Heat-shrinkable multilayer film and method for producing same
By increasing the ratio of polyolefin-based resin and cyclic olefin copolymer in the heat shrinkable multilayer film, and combining with gas barrier resin, the problem of insufficient mechanical properties and tensile properties is solved, and high mechanical properties and heat shrinkage are achieved , suitable for packaging materials and maintain performance during recycling.
Patent Information
- Application Number
- CN202380030796.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing heat shrinkable multilayer films are difficult to meet the mechanical properties and tensile requirements when increasing the proportion of polyolefin resins, and are not suitable for material recycling, especially when packaging contents such as bones and flesh are easily produced. .
A multilayer film structure consisting of polyolefin-based resin, cyclic olefin copolymer and gas barrier resin is adopted, among which polyolefin-based resin accounts for more than 80% and cyclic olefin copolymer accounts for more than 15%, and film is made by the blowing method To optimize stretching and mechanical properties.
It achieves high mechanical properties and heat shrinkability, is suitable as an environmentally friendly packaging material, can withstand pinholes and maintain performance during recycling.
Smart Images

Figure BDA0005061836700000091 
Figure BDA0005061836700000211 
Figure BDA0005061836700000221
Abstract
Description
Technical Field
[0001] The present invention relates to a heat-shrinkable multilayer film containing a polyolefin resin and a method for producing the same. Background Art
[0002] Heat-shrinkable films used for packaging ham, sausage, and other foods have a variety of required properties, such as sealing for packaging contents, mechanical properties for protecting contents, gas barrier properties for maintaining freshness, and shrinkage properties for maintaining a good appearance. In order to meet these requirements, laminated films of various resins are widely used (for example, refer to Patent Documents 1 to 3).
[0003] As described in Patent Document 1, such a heat-shrinkable multilayer film in most cases comprises a polyolefin resin (hereinafter sometimes abbreviated as "PO") having excellent sealing and extrusion properties and a polyamide resin (hereinafter sometimes abbreviated as "PA") having excellent mechanical properties and stretchability as main layers.
[0004] In recent years, the demand for recycling of packaging materials has increased. For example, CEFLEX, a European Union organization, has proposed a rule that packaging materials containing PO of 90% by mass or more and resin components other than PO such as PA of 5% by mass or less can be recycled. Here, material recycling refers to the act of recycling plastic waste after crushing, dissolving, etc.
[0005] As described above, the heat-shrinkable multilayer film formed by laminating PO and PA does not meet the CEFLEX criteria in most cases. Due to the incompatibility of the layers, even if they are melted, mixed, and remolded after use, the mechanical properties and appearance will be significantly impaired due to layer separation, and practical performance as a recycled material cannot be obtained.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2007 / 094144
[0009] Patent Document 2: Japanese Patent Application No. 2015-512801
[0010] Patent Document 3: International Publication No. 2013 / 121874 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] Therefore, in order to achieve a material composition suitable for material recycling, it is ideal to adopt a composition with a PO ratio as high as possible. However, when the PO ratio is increased and the PA usage ratio is reduced, the stretchability and mechanical properties required for manufacturing a heat-shrinkable multilayer film are impaired.
[0013] Here, mechanical properties mainly refer to the strength against needle puncture, which is required to suppress pinholes generated when packaging protruding contents such as meat with bones. In addition, stretchability refers to the stable film-forming properties of the inflation bubble (second bubble) in the inflation (three-bubble process) method described in Patent Document 2. In most cases, heat-shrinkable multilayer films for meat packaging require shrinkage at temperatures below 100°C. In order to meet this requirement, the inflation (three-bubble process) method is used to produce films that can obtain oriented films with high orientation at low cost.
[0014] Patent Document 2 discloses a heat-shrinkable multilayer film using a cyclic olefin copolymer (hereinafter sometimes referred to as COC). The puncture test was conducted with a spherical ball rod at a speed of 1 mm / min. The film of the document has a damage resistance of 2 to 10 J / mm (≈1 to 150 N / mm), but it is difficult to say that it has sufficient strength to package contents with protrusions such as meat with bones. In addition, the film of the document is implemented in a form containing PA, and it is difficult to say that it is a film suitable for recycling. Furthermore, in this document, there is no mention of the material recyclability, tensile properties, elastic modulus, use in the sealing layer, and performance (sealing strength / adhesion) of the film containing COC.
[0015] Furthermore, in film formation using the inflation (three-bubble process) method, when only PO is stretched without using PA, bubbles cannot be formed unless PO is preheated to near the crystal melting point, so the orientation of the molecular chains is weak, making it difficult to obtain sufficient heat shrinkage and mechanical properties.
[0016] As a conventional heat-shrinkable multilayer film-making technology that does not use PA, there is a method of imparting a crosslinked structure to PO by irradiating PO with electron beams and utilizing ionomers, as described in Patent Document 3. However, crosslinked PO gels when melted, thereby hindering the recyclability of the material, and ionomers are expensive, thereby increasing costs. In addition, compared with the case of using PA, mechanical properties are inferior, and the elastic modulus of the film is low, thereby losing toughness and impairing compatibility with packaging machinery.
[0017] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a multilayer film comprising 80% by mass or more of a polyolefin resin and having excellent mechanical properties and heat shrinkage.
[0018] Technical Solution
[0019] The present inventors have found that the above problems can be solved by a heat-shrinkable multilayer film comprising a cyclic olefin copolymer in at least one layer of the multilayer film and the mass ratio of the cyclic olefin copolymer in the multilayer film is 15 mass % or more, thereby completing the present invention.
[0020] The heat-shrinkable multilayer film of the present invention is a multilayer film composed of at least three layers, namely an outer surface layer (a) comprising a polyolefin-based resin, an intermediate layer (b) comprising a gas barrier resin, and an inner surface layer (c) comprising a polyolefin-based resin. At least one layer of the multilayer film contains a cyclic olefin copolymer. When the total mass of the multilayer film is set to 100 mass%, the mass ratio of the polyolefin-based resin in the multilayer film is greater than 80 mass%, and the mass ratio of the cyclic olefin copolymer in the multilayer film is greater than 15 mass%.
[0021] The polyolefin-based resin in the outer surface layer (a) and / or the inner surface layer (c) preferably contains at least one selected from the group consisting of ultra-low-density polyethylene and linear low-density polyethylene, and a cyclic olefin copolymer.
[0022] The cyclic olefin copolymer preferably contains either or both of a cyclic olefin copolymer having a glass transition temperature of 50 to 68°C and a cyclic olefin copolymer having a glass transition temperature of -10 to 20°C.
[0023] The gas barrier resin of the intermediate layer (b) preferably includes at least one selected from the group consisting of partially saponified ethylene-vinyl acetate copolymers and glycolic acid (co)polymer resins.
[0024] In the heat-shrinkable multilayer film, the tensile elastic modulus in the transverse direction (TD) is preferably 200 to 600 MPa.
[0025] In the method for producing a heat-shrinkable multilayer film of the present invention, the portion before stretching in the TD direction ( Figure 1 The surface temperature of the resin at the α position) is 75 to 90°C, and the lower shoulder forming part ( Figure 1 The surface temperature of the resin at the β position) in the TD direction is 5 to 30° C. lower than the surface temperature of the resin at the portion immediately before stretching in the TD direction.
[0026] Beneficial Effects
[0027] The heat-shrinkable multilayer film of the present invention is composed of 80% by mass or more of a polyolefin resin and has excellent mechanical properties and heat shrinkage. Therefore, a heat-shrinkable multilayer film can be obtained, which is an environmentally friendly packaging film and can be used as a packaging film for products with a sudden change in temperature.
[0028] The packaging material also has pinhole resistance for such contents. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a diagram schematically showing an apparatus for producing the heat-shrinkable multilayer film of the present invention. DETAILED DESCRIPTION
[0030] The heat-shrinkable multilayer film of the present invention comprises an outer surface layer (a) comprising a polyolefin resin,
[0031] The intermediate layer (b) comprising a gas barrier resin and the inner surface layer (c) comprising a polyolefin resin
[0032] A multilayer film composed of at least three layers, wherein at least one layer of the multilayer film contains a cyclic olefin copolymer
[0033] When the total mass of the multilayer film is set to 100 mass %, the polyolefin resin
[0034] The mass ratio of the multilayer film is 80 mass % or more, and the cyclic olefin is
[0035] The mass ratio of the polymer in the multilayer film is 15 mass % or more.
[0036] The olefins referred to in the present invention are C n H 2n A hydrocarbon having a double bond represented by the formula
[0037] Olefins are cyclic structures consisting of carbon atoms and having carbon-carbon diolefins in the cyclic structure.
[0038] The number of carbon-carbon double bonds can be one or more (including aromatic
[0039] In addition, in this specification, the term "olefins" refers to compounds containing 50 mol% or more of olefins and / or cyclic olefins.
[0040] A homopolymer or copolymer of a hydrocarbon-derived structural unit is defined as a polyolefin-based resin.
[0041] The heat-shrinkable multilayer film of the present invention comprises a cyclic olefin copolymer in at least one layer of the multilayer film.
[0042] Among them, it is preferred that the outer surface layer (a) and / or the inner surface layer (c) contain a cyclic olefin copolymer.
[0043] The inner surface layer (c) preferably contains a cyclic olefin copolymer.
[0044] In the case of the heat-shrinkable multilayer film of the present invention, when the total mass of the multilayer film is set to 100 mass
[0045] In the case of the polyolefin resin, the proportion of the mass of the multilayer film is 80 mass % or more, preferably 90 mass % or more, and more preferably 95 mass % from the viewpoint of material recyclability.
[0046] If the mass ratio of the polyolefin resin is less than the above range,
[0047] The incompatibility of other components will affect the recyclability of the material.
[0048] The mass ratio can be calculated according to the following calculation formula.
[0049] Mass ratio of polyolefin resin (mass %) = 100 × (total of “density × thickness” of layer containing polyolefin resin) / (total of “density × thickness” of all layers)
[0050] In Table 2 described below, the mass ratio of PO (mass %) is described as "PO mass ratio
[0051] (wt%)".
[0052] The density of a layer formed by mixing two or more resins is the density of the resin multiplied by
[0053] The sum of the densities obtained by mixing the resins.
[0054] In the case of the heat-shrinkable multilayer film of the present invention, when the total mass of the multilayer film is set to 100 mass
[0055] When the mass percentage of the cyclic olefin copolymer is 15 mass % or more in the multilayer film,
[0056] It is preferably 15 to 80% by mass, more preferably 15 to 50% by mass, and most preferably 16 to 29% by mass.
[0057] If the mass ratio of the cyclic olefin copolymer is less than 15 mass %, the tensile strength during stretching is insufficient.
[0058] It is difficult to stably form a film. If the mass ratio of the cyclic olefin copolymer is greater than 80 mass %, there is a risk of
[0059] The mass ratio of COC (cyclic olefin copolymer) can be determined according to
[0060] The following calculation formula is used to calculate.
[0061] Mass ratio of cyclic olefin copolymer (%) = 100 × (total of “density × thickness × COC mixing ratio” of the layer containing COC) / (total of “density × thickness” of all layers)
[0062] In Table 2 described below, the mass ratio (mass %) of COC is described as "COC mass
[0063] Ratio (wt%)".
[0064] The density of a layer formed by mixing two or more resins is the density of the resin multiplied by
[0065] The sum of the densities obtained by mixing the resins.
[0066] It should be noted that the term "stretching" in the present invention refers to the double stretching in the film formation of the heat shrinkable film.
[0067] The process of biaxial stretching. Representative biaxial stretching methods include tentering method and inflation method.
[0068] The process of forming a heat shrinkable film is not limited to any of these methods, but from the perspective of cost,
[0069] Inflation method is particularly preferred. In addition, inflation method is divided into direct method (direct inflation) and tubular stretching method.
[0070] Method (tubular biaxial stretching), the direct method is to directly add the molten resin extruded into a tubular shape
[0071] The tubular stretching method is described in Patent Document 2, and includes the following steps:
[0072] After the tubular molten resin is temporarily cooled and solidified to form a tubular body, the tubular body is heated to an appropriate temperature.
[0073] The temperature is set at 100 °C, and the fluid is added to the inside of the tubular body while pulling it in the longitudinal direction (MD) and the transverse direction (TD).
[0074] The process of stretching is particularly preferred as a method for producing a heat shrinkable film.
[0075] In the process of forming a heat-shrinkable film, the tubular stretching method tends to have higher stress during stretching than the tentering method and the direct method, so there is a tendency to produce a heat-shrinkable film with excellent shrinkage. Depending on the number of bubbles formed in the film-making process, tubular biaxial stretching is sometimes divided into double bubble inflation (double bubble process) and triple bubble inflation (triple bubble process). The difference between the two is the difference in the heat treatment process after biaxial stretching. Either film-making method can be used, but considering the tendency of good dimensional stability of the heat-shrinkable film, the triple bubble inflation method is more preferred.
[0076] The outer surface layer (a) contains a polyolefin-based resin as a thermoplastic resin in order to provide excellent shrinkage characteristics, barrier properties to water vapor, and appropriate material recycling.
[0077] As PO (polyolefin resin) in the outer surface layer (a), for example, there can be listed: ethylene homopolymer; propylene homopolymer; copolymers of α-olefins having 2 to 8 carbon atoms such as VLDPE (ultra-low density polyethylene) and LLDPE (linear low-density polyethylene); propylene-ethylene copolymers, propylene-ethylene-butene-1 copolymers, EVA (ethylene-vinyl acetate copolymer), EAA (ethylene-acrylic acid copolymer), EMAA (ethylene-methacrylic acid copolymer), EMA (ethylene-methyl acrylate copolymer), EEA (ethylene-ethyl acrylate copolymer), EBA (ethylene-butyl acrylate copolymer) and other polyolefin copolymers, including cyclic olefin copolymers. These polyolefin resins can be used alone or in combination of two or more. Among them, LLDPE or VLDPE is particularly preferred, which includes resins produced by Ziegler-Natta type reaction catalysts and resins produced by metallocene or single-active site reaction catalysts.
[0078] As the polyolefin-based resin in the outer surface layer (a), a mixture of at least one selected from VLDPE and LLDPE and COC can be used.
[0079] The density of LLDPE or VLDPE is preferably 0.880 to 0.920 g / cm 3 , more preferably 0.890 to 0.915 g / cm 3 . In addition, the melt flow index (MI) of LLDPE or VLDPE is preferably 0.5 to 7.0 g / 10 min, more preferably 1.0 to 5.0 g / 10 min, and further preferably 3.2 to 4.0 g / 10 min. If the MI is 3.2 to 4.0 g / 10 min, the puncture strength of the film is maintained, and the fluidity when melted is also excellent, and there is a tendency to reduce the uneven thickness of the film. One example is a product sold by PrimePolymer under the name "Evolue", in which the α-olefin other than ethylene is 1-hexene. It should be noted that MI is measured at 190°C in accordance with JIS K 7210.
[0080] The COC in the outer surface layer (a) is a resin having a structural unit derived from a cyclic olefin and a structural unit derived from an olefin such as ethylene other than the cyclic olefin.
[0081] Examples of cyclic olefins include norbornene and its derivatives (eg, 2-norbornene, 5-methyl-2-norbornene); cyclopentadiene and its derivatives (eg, dicyclopentadiene, 2,3-dihydrocyclopentadiene), but are not limited thereto.
[0082] Examples of olefins other than cyclic olefins include α-olefins such as ethylene, propylene, and butene, but are not limited thereto.
[0083] In addition, as COC in the outer surface layer (a), for example, COC containing 60 to 90 mol % of structural units derived from ethylene, preferably 65 to 85 mol % of structural units derived from ethylene, 5 to 45 mol % of structural units derived from cyclic olefins, preferably 10 to 40 mol % of structural units derived from cyclic olefins can be used.
[0084] In addition, the glass transition temperature (Tg) of COC is measured by the peak temperature of the loss modulus E" of the data obtained under the conditions of a heating rate of 5°C / min, a frequency of 62.8 rad / sec, and a strain of 0.1% in the stretching mode of dynamic viscoelasticity measurement (DMA), and its value is preferably 50 to 68°C. If the glass transition temperature is within the above range, in the stretching process of the film, by setting the TD direction to the front part of the stretching (the front part of the lower shoulder of the blown film bubble to be formed): Figure 1 The surface temperature of the resin at the position of α) is 75 to 90°C, and the lower shoulder forming portion ( Figure 1 The surface temperature of the resin at the position of β) is higher than that of the resin immediately before stretching in the TD direction ( Figure 1 Under the condition that the surface temperature of the resin at the position of α) is 5 to 30°C lower than that of the surface temperature of the resin at the position of α, sufficient tensile stress (tensile strength) is exhibited to the internal pressure of the fluid blown into the inside of the tubular body during stretching, and there is a tendency that the film can be stably produced by the three-bubble inflation method. If the glass transition temperature is lower than 50°C, the tensile strength during stretching is insufficient, and there is a tendency that stable film production is difficult. In addition, the elastic modulus of the film becomes smaller, and there is a tendency that the mechanical adaptability is poor when the content is filled. In addition, if the glass transition temperature is higher than 68°C, it is necessary to increase the resin temperature during stretching, and the orientation becomes smaller, so there is a tendency for the hot water shrinkage rate to become smaller. In addition, there is a tendency for the elongation at break during the puncture test to become smaller.
[0085] In addition, the melt flow index (MI) of COC is preferably 0.5 to 5.0 g / 10 min, more preferably 0.8 to 4.0 g / 10 min, and further preferably 1.0 to 3.0 g / 10 min. If MI is less than 0.5 g / 10 min, the fluidity during melting deteriorates, and there is a tendency for uneven film thickness and impaired productivity. If MI is higher than 5.0 g / 10 min, the elongation at break may deteriorate when the film is punctured with needle-like protrusions. COC is sold, for example, by Polyplastics under the name of "TOPAS". It should be noted that MI is measured at 190 ° C according to JIS K 7210.
[0086] The polyolefin resin in the outer surface layer (a) preferably has a melting point of 80 to 170°C, more preferably 95 to 160°C, as measured by DSC (differential scanning calorimeter) at a heating rate of 10°C / min in accordance with JIS K 7121. If the melting point is lower than 80°C, the heat resistance of the multilayer film is insufficient, and problems such as melting during hot water shrinkage and adhesion to the sealing base during heat sealing are likely to occur. On the other hand, if the melting point is higher than 170°C, when the heat-shrinkable multilayer film is recycled after use, the temperature during melt kneading tends to be high, so the recycled product tends to have a yellow tint due to thermal degradation.
[0087] The gas barrier property in the present invention refers to the difficulty of oxygen permeation. The gas barrier resin in the present invention refers to a resin film with an oxygen permeability of 0.01 to 300 cm per 25 μm at 23°C and 0% RH. 3 / m 2 ·day·atm, preferably 0.05~200cm 3 / m 2 ·day·atm, most preferably 0.1~100cm 3 / m 2 ·day·atm of resin.
[0088] The gas barrier resin in the intermediate layer (b) can be selected from partially saponified ethylene-vinyl acetate copolymers called ethylene-vinyl alcohol copolymers (hereinafter sometimes abbreviated as EVOH), glycolic acid (co)polymers (hereinafter sometimes abbreviated as PGA), vinylidene chloride copolymers (hereinafter sometimes abbreviated as PVDC), polyvinyl alcohol (PVA), crystalline polyamide (MXD6) obtained by polycondensation of meta-xylylenediamine and adipic acid, aliphatic polyamide (PA) resins (such as nylon 6, etc.), amorphous aromatic polyamide resins (such as nylon 6I-6T, etc.), polyacrylonitrile copolymers (PAN), polyethylene terephthalate (PET), etc. The intermediate layer (b) preferably has a resin that provides excellent oxygen barrier properties to prevent oxidative degradation of the packaged article.
[0089] The preferred gas barrier resin for the intermediate layer (b) is EVOH, and particularly preferably EVOH having an ethylene content of 20 to 60 mol%, preferably 30 to 50 mol%, and a saponification degree of 95% or more. If the ethylene content of EVOH is lower than the above range, there is a tendency to hinder stretching processability, and if the ethylene content is greater than 60 mol%, there is a tendency for oxygen barrier properties to deteriorate. Furthermore, if the saponification degree of EVOH is less than 95%, there is a tendency for oxygen barrier properties to deteriorate. EVOH is sold, for example, by Kuraray under the name "EVAL".
[0090] As for the preferred gas barrier resin as the intermediate layer (b), there is a glycolic acid (co)polymer resin. As the glycolic acid (co)polymer resin, for example, a homopolymer of polyglycolic acid and a copolymer of polyglycolic acid can be listed. In addition, in the present invention, the glycolic acid (co)polymer resin is preferably formed by polyglycolic acid containing a repeating unit based on the following general formula at a ratio of 60% by mass or more, more preferably formed by polyglycolic acid containing the above repeating unit at a ratio of 70% by mass or more, and particularly preferably formed by polyglycolic acid containing the above repeating unit at a ratio of 80% by mass or more. If the repeating unit represented by the following general formula in the polyglycolic acid is less than the above lower limit, the crystallinity originally possessed by the polyglycolic acid is impaired, and there is a tendency for the gas barrier and heat resistance of the obtained heat-shrinkable multilayer film to be reduced.
[0091] [Chemical formula 1]
[0092]
[0093] The glycolic acid (co)polymer resin has a lower oxygen permeability per unit thickness than other gas barrier resins such as EVOH and PVDC, so even if the thickness of the intermediate layer (b) is further reduced, it can still exhibit gas barrier properties sufficient for practical use. As a result, it is expected that the recyclability will be improved in association with the increase in the volume ratio of the polyolefin layer.
[0094] In addition, the glycolic acid (co)polymer resin is known to be a hydrolyzable resin, and the molecular chain is randomly cut by hydrolysis to reduce the molecular weight. If the molecular weight is reduced to a level that cannot maintain strength, it will disintegrate, and if the molecular weight is further reduced, it will dissolve in water. By recycling the heat shrinkable multilayer film of the present invention after the intermediate layer (b) is hydrolyzed, it can be recycled at a higher polyolefin ratio, and it can be expected that the recyclability will be improved.
[0095] The inner surface layer (c) comprises a polyolefin resin as a sealable thermoplastic resin. The inner surface layer (c) is preferably a resin having excellent heat sealability among the properties required for the heat shrinkable multilayer film, and more preferably also having mechanical properties, shrinkage properties, barrier properties to water vapor, and material recycling adaptability.
[0096] The resin used for the inner surface layer (c) can be selected from the same polyolefin resin as the resin listed for the outer surface layer (a). Considering the heat sealability, it is particularly preferred to use a resin having a melting point of 80 to 150°C, preferably 95 to 130°C, obtained by using a DSC differential scanning calorimeter at a heating rate of 10°C / min according to JIS K 7121. If the melting point of the film is lower than 80°C, it is easy to cause adhesion (blocking) between the inner surface layers (c). If the melting point of the film is higher than 150°C, the temperature at which the seal can be made becomes higher, and there is a tendency to hinder the stretchability in the three-bubble inflation. In addition, additives such as lubricants can be added within the range that does not hinder the transparency of the film.
[0097] As the polyolefin resin in the inner surface layer (c), in order to suppress adhesion (blocking) between the inner surface layers (c), a mixture of at least one selected from VLDPE and LLDPE and COC can be used. The mass ratio (mixing ratio) of COC in the mixture is preferably 1 to 70 mass%, more preferably 20 to 60 mass%, and further preferably 40 to 50 mass%. If the mass of COC is less than 1 mass%, there is a tendency to lack the adhesion suppression effect, and if the mass of COC is more than 70 mass%, there is a tendency to reduce the heat sealability.
[0098] The COC used for the inner surface layer (c) can be selected from the same COC as the COC listed for the outer surface layer (a), for example, COC having a glass transition temperature of 50 to 68°C can be used. In addition, in order to improve the heat sealability of the inner surface layer (c) at low temperatures, COC having a glass transition temperature of 0 to 10°C can be further mixed. That is, either or both of COC having a glass transition temperature of 50 to 68°C and COC having a glass transition temperature of -10 to 20°C can be used. When the resin constituting the inner surface layer (c) is set to 100% by mass, the mass ratio (mixing ratio) of COC having a glass transition temperature of 0 to 10°C is preferably 5 to 30% by mass, and more preferably 10 to 20% by mass. If the COC having a glass transition temperature of 0 to 10°C is less than 5% by mass, there is a tendency that the effect of improving the low-temperature heat sealability is insufficient, and if the COC having a glass transition temperature of 0 to 10°C is more than 30% by mass, there is a tendency that the effect of suppressing blocking is reduced.
[0099] The heat-shrinkable multilayer film of the present invention includes the above-mentioned outer surface layer (a) containing a polyolefin resin, the intermediate layer (b) containing a gas barrier resin, and the inner surface layer (c) containing a polyolefin resin as necessary constituent layers, but in addition, it is also possible to include a plurality of other layers (z) in the intermediate layer other than the intermediate layer (b) containing a gas barrier resin for the purpose of improving the functionality or processability of the multilayer film as required. As an example of such other layers (z), a layer containing the polyolefin resin is preferred. In addition, in the case where the bonding force between the layers is insufficient, an adhesive resin layer can be provided.
[0100] The adhesive resin layer can be provided between the layers as required. As the adhesive resin, EVA, EEA, acid-modified polyolefins (reaction products of homopolymers or copolymers of olefins and unsaturated carboxylic acids, anhydrides, esters or metal salts such as maleic acid and fumaric acid, etc., such as acid-modified VLDPE, acid-modified LLDPE, acid-modified EVA) etc. can be used. As preferred adhesive resins, olefin resins modified by acids such as maleic acid or their anhydrides etc. can be cited.
[0101] The melting point of the thermoplastic resin selected for the other layer (z) is preferably 40 to 170° C., more preferably 50 to 160° C. If the melting point is lower than 40° C., the heat resistance of the multilayer film tends to deteriorate, and if the melting point is higher than 170° C., when the heat-shrinkable multilayer film is recycled after use, the temperature during melt kneading tends to be high, so the recycled product tends to have a yellow tint due to thermal deterioration.
[0102] Furthermore, in the above-mentioned layer constitution, an organic lubricant, an inorganic lubricant (anti-blocking agent) and / or an antistatic agent may be added to any layer.
[0103] In order to improve the slipperiness of the film during film manufacturing, the bag-making property during secondary processing, and the packaging machine adaptability during content filling, etc., it is preferred that an organic and / or inorganic lubricant is included in the inner surface layer (c) or the outer surface layer (a). Furthermore, corn starch or the like can be sprinkled on the inner and outer surfaces of the film as needed.
[0104] Examples of the organic lubricant include hydrocarbon lubricants, fatty acid lubricants, fatty acid amide lubricants, ester lubricants, and metal soaps. The organic lubricant may be liquid or solid. Among these lubricants, fatty acid amide lubricants and metal soaps are preferably used from the viewpoint of excellent compatibility with polyolefin resins. The organic lubricant is preferably used in a ratio of 0.1 to 0.2 mass % in the desired layer.
[0105] As the inorganic lubricant (anti-blocking agent), known inorganic fillers added to the resin for the purpose of suppressing adhesion between films can be used, such as talc, diatomaceous earth, silica, zeolite, calcium carbonate, aluminosilicate, etc. From the viewpoint of refractive index and dispersibility, for example, silica, aluminosilicate, zeolite, etc. are preferably used.
[0106] In addition, the inorganic lubricant preferably has a volume average particle size D50 measured by a Coulter counter method of 0.5 to 10 μm, and more preferably 1 to 7 μm. It is more preferred to use an inorganic lubricant having the above average particle size, wherein a portion having a particle size exceeding 10 μm is removed. The amount of the inorganic lubricant added is, for example, 0.05 to 2% by mass or less, and particularly preferably 0.1 to 1% by mass in the desired layer.
[0107] The organic or inorganic lubricant is preferably added to the desired resin layer in the form of a masterbatch containing the lubricant at a concentration of, for example, about 1 to 10% by mass in the resin constituting the desired layer or a resin having affinity therewith.
[0108] As the antistatic agent, a surfactant is preferably used. As the surfactant, an anionic surfactant, a cationic surfactant, a nonionic surfactant, an amphoteric surfactant, and a mixture thereof can be used. The antistatic agent can be added at a ratio of 0.05 to 2% by mass relative to the resin of the layer to be added as needed.
[0109] The heat-shrinkable multilayer film of the present invention is preferably formed into a film having a thickness of 10 to 150 μm, particularly 30 to 120 μm, by laminating the above-mentioned layers and stretching the film.
[0110] More specifically, the thickness of the outer surface layer (a) is, for example, 0.5 to 50 μm, preferably 0.5 to 30 μm, and more preferably 0.5 to 20 μm.
[0111] In addition, the thickness of the intermediate layer (b) is 0.5 to 30 μm, and particularly preferably 1 to 10 μm. If the thickness of the intermediate layer (b) composed of the gas barrier resin is thinner than 0.5 μm, there is a tendency that the improvement effect of oxygen barrier is insufficient, and if the thickness of the intermediate layer (b) composed of the gas barrier resin is thicker than 30 μm, the stretching processing of the multilayer film becomes difficult and the recyclability of the material is hindered.
[0112] Furthermore, in order to provide the multilayer film with a sufficient sealing strength required, the thickness of the inner surface layer (c) is preferably 0.5 to 50 μm, more preferably 1 to 30 μm.
[0113] Furthermore, a plurality of adhesive resin layers may be provided, and the thickness of each layer is preferably 0.5 to 15 μm.
[0114] It should be noted that when glycolic acid (co)polymer resin is used in the above-mentioned intermediate layer (b), the intermediate layer (b) can be 0.1 to 30 μm thick, preferably 0.2 to 10 μm thick, from the perspective of excellent oxygen barrier properties.
[0115] The oxygen permeability (O2TR) of the heat-shrinkable multilayer film used in the present invention is measured in accordance with JIS K7126 using an oxygen permeability tester (MOCON Co., Ltd., "OX-TRAN 2 / 20") at a temperature of 23°C and a relative humidity of 80% on both sides. For example, in the case of packaging raw meat, the oxygen permeability of the heat-shrinkable multilayer film is preferably 1 to 100 cm 3 / m 2 ·day·atm, more preferably 1 to 80cm 3 / m 2 ·day·atm, particularly preferably 1 to 60 cm 3 / m 2 ·day·atm. If the oxygen permeability exceeds 100cm 3 / m 2 ·day·atm, the shelf life is reduced due to oxidative degradation, and in the case of packaged raw meat, there is a tendency that it cannot be stored at 5°C or below for 40 days.
[0116] The heat shrinkable multilayer film of the present invention is punctured from the inner surface layer of the fixed sample at a speed of 50 mm / min using a puncture needle having a hemispherical tip with a radius of curvature of 0.5 mm, and the value obtained by dividing the measured value (N) at the maximum point until the film breaks by the thickness (μm) (puncture strength per unit thickness) is preferably 0.20 to 0.50 N / μm, more preferably 0.22 to 0.45 N / μm, and most preferably 0.30 to 0.40 N / μm. When the puncture strength is less than 0.20 N / μm, especially in the case of a package body with protrusions such as meat with bones or hard food, in order to suppress the occurrence of bag breakage and pinholes caused by impact such as falling, there is a tendency to require a larger thickness, which is not preferred from the viewpoints of cost and film forming properties. When the puncture strength is higher than 0.50 N / μm, the rigidity of the film becomes high, so there is a tendency for bag making properties during secondary processing using the film and opening properties of the package during filling of the content to deteriorate, which is not preferred from the viewpoint of workability.
[0117] The heat-shrinkable multilayer film of the present invention preferably has a hot water shrinkage rate of 40% to 60% in any direction of MD (longitudinal direction) / TD (transverse direction) after being immersed in hot water at a temperature of 80°C for 10 seconds, preferably 43% to 55%. In the case where the hot water shrinkage rate is lower than 40%, there is a tendency that the package cannot fit tightly with the contents and cannot be beautifully packaged, depending on the size or shape of the packaged body. In addition, in the case where the hot water shrinkage rate is higher than 60%, the contents are over-tightened, and there is a tendency that dripping (blood) is easily generated when, for example, meat is packaged.
[0118] The tensile elastic modulus in the TD direction of the heat-shrinkable multilayer film of the present invention is preferably 200 to 600 MPa, more preferably 300 to 550 MPa. When the elastic modulus is less than 200 MPa, there is a tendency for the mechanical adaptability to be poor when the content is filled, and when the elastic modulus is greater than 600 MPa, there is a tendency for the film to be hard and poor in the ability to follow the content. In this specification, the tensile elastic modulus in the TD direction is a value measured by the method described in the examples described later.
[0119] In the case where the heat-shrinkable multilayer film of the present invention contains a polyamide resin, the material recyclability is insufficient due to incompatibility with polyolefin resins. For the above reasons, when a polyamide resin is contained, when the total thickness of all layers is set to 100%, the ratio of the thickness of the layer containing polyamide to the total layers is preferably less than 10%, more preferably less than 5%, and further preferably less than 2%. Polyamide hinders hot water shrinkage, so when the ratio of the thickness of the layer containing polyamide to the total layers is 10% or more, there is a tendency that it is difficult to make the hot water shrinkage rate of the film in the MD (longitudinal direction) or TD (transverse direction) after immersion in hot water at a temperature of 80°C for 10 seconds to be 40% or more.
[0120] As polyamide resins, aliphatic polyamide resins and amorphous aromatic polyamide resins are preferably used. As aliphatic polyamide resins, polyamide 6 (nylon 6) polymers, polyamide 6-66 (nylon 6-66) copolymers, polyamide 6-69 (nylon 6-69) copolymers, polyamide 6-12 (nylon 6-12) copolymers, and polyamide 6-66-12 (nylon 6-66-12) copolymers are preferably used. As amorphous aromatic polyamide resins, for example, polycondensates with aliphatic diamines having isophthalic acid and terephthalic acid as main acid components are used. As the acid component, a mixture containing 40 mol% or more and 98 mol% or less of an isophthalic acid component and 2 mol% or more and 60 mol% or less of a terephthalic acid component is preferably used. In particular, from the viewpoint of versatility, it is preferable to use an amorphous nylon copolymer commonly called nylon 6I-6T (Ny6I-6T), in which the aliphatic diamine is composed solely of hexamethylene.
[0121] When the heat shrinkable multilayer film of the present invention contains a polyester resin, the material recyclability is insufficient due to incompatibility with polyolefin resins. For the above reasons, when the polyester resin is contained, when the total thickness of all layers is set to 100%, the ratio of the thickness of the layer containing polyester to the total layers is preferably less than 10%, more preferably less than 5%, and further preferably less than 2%. If the proportion of the polyester resin is 10% or more, when the heat shrinkable multilayer film is melt-kneaded for material recycling, there is a tendency that the haze value and internal haze value of the recycled sheet increase due to incompatibility with polyolefins.
[0122] As the polyester resin, for example, aliphatic polyester resin and aromatic polyester resin are used. As the dicarboxylic acid component used for the polyester resin, any dicarboxylic acid component that can obtain polyester by a common production method may be used, for example, terephthalic acid, isophthalic acid, dimer acid composed of dimers of unsaturated fatty acids, adipic acid, oxalic acid, malonic acid, succinic acid, azelaic acid, sebacic acid, phthalic acid, 5-tert-butylisophthalic acid, naphthalene dicarboxylic acid, diphenyl ether dicarboxylic acid, cyclohexane dicarboxylic acid, etc., and two or more thereof may be used. In addition, as the diol component used for the polyester resin, any diol component that can obtain polyester by a common production method may be used, for example, ethylene glycol, propylene glycol, tetramethylene glycol, neopentyl glycol, hexanediol, diethylene glycol, polyalkylene glycol, 1,4-cyclohexanedimethanol, 2-alkyl-1,3-propanediol, 1,4-butanediol, etc., and two or more thereof may be used.
[0123] The heat-shrinkable multilayer film of the present invention preferably does not contain an ionomer and an electron beam crosslinked layer. An ionomer is not preferred from the viewpoint of cost, and furthermore, there is a tendency for the puncture strength and elastic modulus per unit thickness to decrease, and the electron beam crosslinked layer gels when melted, thus there is a tendency to hinder the recyclability of the material.
[0124] When the heat-shrinkable multilayer film of the present invention contains an ionomer resin, from the viewpoint of cost and puncture strength per unit thickness, when the total thickness of all layers is set to 100%, the ratio of the thickness of the layer containing the ionomer to the total layers is preferably less than 20%, more preferably less than 10%, and most preferably less than 5%. If the ionomer resin is 20% or more, the puncture strength per unit thickness becomes small, so in the case of a packaging body with protrusions or hard food in circulation packaging, in order to suppress the occurrence of bag breakage and pinholes caused by impact such as falling, there is a tendency to require a larger thickness, which is not preferred from the viewpoint of cost and film forming properties.
[0125] As the ionomer resin, there can be cited: resins obtained by using ethylene-unsaturated carboxylic acid copolymers or ethylene-ethylenically unsaturated carboxylic acid-ethylenically unsaturated carboxylic acid ester terpolymers (preferably ethylene-ethylenically unsaturated carboxylic acid-ethylenically unsaturated carboxylic acid ester terpolymers) as basic polymers and neutralizing the carboxyl groups in these copolymers with cations. As the unsaturated carboxylic acid, methacrylic acid and acrylic acid are preferred, and as the unsaturated carboxylic acid ester, methacrylic acid or acrylic acid alkyl esters having 1 to 6 carbon atoms are preferred. In addition, as the above-mentioned terpolymer, ethylene-methacrylic acid (or acrylic acid)-methacrylic acid alkyl ester (or acrylic acid alkyl ester) such as ethylene-methacrylic acid-isobutyl acrylate is preferred.
[0126] Examples of the cation include: Na + , K + , Li + , Cs + 、Ag + , Hg + , Cu + Mg 2+ 、Zn 2+ 、Be 2+ , Ca 2+ , Ba 2 + , Cu 2+ 、Cd 2+ , Hg 2+ Sn 2+ , Pb 2+ , Fe 2+ 、Co 2+ 、Ni 2+ 、Al 3+ Sc 3+ , Fe 3+ , Y 3+ Among these cations, Na + , K + , Ca 2+ 、Zn 2+ .
[0127] The heat-shrinkable multilayer film of the present invention is characterized in that when the recyclable material thereof is melt-molded for recycling, degradation of the resin (decomposition / gelation) and deterioration of the appearance due to layer separation are suppressed, and the material recyclability is excellent.
[0128] The heat-shrinkable multilayer film of the present invention is kneaded in a melt kneader as it is, and then subjected to a pressure of 150 kgf / cm 2The sheet is formed into a thickness of 70 to 120 μm under a pressure of , and the haze (haze value) of the sheet is preferably 1% to 85% and more preferably 1% to 80% in terms of the value (HA) per 100 μm of sheet thickness. The haze value (HA) in the present invention is preferably smaller. When the haze value (HA) is greater than 85%, the appearance of the material recycling product is damaged.
[0129] Furthermore, the heat-shrinkable multilayer film of the present invention is kneaded in a melt kneader as it is, and then kneaded at 150 kgf / cm using a press. 2 The sheet is formed into a thickness of 70 to 120 μm under a pressure of , and the internal haze value of the sheet is preferably 1% to 80% per 100 μm of sheet thickness (HI), and more preferably 1% to 75%. When the internal haze value (HI) in the present invention is greater than 80%, the compatibility of the resin contained in the sheet may be significantly poor, and there is a tendency for poor mechanical properties.
[0130] Furthermore, in the case of the heat-shrinkable multilayer film of the present invention, it is desirable that the film is kneaded as it is in a melt kneader and then pressed at a pressure of 150 kgf / cm 2 The sheet is formed into a thickness of 70 to 120 μm under pressure, and the yellow hue of the sheet (b * ) value is 1 to 10, more preferably 1 to 8, and most preferably 1 to 6, per 100 μm of sheet thickness. * The value (BY) is preferably smaller, and there is a tendency that the resin decomposes more when the value is larger. * When the value (BY) is larger than 10, the appearance of the material recycled product is impaired.
[0131] It should be noted that the film is kneaded in a melt kneader as it is, and then formed into a sheet.
[0132] Determination of haze (haze value), internal haze value and yellow hue (b * ) value can be listed as follows
[0133] The method described in the examples described below.
[0134] It should be noted that the haze value (HA), internal haze value (HI),
[0135] b * The value (BY) can be calculated using the following formula.
[0136] Haze value per 100 μm (HA) = measured haze value × measured sheet thickness (μm) / 100 Internal haze value per 100 μm (HI) = measured internal haze value × measured sheet thickness (μm) / 100 *Value(BY) = b * Measured value of the value × measured sheet thickness (μm) / 100
[0137] Next, examples of preferred embodiments of the layer constitution of the heat-shrinkable multilayer film of the present invention are shown.
[0138] However, these are only examples, and the present invention is not limited thereto.
[0139] COCDifferent types of COC.
[0140] (1) LLDPE+COC / adhesive resin / EVOH / adhesive resin / LLDPE.
[0141] (2) LLDPE / adhesive resin / EVOH / adhesive resin / LLDPE+COC.
[0142] (3) LLDPE / adhesive resin / EVOH / adhesive resin / LLDPE+COC+COC2.
[0143] (4) LLDPE+COC / adhesive resin / LLDPE / adhesive resin / EVOH / adhesive resin
[0144] Grease / LLDPE.
[0145] (5)LLDPE / adhesive resin / LLDPE+COC / adhesive resin / EVOH / adhesive resin
[0146] Grease / LLDPE.
[0147] (6) LLDPE / adhesive resin / LLDPE / adhesive resin / EVOH / adhesive resin / LLDPE+COC.
[0148] (7)LLDPE / adhesive resin / LLDPE / adhesive resin / EVOH / adhesive resin / LLDPE+COC+COC2.
[0149] (8)LLDPE+COC / adhesive resin / LLDPE+COC / adhesive resin / EVOH / adhesive
[0150] Adhesive resin / LLDPE.
[0151] (9) VLDPE+COC / adhesive resin / EVOH / adhesive resin / VLDPE.
[0152] (10) VLDPE / adhesive resin / EVOH / adhesive resin / VLDPE+COC.
[0153] (11) VLDPE / adhesive resin / EVOH / adhesive resin / VLDPE+COC+COC2.
[0154] (12) VLDPE+COC / adhesive resin / VLDPE / adhesive resin / EVOH / adhesive resin / VLDPE.
[0155] (13) VLDPE / adhesive resin / VLDPE+COC / adhesive resin / EVOH / adhesive resin / VLDPE.
[0156] (14) VLDPE / adhesive resin / VLDPE / adhesive resin / EVOH / adhesive resin / VLDPE+COC.
[0157] (15) VLDPE / adhesive resin / VLDPE / adhesive resin / EVOH / adhesive resin / VLDPE+COC+COC2.
[0158] (16) VLDPE+COC / adhesive resin / VLDPE+COC / adhesive resin / EVOH / adhesive resin / VLDPE.
[0159] (17)LLDPE+COC / adhesive resin / EVA / adhesive resin / EVOH / adhesive resin / LLDPE.
[0160] (18)LLDPE / adhesive resin / EVA / adhesive resin / EVOH / adhesive resin / LLDPE+COC.
[0161] (19)LLDPE / adhesive resin / EVA / adhesive resin / EVOH / adhesive resin / LLDPE+COC+COC2.
[0162] (20) VLDPE+COC / adhesive resin / EVA / adhesive resin / EVOH / adhesive resin / VLDPE.
[0163] (21) VLDPE / adhesive resin / EVA / adhesive resin / EVOH / adhesive resin / VLDPE+COC.
[0164] (22) VLDPE / adhesive resin / EVA / adhesive resin / EVOH / adhesive resin / VLDPE+COC+COC2.
[0165] (23)LLDPE / adhesive resin / LLDPE+COC / adhesive resin / PGA / adhesive resin / LLDPE+COC
[0166] (24)LLDPE+COC / adhesive resin / PGA / adhesive resin / LLDPE.
[0167] (25)LLDPE / adhesive resin / PGA / adhesive resin / LLDPE+COC.
[0168] (26)LLDPE / adhesive resin / PGA / adhesive resin / LLDPE+COC+COC2.
[0169] (27)LLDPE+COC / adhesive resin / LLDPE / adhesive resin / PGA / adhesive resin / LLDPE.
[0170] (28)LLDPE / adhesive resin / LLDPE+COC / adhesive resin / PGA / adhesive resin / LLDPE.
[0171] (29)LLDPE / adhesive resin / LLDPE / adhesive resin / PGA / adhesive resin / LLDPE+COC.
[0172] (30)LLDPE / adhesive resin / LLDPE / adhesive resin / PGA / adhesive resin / LLDPE+COC+COC2.
[0173] (31)LLDPE+COC / adhesive resin / LLDPE+COC / adhesive resin / PGA / adhesive resin / LLDPE.
[0174] (32) VLDPE+COC / adhesive resin / PGA / adhesive resin / VLDPE.
[0175] (33) VLDPE / adhesive resin / PGA / adhesive resin / VLDPE+COC.
[0176] (34) VLDPE / adhesive resin / PGA / adhesive resin / VLDPE+COC+COC2.
[0177] (35) VLDPE+COC / adhesive resin / VLDPE / adhesive resin / PGA / adhesive resin / VLDPE.
[0178] (36) VLDPE / adhesive resin / VLDPE+COC / adhesive resin / PGA / adhesive resin / VLDPE.
[0179] (37) VLDPE / adhesive resin / VLDPE / adhesive resin / PGA / adhesive resin / VLDPE+COC.
[0180] (38)VLDPE / adhesive resin / VLDPE / adhesive resin / PGA / adhesive resin / VLDPE+COC+COC2.
[0181] (39)VLDPE+COC / adhesive resin / VLDPE+COC / adhesive resin / PGA / adhesive resin / VLDPE.
[0182] (40)LLDPE+COC / adhesive resin / EVA / adhesive resin / PGA / adhesive resin / LLDPE.
[0183] (41)LLDPE / adhesive resin / EVA / adhesive resin / PGA / adhesive resin / LLDPE+COC.
[0184] (42)LLDPE / adhesive resin / EVA / adhesive resin / PGA / adhesive resin / LLDPE+COC+COC2.
[0185] (43) VLDPE+COC / adhesive resin / EVA / adhesive resin / PGA / adhesive resin / VLDPE.
[0186] (44) VLDPE / adhesive resin / EVA / adhesive resin / PGA / adhesive resin / VLDPE+COC.
[0187] (45) VLDPE / adhesive resin / EVA / adhesive resin / PGA / adhesive resin / VLDPE+COC+COC2.
[0188] The heat-shrinkable multilayer film of the present invention can be manufactured, for example, by a method comprising the following steps: a step of co-extruding a molten resin into a tube to form a tubular body consisting of at least three layers: an outer surface layer (a) comprising a polyolefin resin, an intermediate layer (b) comprising a gas barrier resin, and an inner surface layer (c) comprising a polyolefin resin; a step of cooling the tubular body to below the melting point of the resin, then reheating the tubular body to a temperature below the melting point of the resin, adding a fluid to the interior of the tubular body while pulling the tubular body out in the longitudinal direction (MD), and stretching it in the longitudinal and transverse directions (TD) to form a biaxially stretched film; and then, folding the biaxially stretched film, then adding a fluid to the interior of the biaxially stretched film while heat treating the biaxially stretched film from the outer surface side, and simultaneously performing a relaxation (shrinkage) treatment in the longitudinal and transverse directions while performing the heat treatment.
[0189] In the step of forming the biaxially stretched film, it is preferred that the portion immediately before stretching in the TD direction ( Figure 1 The surface temperature of the resin of the tubular body at the α position) is 75 to 90°C, and the lower shoulder forming part ( Figure 1The surface temperature of the resin at the β position of the TD direction is 5 to 30° C. lower than the surface temperature of the resin at the portion immediately before stretching in the TD direction.
[0190] More specifically, the heat-shrinkable multilayer film of the present invention can be used, for example Figure 1 The device shown in FIG. Figure 1 In the device shown in, for example, an extruder 1 having a number corresponding to the number of types of laminated resins constituting the multilayer film (only one is shown in the figure) is used to seal an opening agent represented by soybean oil, fatty acid esters of glycerol, propylene glycol, etc. as needed through an annular die head 2, and a tubular body (preform) 3 having an outer surface layer, an intermediate layer and an inner surface layer is co-extruded, and the molten tubular body 3 just after co-extruded is cooled to below the melting point of the main resin occupying each layer by a water bath 4, preferably below 20°C, and more preferably below 15°C, and is flattened by a pressure roller 5 and pulled.
[0191] Next, the pulled out flat body 3a (multilayer film) is sealed with an opening agent represented by soybean oil, fatty acid esters of glycerol, propylene glycol, etc. as needed, and the flat body 3a is introduced into a warm water bath 6 at a temperature below the melting point of the main resin occupying each layer, for example, 75 to 95°C, and the heated flat body 3b is pulled upward.
[0192] Then, by introducing fluid air between a pair of pressure rollers 7 and 8, a bubble-shaped tubular body 3c is formed from the flat body 3b, and while being cooled by a cooling medium blown from an air cooling device at 10 to 30°C and 5 to 20 m / s, biaxial stretching is simultaneously performed in the machine direction (longitudinal direction, MD) and the direction perpendicular to the machine direction (transverse direction, TD).
[0193] At this time, the front part is about to be stretched in the TD direction ( Figure 1 The surface temperature of the tubular body 3c at the α position (α position) is preferably 75 to 90° C., more preferably 80 to 88° C., when measured with an infrared thermal imager (Teledyne FLIR LLC "FLIR E4") with the emissivity set to 0.83. When the surface temperature of the portion immediately before stretching in the TD direction is lower than 75° C., the yield point stress of the tubular body 3c is large, so the internal pressure of the enclosed fluid air becomes high, and thus there is a tendency to be difficult to stretch. When the surface temperature of the portion immediately before stretching in the TD direction is higher than 90° C., there is a tendency to be difficult to stop stretching in the TD direction.
[0194] In addition, the lower shoulder forming portion ( Figure 1 The surface temperature of the portion immediately before stretching in the TD direction ( Figure 1 The temperature of the α position) is cooled by 5 to 30°C, preferably by more than the temperature of the portion immediately before stretching in the TD direction ( Figure 1 The lower shoulder forming portion ( Figure 1 The surface temperature of the β position) is higher than that of the part before the TD direction stretching ( Figure 1 When the temperature is cooled to less than 5°C, the tubular body 3c tends to be easily broken, and when the temperature is cooled to more than 30°C, the width of the tubular body 3c tends to be reduced.
[0195] The stretching ratio is calculated based on the following formula, and is preferably 2.0 to 4.0 times in both directions, more preferably 2.5 to 3.5 times, and particularly preferably 2.8 to 3.5 times.
[0196] Formula 1: Stretch ratio in longitudinal direction (MD) = pulling speed of pressure roller 8 / pulling speed of pressure roller 7 Formula 2: Stretch ratio in transverse direction (TD) = width of flat body 3d / width of flat body 3b
[0197] Next, the stretched flat body 3d is pulled downward, and the fluid air introduced between the pair of pressure rollers 10 and 11 forms a bubble-shaped tubular body 3e again from the flat body 3d, and is held in the heat treatment cylinder 12. Then, steam is blown alone or air and steam are blown together from the blowing port 13 of the heat treatment cylinder 12, and the tubular body 3e being heat-treated is preferably heat-treated at a temperature of 50°C to 100°C, more preferably 60°C to 95°C, for a period of preferably 1 second to 20 seconds, more preferably 1.5 seconds to 10 seconds.
[0198] Then, the tubular body 3e being heat-treated is loosened in the longitudinal direction (MD) and the transverse direction (TD).
[0199] The relaxation rate is set to be 2% or more and 40% or less, preferably 5% or more and 30% or less.
[0200] Relaxation (contraction): The bidirectional relaxation rate is calculated based on the following formula.
[0201] Formula 3: Relaxation rate in longitudinal direction (MD) = (1-(pulling speed of roller 11 / pulling speed of roller 10)) × 100 (%) Formula 4: Relaxation rate in transverse direction (TD) = (1-(width of flat body 3f / width of flat body 3d)) × 100 (%)
[0202] The flat body 3f after such relaxation heat treatment corresponds to the heat-shrinkable multilayer film of the present invention.
[0203] The liquid is wound around the winding roller 14 .
[0204] Example
[0205] Hereinafter, the present invention will be described in more detail based on examples and comparative examples, but the present invention is not limited to
[0206] It is not limited to the following examples.
[0207] The resins used in Examples and Comparative Examples are listed together with their abbreviations in Table 1 below.
[0208] It should be noted that the "0" in the "Remarks" column refers to a polyolefin-based resin in this specification.
[0209] [Table 1]
[0210]
[0211]
[0212] (Example 1)
[0213] Using a blow-up device, the resins were extruded from multiple extruders in a layer structure of LLDPE1 / MA-g-PE / EVA1 / MA-g-PE / EVOH / MA-g-PE / LLDPE1+COC1 (50% by mass + 50% by mass) from the outside to the inside, and the molten resin was introduced into a circular die, where it was melt-bonded and co-extruded in a layer structure as described above. The molten tubular body flowing out of the die outlet was quenched to 10-25°C in a water bath to form a flat body with a flat width of 157 mm and a thickness of 270 μm. Next, the flat body was passed through a warm water bath controlled at 90°C±5°C to form a tubular film in the shape of a bubble, and while being cooled by a cooling medium blown from an air cooler at 20°C and 15 m / s, it was biaxially stretched simultaneously by a blow-up method at a stretch ratio of 2.4 times in the longitudinal direction (MD) and a stretch ratio of 2.8 times in the transverse direction (TD). At this time, the front part is about to be stretched in the TD direction ( Figure 1 The surface temperature of the tubular body at the α position) is 80°C, and the lower shoulder of the tubular body ( Figure 1 The temperature of the β position) is 65°C, which is 15°C lower than the surface temperature of the part just before stretching in the TD direction. Then, the biaxially stretched film is heat-treated by a 360°C IR heat treatment heater while relaxing (shrinking) 3% in the longitudinal direction and 6% in the transverse direction to produce a biaxially stretched film (heat-shrinkable multilayer film). The layer composition of the obtained biaxially stretched film, the thickness (μm) of the whole and each layer, the mass proportion of the polyolefin resin and the cyclic olefin copolymer in the whole, whether it can be stretched by the inflation method, and other embodiments and comparative examples are summarized in Table 2. It should be noted that the "※" in Comparative Example 3 refers to the electron beam cross-linked layer, and the "○" and "×" of "whether it can be stretched" refer to stretchable and non-stretchable, respectively.
[0214] Here, the arithmetic calculation method of the "PO mass ratio (wt%)" and the "COC mass ratio (wt%)" of Example 1 described in Table 2 is shown as an example.
[0215] “PO mass ratio (wt%)”: 95≈(100×(0.903×1.4+0.9×1.0+0.94×20.0+0.9×1.0+0.9×1.0+(0.903×0.5+1.01×0.5)×12.0)) / (0.903×1.4+0.9×1.0+0.94×20.0+0.9×
[0216] 1.0+1.12×1.6+0.9×1.0+(0.903×0.5+1.01×0.5)×12.0))
[0217] “COC mass ratio (wt%)”: 16≈(100×(0.903×0.5+1.01×0.5)×12.0×0.5)) / ((0.903×1.4+0.9×1.0+0.94×20.0+0.9×1.0+1.12×1.6+0.9×1.0+(0.903×0.5+1.01
[0218] ×0.5)×12.0))
[0219] (Examples 2 to 5, Comparative Example 1)
[0220] The same method as in Example 1 was used except that the layer composition was changed as shown in Table 2.
[0221] Various biaxially stretched films (heat-shrinkable multilayer films) were obtained.
[0222] Biaxial stretching by inflation method could not be performed, and a biaxially stretched film (heat-shrinkable multilayer film) could not be obtained.
[0223] (Comparative Example 2)
[0224] Using a blowing device, the layer composition from the outside to the inside is Co-PET / MA-g-PE / PA6+A-PA
[0225] (85 mass% + 15 mass%) / EVOH / MA-g-PE / VLDPE, using multiple extruders
[0226] The resins are extruded separately, and the molten resins are introduced into the annular die, where they are melt-joined and co-extruded in the form of the above-mentioned layer structure. The molten tubular body flowing out of the die outlet is suddenly heated in a water bath.
[0227] After cooling to 20°C, a film-like flat body is formed. Then, the flat body is passed through a warm water bath at 87°C.
[0228] The tubular film in the shape of a bubble is cooled by air cooling at 22°C and then inflated.
[0229] The stretch ratio was 3.0 times in the longitudinal direction (MD) and 3.1 times in the transverse direction (TD).
[0230] Next, the biaxially stretched film is introduced into a heat treatment tower having a tube length of about 2 m to form a tubular film in the shape of a film bubble, and heated by steam blown from a wiping outlet.
[0231] to 70°C, while relaxing (shrinking) it by 6% in the longitudinal direction and 6% in the transverse direction.
[0232] The film was heat-treated to produce a biaxially stretched film (heat-shrinkable multilayer film).
[0233] (Comparative Example 3)
[0234] Use the inflation device to form a layer from the outside to the inside.
[0235] VLDPE / EVA2 / EMA / PVDC / EMA / EVA2 / EVA3 method, using multiple extruders
[0236] The resins are extruded and the molten resins are introduced into an annular die where they are formed into the above-mentioned layer structure.
[0237] The molten tubular body flowing out of the die outlet is quenched in a water bath.
[0238] To 12°C, a flat body was made. Then, in an electron beam irradiation device with an acceleration voltage of 300keV, the flat body was irradiated with electron beams from the outside of the flat body, providing an irradiation dose of 80 kGy. Then, after passing through a warm water bath at 82°C, a tubular body film in the shape of a bubble was made, and while being cooled by air cooling at a temperature of 15°C or more and 20°C or less, biaxial stretching was simultaneously performed by an inflation method at a stretching ratio of 3.1 times in the longitudinal direction (MD) and a stretching ratio of 3.0 times in the transverse direction (TD), thereby producing a biaxially stretched film (heat-shrinkable multilayer film).
[0239] <Evaluation of Heat Shrinkable Multilayer Film>
[0240] The puncture strength, hot water shrinkage, tensile elastic modulus, and material recyclability of the heat-shrinkable multilayer films obtained in the examples and comparative examples were measured by the following methods. The puncture strength was measured from the inner surface layer side of the film. The values obtained by the measurement are shown in Table 2.
[0241] (1) Puncture strength
[0242] According to JIS Z 1707, under an atmosphere of 23°C and 50% RH, a TENSILON universal material testing machine ("RTC-1210 Model" manufactured by ORIENTEC Corporation) equipped with a puncture needle having a hemispherical top portion with a curvature radius of 0.5 mm was used. The puncture needle was punctured from the inner surface layer of the fixed sample at a speed of 50 mm / min, and the value obtained by dividing the measured value (N) at the maximum point until fracture by the thickness (μm) was used as the puncture strength from the inner surface layer side.
[0243] (2) Hot water shrinkage
[0244] The film sample marked with marks at a distance of 10 cm in the machine direction (longitudinal direction, MD) and the direction perpendicular to the machine direction (transverse direction, TD) of the film is immersed in hot water adjusted to 80°C for 10 seconds, then taken out and immediately cooled with water at room temperature (25±5°C). Then, the marked distance is measured, and the ratio of the reduction value from 10 cm to the original length of 10 cm is expressed as a percentage for the longitudinal and transverse directions. Five tests are performed on one sample, and the average values are calculated for the longitudinal direction (MD) and transverse direction (TD) respectively, which are used as the hot water shrinkage rate.
[0245] (3) Tensile elastic modulus
[0246] According to JIS K 7127, a strip-shaped film sample of 20 mm in width and 130 mm in length was attached to a TENSILON universal material testing machine ("RTC-1210 Model" manufactured by ORIENTEC) at 23°C and 50% RH with a chuck spacing of 100 mm, and the film was stretched by 5 mm at a tensile speed of 10 mm / min in the machine direction (longitudinal direction, MD) and the direction perpendicular to the machine direction (transverse direction, TD), and the strain and load at this time were measured. From the obtained strain and load, the tensile modulus of elasticity was calculated according to JIS K 7161.
[0247] (4) Material recyclability
[0248] The heat-shrinkable multilayer films of Examples 1 to 5, Comparative Examples 2 and 3 were placed in a mixing / extrusion molding evaluation test device Labo Plastomill ("4C150 Model" manufactured by Toyo Seiki Seisaku-sho Co., Ltd.), and melt-mixed at a mixer speed of 50 rpm and a mixing time of 3 minutes. After the mixing is completed, 5 g of the molten resin is recovered with a bamboo scraper, etc., and the molten resin is overlapped in the order of a SUS plate with a thickness of 400 μm, a glass fiber cloth sheet impregnated with PTFE with a thickness of 250 μm, 5 g of the molten mixed product, a glass fiber cloth sheet impregnated with PTFE with a thickness of 250 μm, and a SUS plate with a thickness of 400 μm, to prepare a pressing sample. The sample was subjected to a compression (pressing) molding machine ("AYSR.5" manufactured by Kinto Metal Industries) with a preheating time of 1 minute, a pressurizing time of 1 minute, a pressure of 150 kgf / cm 2 The compression molding was performed to form a sheet, and the thickness of each sheet was measured. The results showed that the thickness of Example 1 was 97 μm, that of Example 2 was 110 μm, that of Example 3 was 104 μm, that of Example 4 was 100 μm, that of Example 5 was 83 μm, that of Comparative Example 2 was 84 μm, and that of Comparative Example 3 was 115 μm. As for the temperature during Labo Plastomill and compression molding, the temperature of Examples 1 to 4 and Comparative Example 3 was 190°C, and that of Example 5 and Comparative Example 2 was 240°C. The setting of the temperature is based on the melting point of the resin with the highest melting point contained in the multilayer film, and the reference temperature is preferably above +10°C and below 60°C, more preferably above +15°C and below 50°C, and most preferably above +20°C and below 35°C. If the setting temperature is lower than the reference temperature +10°C, there is a tendency for unmelted resin to remain in the sheet as foreign matter, and if the setting temperature is higher than the reference temperature +60°C, the formed sheet is easily colored due to the decomposition of the resin. It should be noted that the resin with the highest melting point in Examples 1 to 4 is EVOH (157°C), in Example 5 it is PGA (220°C), in Comparative Example 2 it is Co-PET (220°C), and in Comparative Example 3 it is PVDC (160°C). The melting point was measured by DSC (differential scanning calorimeter) at a heating rate of 10°C / min in accordance with JIS K 7121. The haze (haze value) of the obtained sheet was measured using a HazeMeter ("NDH7000" manufactured by Nippon Denshoku Industries Co., Ltd.) and a light source of D65 in accordance with JIS K 7136. In addition, using the same HazeMeter, silicon was coated on the surface of the film to measure the internal haze value. Furthermore, using a Spectrophotometer ("SE7700" manufactured by Nippon Denshoku Industries Co., Ltd.) and a light source of D65, the b value of the obtained sheet was measured by a reflection method in accordance with JIS K 7373 by placing a white board on the sheet. * Value. * The value serves as an indicator of the yellow hue of the film.
[0249] [Table 2]
[0250]
Claims
1. A heat-shrinkable multilayer film, the heat-shrinkable multilayer film being a multilayer film consisting of at least three layers: an outer surface layer (a) comprising a polyolefin resin, an intermediate layer (b) comprising a gas barrier resin, and an inner surface layer (c) comprising a polyolefin resin, A cyclic olefin copolymer is included in at least one layer of the multilayer film, When the total mass of the multilayer film is 100 mass %, the mass ratio of the polyolefin-based resin in the multilayer film is 80 mass % or more, and the mass ratio of the cyclic olefin copolymer in the multilayer film is 15 mass % or more.
2. The heat-shrinkable multilayer film according to claim 1, wherein The polyolefin-based resin in the outer surface layer (a) and / or the inner surface layer (c) includes at least one selected from the group consisting of ultra-low-density polyethylene and linear low-density polyethylene, and a cyclic olefin copolymer.
3. The heat-shrinkable multilayer film according to claim 2, wherein The cyclic olefin copolymer includes any one or both of a cyclic olefin copolymer having a glass transition temperature of 50 to 68°C and a cyclic olefin copolymer having a glass transition temperature of -10 to 20°C.
4. The heat-shrinkable multilayer film according to claim 1, wherein The gas barrier resin of the intermediate layer (b) includes at least one selected from the group consisting of a partially saponified ethylene-vinyl acetate copolymer and a glycolic acid polymer resin or a glycolic acid copolymer resin.
5. The heat-shrinkable multilayer film according to claim 1, wherein The tensile elastic modulus in the transverse direction (TD) is 200 to 600 MPa.
6. A method for producing a heat-shrinkable multilayer film, the method being the method for producing a heat-shrinkable multilayer film according to any one of claims 1 to 4, The surface temperature of the resin just before stretching in the TD direction is 75-90°C. The surface temperature of the resin at the lower shoulder forming portion of the inflated bubble is in the range of 5 to 30° C. lower than the surface temperature of the resin at the portion immediately before stretching in the TD direction.
Citation Information
Patent Citations
Heat-shrinkable multiplayer film
CN1300250A
Wrap film
JP1993051468A
Coextruded heat-shrinkable polyethylene film
JP1996267679A
Heat-shrinkable stretched multilayered film, packaging material using it and package
JP2007160573A
Cycloolefin copolymer heat sealable films
US20050112337A1