain a replaced bacterial cellulose ethanol gel film;
[0021] In step 1, the bacterial cellulose hydrogel is soaked in an ethanol solution three times, each time for 5 to 8 hours. Bacterial cellulose has an expanded three-dimensional network structure, contains a large number of hydroxyl groups in the molecules, and forms a large number of hydrogen bonds with water to form a bacterial cellulose hydrogel. It is soaked in an ethanol solution, and ethanol molecules replace water molecules to enter between bacterial cellulose molecules and displace the water molecules. It is soaked three times, each time for 5 to 8 hours, in order to completely displace the water molecules, and obtain a bacterial cellulose ethanol gel film.
[0022] The ethanol solution in step 1 is anhydrous ethanol. Sodium metal is highly active and reacts violently with water. In order to obtain a solid bacterial cellulose membrane without water molecules, anhydrous ethanol needs to be used; and ethanol molecules are more volatile than water molecules during the drying process, and the drying process has less impact on the collapse of the three-dimensional network structure of bacterial cellulose, thereby making the gap and pore structure of the solid bacterial cellulose membrane after drying better.
[0023] Step 2, sandwiching the bacterial cellulose ethanol gel membrane obtained in step 1 between two filter papers and drying in a vacuum oven to obtain a solid bacterial cellulose membrane;
[0024] In step 2, drying is performed in a vacuum oven, the vacuum oven temperature is 60-80°C, and the drying time is 3h-5h. In the vacuum oven, the influence of oxygen in the air is avoided under vacuum conditions, and the temperature should not be too high. Too high a temperature will reduce the mechanical strength of the solid cellulose film and affect the performance of the final sodium ion battery. Too low a temperature will cause the ethanol molecules to evaporate too slowly, and the good gap and pore structure of the solid bacterial cellulose film cannot be obtained. Therefore, the solid bacterial cellulose film finally obtained retains a good gap and pore structure under 60-80°C conditions, and retains good flexibility, which is more in line with the requirements of the sodium ion battery separator.
[0025] Step 3: Infiltrate the dried bacterial cellulose membrane obtained in step 2 into a sodium ion battery electrolyte to obtain a sodium ion battery bacterial cellulose membrane.
[0026] In step 3, the sodium ion battery electrolyte is 1M NaClO4 / PC. 1M NaClO4 / PC electrolyte is currently a commonly used electrolyte in sodium ion batteries, and has good compatibility with sodium metal and various electrodes of sodium ion batteries. Therefore, 1M NaClO4 / PC is used to analyze the effect of the prepared diaphragm on the battery cycle stability, which is more general.
[0027] The immersion time in step 3 is 12h-24h, so that the diaphragm is better and more completely infiltrated by the electrolyte and the interface contact with the sodium metal electrode is closer, thereby reducing the resistance, obtaining good kinetic performance, and reducing the occurrence of side reactions between the sodium metal interface and the electrolyte.
[0028] Example 1
[0029] The method for preparing the bacterial cellulose membrane for sodium ion batteries of the present invention is specifically implemented according to the following steps:
[0030] Step 1, soaking the bacterial cellulose hydrogel in an ethanol solution to obtain a replaced bacterial cellulose ethanol gel film;
[0031] Step 2, sandwiching the bacterial cellulose ethanol gel membrane obtained in step 1 between two filter papers and drying in a vacuum oven to obtain a solid bacterial cellulose membrane;
[0032] Step 3: Infiltrate the dried bacterial cellulose membrane obtained in step 2 into a sodium ion battery electrolyte to obtain a sodium ion battery bacterial cellulose membrane.
[0033] Example 2
[0034] The method for preparing the bacterial cellulose membrane for sodium ion batteries of the present invention is specifically implemented according to the following steps:
[0035] Step 1, soaking the bacterial cellulose hydrogel in an ethanol solution to obtain a replaced bacterial cellulose ethanol gel film;
[0036] In step 1, the bacterial cellulose hydrogel is soaked in an ethanol solution three times, each time for 5 to 8 hours. Bacterial cellulose has an expanded three-dimensional network structure, contains a large number of hydroxyl groups in the molecules, and forms a large number of hydrogen bonds with water to form a bacterial cellulose hydrogel. It is soaked in an ethanol solution, and ethanol molecules replace water molecules to enter between bacterial cellulose molecules and displace the water molecules. It is soaked three times, each time for 5 to 8 hours, in order to completely displace the water molecules, and obtain a bacterial cellulose ethanol gel film.
[0037] The ethanol solution in step 1 is anhydrous ethanol. Sodium metal is highly active and reacts violently with water. In order to obtain a solid bacterial cellulose membrane without water molecules, anhydrous ethanol needs to be used; and ethanol molecules are more volatile than water molecules during the drying process, and the drying process has less impact on the collapse of the three-dimensional network structure of bacterial cellulose, thereby making the gap and pore structure of the solid bacterial cellulose membrane after drying better.
[0038] Step 2, sandwiching the bacterial cellulose ethanol gel membrane obtained in step 1 between two filter papers and drying in a vacuum oven to obtain a solid bacterial cellulose membrane;
[0039] In step 2, drying is performed in a vacuum oven, the vacuum oven temperature is 60-80°C, and the drying time is 3h-5h. In the vacuum oven, the influence of oxygen in the air is avoided under vacuum conditions, and the temperature should not be too high. Too high a temperature will reduce the mechanical strength of the solid cellulose film and affect the performance of the final sodium ion battery. Too low a temperature will cause the ethanol molecules to evaporate too slowly, and the good gap and pore structure of the solid bacterial cellulose film cannot be obtained. Therefore, the solid bacterial cellulose film finally obtained retains a good gap and pore structure under 60-80°C conditions, and retains good flexibility, which is more in line with the requirements of the sodium ion battery separator.
[0040] Step 3: Infiltrate the dried bacterial cellulose membrane obtained in step 2 into a sodium ion battery electrolyte to obtain a sodium ion battery bacterial cellulose diaphragm.
[0041] Example 3
[0042] The bacterial cellulose hydrogel was soaked in anhydrous ethanol solution for 5 hours. After three times, the obtained bacterial cellulose hydrogel was sandwiched between two filter papers and placed in a vacuum drying oven at 60°C for five hours. The obtained bacterial cellulose membrane was soaked in 1M NaClO4 / PC solution for 24 hours, and repeated twice. The bacterial cellulose membrane prepared in Example 1 was used to make a battery according to the following method.
[0043] The metallic sodium sheet is the counter electrode, and the prepared bacterial cellulose membrane has been soaked in the electrolyte of the sodium ion battery and can be used directly to assemble it into a sodium metal symmetric battery. Figure 1 For the corresponding battery at 1mAcm -2 At a current density of 1 mAh cm -2 The cycle time curves below show that the sodium metal symmetric battery has significantly improved cycle life and coulombic efficiency compared with the commercial glass fiber separator.
Claims
1. A method for preparing a bacterial cellulose membrane for a sodium ion battery, characterized in that: Follow the steps below to implement it: Step 1, soaking the bacterial cellulose hydrogel in an ethanol solution to obtain a replaced bacterial cellulose ethanol gel film; Step 2, sandwiching the bacterial cellulose ethanol gel membrane obtained in step 1 between two filter papers and drying them to obtain a solid bacterial cellulose membrane; Step 3: Infiltrate the dried bacterial cellulose membrane obtained in step 2 into a sodium ion battery electrolyte to obtain a sodium ion battery bacterial cellulose membrane.
2. The method for preparing a bacterial cellulose membrane for a sodium ion battery according to claim 1, characterized in that: In the step 1, the bacterial cellulose hydrogel is immersed in the ethanol solution for three times, and each immersion time is 5 to 8 hours.
3. The method for preparing a bacterial cellulose membrane for a sodium ion battery according to claim 1, characterized in that: The ethanol solution in step 1 is anhydrous ethanol.
4. The method for preparing a bacterial cellulose membrane for a sodium ion battery according to claim 1, characterized in that: In step 2, drying is performed in a vacuum oven, the temperature of the vacuum oven is 60-80° C., and the drying time is 3 h to 5 h.
5. The method for preparing a bacterial cellulose membrane for a sodium ion battery according to claim 1, characterized in that: The sodium ion battery electrolyte in step 3 is 1M NaClO4 / PC.
6. The method for preparing a bacterial cellulose membrane for a sodium ion battery according to claim 1, characterized in that: The soaking time in step 3 is 12h-24h.
Citation Information
Patent Citations
Bacterial cellulose porous thin film and preparation method thereof
CN104157815A
Drying method of bacterial cellulose material for preparing lithium ion battery separation membrane
CN106549127A
Method for preparing three-dimensional network polymer gel electrolyte film based on bacterial cellulose
CN109841899A
Polydopamine-coated bacterial cellulose membrane and preparation method thereof
CN109950453A
Method for preparing lithium battery diaphragm
CN110474008A
Cited By
Nanocellulose-based sodium-ion battery diaphragm as well as preparation method and application thereof
CN119944227A