Acellular matrix bridle as well as preparation method and application thereof

The decellularized matrix band prepared by lyophilization treatment and braiding cross-linking technology solves the problems of poor elasticity and strong foreign body sense in the prior art, provides vaginal repair materials that are more suitable for patients' needs, and reduces foreign body sense and Painful, improving biocompatibility and anti-degradation properties.

CN118949149APending Publication Date: 2024-11-15SHENZHEN LANDO BIOMATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411183342.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing decellularized matrix biotabelts have poor elasticity after implantation into the vagina, exposed materials, and mismatched with their own soft tissues, resulting in strong foreign body sensation and obvious postoperative pain, and cannot meet the needs of different levels of vaginal relaxation.

Method used

Decellular matrix wires were prepared by lyophilization treatment, and a decellular matrix band with adjustable elasticity was prepared using braiding and cross-linking techniques to reduce the band density, match the patient's soft tissue characteristics, and adapt to different relaxation through different sizes and braiding methods. degree of demand.

Benefits of technology

It improves the elasticity and biocompatibility of the band, reduces the sense of foreign body and pain after implantation, provides more matching mechanical properties, meets the needs of different patients, and achieves more lasting vaginal repair support.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949149A_ABST
    Figure CN118949149A_ABST
Patent Text Reader

Abstract

The invention relates to an acellular matrix bridle as well as a preparation method and application thereof. The invention relates to a preparation method of an acellular matrix band, which comprises the following steps: providing an acellular matrix of a mammal tissue, and carrying out freeze-drying treatment on the acellular matrix to prepare a freeze-dried acellular matrix; preparing the freeze-dried acellular matrix into a wire rod; weaving the wire rod to prepare a prefabricated bridle; and cross-linking the prefabricated band with a cross-linking agent to prepare the acellular matrix band. According to the application, the acellular matrix is firstly processed into the wires and then woven, so that the structure of the acellular matrix bridle is looser, the density of the bridle is reduced, the elasticity is better, the foreign body sensation after the bridle is implanted into the vagina is reduced, the pain of a patient is reduced, the wires with different sizes can be adopted and woven in different modes, and the cost is reduced. And therefore, the decellularized matrix bridle with better matched mechanical properties is provided for patients with different vagina relaxation degrees.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of bionic materials, and in particular to a decellularized matrix belt and a preparation method and application thereof. Background Art

[0002] The vagina, bladder, uterus, rectum and other organs are supported and supported by the pelvic floor muscles. Due to childbirth and other reasons, the pelvic floor muscles and pelvic floor tissues are damaged, or the pelvic floor tissues relax due to aging and decreased estrogen levels, which reduces and shallows the vaginal mucosal folds, resulting in a wide and loose vagina. According to statistics, the incidence of vaginal relaxation in female urology clinics is as high as 24%. For women after childbirth, the incidence of vaginal relaxation is as high as 60.7%. The incidence of simple vaginal relaxation is high and the rate of seeking medical treatment is low. There are many ways to evaluate the degree of vaginal relaxation, among which the finger measurement method has the highest recognition: the vagina can be inserted 2 horizontal fingers for normal, 2-3 fingers for mild relaxation, 3-4 fingers for moderate relaxation, and 4 fingers and above for severe relaxation. Patients with different degrees of relaxation have different pelvic floor muscle strength, and the treatment methods for vaginal relaxation are also different.

[0003] The traditional treatment for vaginal relaxation is to remove part of the vaginal soft tissue and then suture it to make the vagina tighter. This method is very traumatic, causes a lot of bleeding during the operation, is prone to recurrence after the operation, and has low patient satisfaction.

[0004] Compared with traditional surgery, vaginal tightening with biological bands is a better alternative. Vaginal tightening with biological bands only requires openings at the 3 o'clock and 9 o'clock positions of the vaginal opening, implanting the biological band into the vagina, and tightening the band to complete the vaginal tightening. The above method has a short operation time, less intraoperative bleeding, and higher patient satisfaction. Therefore, the number of patients choosing the above method for treatment is also increasing year by year.

[0005] Acellular matrix materials have become the most commonly used bio-band materials in clinical practice because of their many advantages such as good biocompatibility and high mechanical strength. However, it has been found clinically that after being implanted into the vagina, problems such as poor elasticity, material exposure, and mismatch between mechanical properties and self-soft tissues will occur, resulting in strong foreign body sensation in patients and obvious postoperative pain. In addition, the existing bio-band products cannot meet the needs of patients with different degrees of relaxation due to their single preparation and molding methods. Therefore, it is very important to improve the performance of bio-band products based on acellular matrix. For example, CN115281884A provides an elastic tight band for vaginal tightening, which is prepared from elastomers such as silicone rubber / polyurethane, needs to be fixed by a traction line, has poor material touch, strong foreign body sensation, and a complicated preparation process, which is inconvenient for clinical operation. CN215080256U provides a bio-band for vaginal tightening and pelvic floor muscle relaxation repair, which is prepared by acellular allogeneic dermis, has limited material collection, and a single processing and molding method, and cannot adapt to patients with different needs. Summary of the invention

[0006] Based on this, the present application provides a method for preparing an acellular matrix band, which can be processed and formed in different ways to meet the needs of patients. The prepared acellular matrix band has good elasticity and is adjustable, which is more compatible with the patient's own soft tissue and can reduce the foreign body sensation after implantation.

[0007] Furthermore, the present application also provides a decellularized matrix belt.

[0008] Furthermore, the present application also provides a use of a decellularized matrix band in the preparation of a vaginal tightening biological band product.

[0009] The present application provides a method for preparing an acellular matrix belt, comprising the following steps:

[0010] Providing a decellularized matrix of mammalian tissue, and freeze-drying the decellularized matrix to prepare a freeze-dried decellularized matrix;

[0011] preparing the freeze-dried decellularized matrix into wire;

[0012] Weaving the wires to prepare a prefabricated strap; and

[0013] The prefabricated band is cross-linked with a cross-linking agent to prepare an acellular matrix band.

[0014] In some of these embodiments, the freeze-drying conditions meet one or more of the following conditions: the freeze-drying temperature is -30°C to -50°C, and the freeze-drying time is 24 h to 48 h;

[0015] and / or, the processing method of preparing the freeze-dried decellularized matrix into wires includes one or more of cutting and forming, filament twisting, and mechanical stretching;

[0016] And / or, the diameter of the wire is 0.1 mm to 3 mm;

[0017] And / or, the weaving method includes one or more of hexagonal weaving, three-twist weaving, five-twist weaving and plain weaving.

[0018] In some embodiments, the step of cross-linking the prefabricated band with a cross-linking agent comprises:

[0019] The prefabricated belt is immersed in a solution containing the cross-linking agent.

[0020] In some embodiments, the prefabricated band is immersed in a solution containing the cross-linking agent to meet one or more of the following conditions:

[0021] (1) The cross-linking agent includes one or more of glutaraldehyde, formaldehyde, butanediol diglycidyl ether and genipin;

[0022] (2) In the solution containing the cross-linking agent, the mass percentage concentration of the cross-linking agent is 0.1% to 5%;

[0023] (3) The soaking time is 4h~48h.

[0024] In some embodiments, the steps of preparing the decellularized matrix of mammalian tissue include:

[0025] placing the mammalian tissue in an alkaline solution for alkaline soaking to prepare an alkaline-soaked mammalian tissue; and

[0026] The mammalian tissue after alkali soaking is placed in an acidic solution for acid soaking to prepare the decellularized matrix.

[0027] In some embodiments, the alkaline soaking satisfies one or more of the following conditions:

[0028] (1) The alkali in the alkaline solution includes one or more of sodium hydroxide and potassium hydroxide;

[0029] (2) The mass percentage concentration of the alkali in the alkaline solution is 0.3% to 10%;

[0030] (3) The alkali soaking time is 4h~24h;

[0031] And / or, the acid soaking meets one or more of the following conditions:

[0032] (1) The acid in the acidic solution includes one or more of hydrochloric acid, lactic acid, citric acid and acetic acid;

[0033] (2) The mass percentage concentration of the acid in the acidic solution is 1% to 8%;

[0034] (3) The acid soaking time is 4h~24h.

[0035] In some embodiments, the tissue site of the mammalian tissue is selected from one or more of skin, pericardium and peritoneum.

[0036] In some embodiments, the mammalian tissue is derived from one or more of pigs, cows and sheep.

[0037] In some embodiments, before the step of preparing the decellularized matrix, the following step of pretreating the mammalian tissue is also included:

[0038] washing the mammalian tissue; and

[0039] The washed mammalian tissue is freed of fat.

[0040] The present application also provides a decellularized matrix belt, which is prepared by the preparation method described in any of the above embodiments.

[0041] The present application also provides the use of the acellular matrix band described in any of the above embodiments in the preparation of a vaginal tightening biological band product.

[0042] The present application provides a method for preparing an acellular matrix band, wherein the acellular matrix is ​​first freeze-dried and solidified, and then the acellular matrix is ​​made into a relatively soft and easy-to-process wire, and then the wire is woven to form a prefabricated band, and finally a cross-linking agent is used to cross-link the prefabricated band to obtain the band. Compared with the sheet material formed by the traditional natural acellular matrix solidification, the method of first processing the acellular matrix into a wire and then weaving it can make the structure of the acellular matrix band looser, thereby reducing the density of the band and having better elasticity, which is conducive to reducing the foreign body sensation after implantation in the vagina and reducing the pain of the patient. Moreover, wires of different sizes can be used and woven in different ways to achieve elastic adjustment of the band, thereby providing a acellular matrix band with better matching mechanical properties for patients with different degrees of vaginal relaxation. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 A process roadmap for preparing acellular matrix belts in some embodiments;

[0044] Figure 2 This is a schematic diagram of the structure of the acellular matrix belt prepared in Example 1;

[0045] Figure 3 This is a schematic diagram of the structure of the acellular matrix belt prepared in Example 2;

[0046] Figure 4 This is a schematic diagram of the structure of the decellularized matrix belt prepared in Example 3. DETAILED DESCRIPTION

[0047] For ease of understanding of the present application, the present application will be described more comprehensively below in conjunction with embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described in the present application. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0048] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items.

[0049] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0050] In the description of the present application, “plurality” means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.

[0051] In the present application, the terms “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of the present application.

[0052] In the present application, the terms “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.

[0053] In this application, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0054] In this application, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, as well as each numerical value between the two numerical endpoints. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.

[0055] like Figure 1 As shown, the present application provides a method for preparing a decellularized matrix belt, comprising the following steps S100 to S600.

[0056] Step S100: pre-treating the mammalian tissue. The pre-treatment can obtain relatively clean mammalian tissue, which is beneficial for subsequent decellularization treatment.

[0057] In some embodiments, the tissue site of the mammalian tissue is selected from one or more of skin, pericardium and peritoneum. Further, the mammalian tissue is derived from one or more of pigs, cattle and sheep. The raw materials of the above-mentioned mammalian tissues are very easy to obtain, which provides an important basis for the smooth progress of the subsequent preparation process.

[0058] The specific preprocessing steps include step S110 to step S120.

[0059] Step S110: Washing the mammalian tissue may be performed with running water, and the number of washing times may be, but is not limited to, 2 to 4 times.

[0060] Step S120: removing fat from the washed mammalian tissue. The fat removal method may be, for example but not limited to, scraping.

[0061] Step S200: Decellularize the pretreated mammalian tissue to prepare a decellularized matrix. The decellularized matrix prepared by decellularization removes the cellular components in the mammalian tissue while retaining the original three-dimensional structure and functional proteins has good biocompatibility. The specific decellularization steps include steps S210 to S220.

[0062] Step S210: placing the mammalian tissue in an alkaline solution for alkaline soaking to prepare the alkaline-soaked mammalian tissue.

[0063] In some embodiments, the alkali in the alkaline solution includes one or more of sodium hydroxide and potassium hydroxide.

[0064] In some embodiments, the mass percentage concentration of the alkali in the alkaline solution is 0.3% to 10%.

[0065] In some embodiments, the alkali soaking time is 4h~24h.

[0066] Step S220: placing the mammalian tissue after alkali soaking in an acid solution for acid soaking to prepare a decellularized matrix.

[0067] In some embodiments, the acid in the acidic solution includes one or more of hydrochloric acid, lactic acid, citric acid and acetic acid;

[0068] In some embodiments, the mass percentage concentration of the acid in the acidic solution is 1% to 8%.

[0069] In some embodiments, the acid soaking time is 4h~24h.

[0070] In some of the embodiments, after step S220, step S230 may be further included.

[0071] Step S230: Cleaning the acid-soaked mammalian tissue.

[0072] The cleaning step may include, for example, soaking in sodium chloride and sodium bicarbonate in sequence.

[0073] Step S300: freeze-drying the decellularized matrix to prepare a freeze-dried decellularized matrix. The freeze-drying process can solidify the decellularized matrix into a shape to facilitate subsequent processing.

[0074] In some embodiments, the freeze-drying conditions meet one or more of the following conditions:

[0075] The freeze-drying temperature is -30℃~-50℃, and the freeze-drying time is 24 h~48 h.

[0076] Step S400: Processing the freeze-dried decellularized matrix into a wire. The wire is relatively soft and easy to braid later.

[0077] In some embodiments, the processing method of making the freeze-dried decellularized matrix into a wire includes one or more of cutting and forming, filament twisting, and mechanical stretching. Through a variety of different processing methods, wires with different mechanical properties can be made, which is conducive to adjusting the elasticity of the band. It can be understood that in other embodiments, other methods can also be used to make the freeze-dried decellularized matrix into a wire.

[0078] In some embodiments, the diameter of the wire is 0.1 mm to 3 mm. The wire within the above diameter range is easy to braid and process, not easy to break, and is conducive to controlling the density of the final prepared band material within a lower range, thereby reducing the foreign body sensation after implantation.

[0079] Step S500: braiding the wires to prepare a prefabricated strap.

[0080] In some embodiments, the weaving method includes one or more of hexagonal weaving, three-twist weaving, five-twist weaving and plain weaving. According to different needs, different weaving methods can be used to make the prepared prefabricated straps have different densities, thereby achieving adjustment of the strap elasticity.

[0081] In some embodiments, the prefabricated band has a width of 0.5 cm to 4.0 cm and a length of 10 cm to 30 cm. The band of the above size is suitable for vaginal implantation.

[0082] Step S600: cross-linking the prefabricated band with a cross-linking agent to prepare an acellular matrix band. The braided prefabricated band is cross-linked with a cross-linking agent to obtain an acellular matrix band with better anti-degradation performance, which can provide a more durable vaginal repair support effect. The step of cross-linking the prefabricated band with a cross-linking agent includes S610.

[0083] Step S610: soaking the prefabricated strap in a solution containing a cross-linking agent.

[0084] In some embodiments, the crosslinking agent includes one or more of glutaraldehyde, formaldehyde, butanediol diglycidyl ether and genipin. The crosslinking agent can perform efficient crosslinking reaction with the decellularized matrix.

[0085] In some embodiments, the mass percentage concentration of the crosslinking agent in the solution containing the crosslinking agent is 0.1% to 5%. Within the above suitable concentration range, the crosslinking agent can efficiently and fully crosslink the decellularized matrix, while also avoiding the increase of the cytotoxicity of the band due to excessively high concentration of the crosslinking agent, which is beneficial to improving biocompatibility.

[0086] In some embodiments, the immersion time is 4h~48h. If the immersion time is too short, the cross-linking is not sufficient, and the material's anti-degradation performance is poor. If the immersion time is too long, excessive cross-linking will occur, thereby increasing cytotoxicity. It is best to control the immersion cross-linking time within 4h~48h.

[0087] In some of the embodiments, step S620 is further included after step S610.

[0088] Step S620: cleaning and sterilizing the cross-linked acellular matrix band.

[0089] Furthermore, the cleaning method may be, for example, water injection cleaning, and the number of cleaning times may be, for example but not limited to, 6 to 8 times.

[0090] Furthermore, the sterilization method may be, for example, irradiation sterilization, and the irradiation dose may be, for example but not limited to, 20 KGy to 25 KGy.

[0091] The present application provides a method for preparing an acellular matrix band, wherein the acellular matrix is ​​first freeze-dried and solidified, and then the acellular matrix is ​​made into a relatively soft and easy-to-process wire, and then the wire is woven to form a prefabricated band, and finally a cross-linking agent is used to cross-link the prefabricated band to obtain a band. Compared with the sheet material formed by the solidification of the traditional natural acellular matrix, the method of first processing the acellular matrix into a wire and then weaving it can make the structure of the acellular matrix band looser, thereby reducing the density of the band and having better elasticity, which is conducive to reducing the foreign body sensation after implantation in the vagina and reducing the pain of the patient. Moreover, wires of different sizes can be used and woven in different ways to achieve elastic adjustment of the band, thereby providing a more matched acellular matrix band with mechanical properties for patients with different degrees of vaginal relaxation. The acellular matrix is ​​taken from mammalian tissue, which is convenient to obtain and is conducive to reducing the preparation cost. Moreover, after weaving and cross-linking, the prepared band has excellent biocompatibility and anti-degradation properties, which can provide patients with more lasting vaginal repair support.

[0092] The present application also provides a decellularized matrix belt, which is prepared by the preparation method in any of the above embodiments.

[0093] The present application also provides the use of the acellular matrix band in any of the above embodiments in the preparation of a vaginal tightening biological band product.

[0094] The present application is further described in detail below through specific examples. The following examples are more specific, and it can be understood that in other embodiments, it is not limited thereto. In the following specific examples, the instruments, reagents, and materials involved, unless otherwise specified, are conventional instruments, reagents, and materials already available in the prior art, and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following embodiments, unless otherwise specified, are conventional experimental methods and detection methods already available in the prior art.

[0095] Example 1

[0096] A method for preparing an acellular matrix belt comprises the following steps:

[0097] (1) Pretreatment: Take fresh porcine dermis as mammalian tissue, rinse it with purified water for 4 times, and then use a mechanical method to scrape off excess fat on the skin surface for later use.

[0098] (2) Decellularization: The mammalian tissue pretreated in step (1) is first placed in a sodium hydroxide solution with a mass percentage concentration of 4% for alkaline immersion for 8 hours to prepare an alkaline-immersed mammalian tissue; then the mammalian tissue after alkaline immersion is placed in a hydrochloric acid solution with a mass percentage concentration of 1% for acid immersion for 24 hours to obtain a decellularized matrix.

[0099] (3) Freeze-drying: The decellularized matrix prepared in step (2) is freeze-dried. The freeze-drying conditions include: a freeze-drying temperature of -45°C and a freeze-drying time of 30 h to prepare a freeze-dried decellularized matrix.

[0100] (4) Preparation of wires: The freeze-dried decellularized matrix prepared in step (3) was physically cut into thin wires with a length of 50 cm and a width of 1 mm. Three thin wires were twisted into one to make a wire with a diameter of 3 mm.

[0101] (5) Weaving: The wire prepared in step (4) is hexagonally woven into a pattern such as Figure 2 As shown, after weaving is completed, it is cut into prefabricated straps with a width of 1.5 cm and a length of 20 cm.

[0102] (6) Cross-linking: The prefabricated band prepared in step (5) is immersed in a glutaraldehyde solution having a mass percentage concentration of 2% to allow the prefabricated band to be cross-linked with the glutaraldehyde cross-linking agent. The immersion time is 10 hours to prepare a decellularized matrix band.

[0103] (7) The decellularized matrix band of step (6) is cleaned 4 times with injection water, and then the cleaned decellularized matrix band is packaged and sterilized by irradiation with an irradiation dose of 20-25 KGy.

[0104] Example 2

[0105] A method for preparing an acellular matrix belt comprises the following steps:

[0106] (1) Pretreatment: Take fresh sheep peritoneal tissue as mammalian tissue, rinse it twice with purified water, and then use a mechanical method to scrape off excess fat on the peritoneal surface for later use.

[0107] (2) Decellularization: The mammalian tissue pretreated in step (1) is first placed in a 2% by mass potassium hydroxide solution for alkaline immersion for 12 hours to prepare an alkaline-immersed mammalian tissue; then the alkaline-immersed mammalian tissue is placed in a 1% by mass hydrochloric acid solution for acid immersion for 24 hours; the acid-immersed mammalian tissue is placed in a 1% by mass sodium chloride solution for immersion for 24 hours, and then the sodium chloride-immersed mammalian tissue is placed in a 1% by mass sodium bicarbonate solution for immersion for 24 hours to obtain a decellularized matrix.

[0108] (3) Freeze-drying: freeze-drying the decellularized matrix prepared in step (2). The freeze-drying conditions include: freeze-drying temperature of -30°C and freeze-drying time of 40 h to prepare a freeze-dried decellularized matrix.

[0109] (4) Preparation of wires: The freeze-dried decellularized matrix prepared in step (3) was physically cut into thin wires with a length of 50 cm and a width of 0.5 mm. Three thin wires were twisted into one to make a wire with a diameter of 1.5 mm.

[0110] (5) Weaving: The wire prepared in step (4) is hexagonally woven into a pattern such as Figure 3 As shown, after weaving is completed, it is cut into prefabricated straps with a width of 1.5 cm and a length of 20 cm.

[0111] (6) Cross-linking: The prefabricated band prepared in step (5) is immersed in a glutaraldehyde solution having a mass percentage concentration of 2% to allow the prefabricated band to be cross-linked with the glutaraldehyde cross-linking agent. The immersion time is 10 hours to prepare a decellularized matrix band.

[0112] (7) The decellularized matrix band of step (6) is cleaned 4 times with injection water, and then the cleaned decellularized matrix band is packaged and sterilized by irradiation with an irradiation dose of 20-25 KGy.

[0113] Example 3

[0114] A method for preparing an acellular matrix belt comprises the following steps:

[0115] (1) Pretreatment: Take fresh bovine skin tissue as mammalian tissue, rinse it with purified water for 4 times, and then use a mechanical method to scrape off excess fat on the surface of the dermis tissue for later use.

[0116] (2) Decellularization: The mammalian tissue pretreated in step (1) is first placed in a 4% by mass potassium hydroxide solution for alkaline immersion for 6 hours to prepare an alkaline-immersed mammalian tissue; then the alkaline-immersed mammalian tissue is placed in a 2% by mass hydrochloric acid solution for acid immersion for 24 hours; the acid-immersed mammalian tissue is placed in a 1% by mass sodium chloride solution for immersion for 24 hours, and then the sodium chloride-immersed mammalian tissue is placed in a 1% by mass sodium bicarbonate solution for immersion for 24 hours to obtain a decellularized matrix.

[0117] (3) Freeze-drying: freeze-drying the decellularized matrix prepared in step (2). The freeze-drying conditions include: freeze-drying temperature of 50° C. and freeze-drying time of 48 h to prepare a freeze-dried decellularized matrix.

[0118] (4) Preparation of wires: The freeze-dried decellularized matrix prepared in step (3) was physically cut into filaments with a length of 50 cm and a width of 3 mm to prepare wires with a diameter of 3 mm.

[0119] (5) Weaving: The wire prepared in step (4) is flat-woven, and the weaving pattern is as follows: Figure 4 As shown, after weaving is completed, it is cut into prefabricated straps with a width of 1.5 cm and a length of 20 cm.

[0120] (6) Cross-linking: The prefabricated band prepared in step (5) is immersed in a 1,4-butanediol diglycidyl ether solution having a mass percentage concentration of 5%, so that the prefabricated band is cross-linked with the 1,4-butanediol diglycidyl ether cross-linking agent. The immersion time is 16 hours to prepare a decellularized matrix band.

[0121] (7) The decellularized matrix band of step (6) is cleaned 6 times with injection water, and then the cleaned decellularized matrix band is packaged and sterilized by irradiation with an irradiation dose of 20-25 KGy.

[0122] Comparative Example 1

[0123] The method is substantially the same as Example 1, except that the decellularized matrix is ​​not woven. Specifically:

[0124] A method for preparing an acellular matrix belt comprises the following steps:

[0125] (1) Pretreatment: Take fresh porcine dermis as mammalian tissue, rinse it with purified water for 4 times, and then use a mechanical method to scrape off excess fat on the skin surface for later use.

[0126] (2) Decellularization: The mammalian tissue pretreated in step (1) is first placed in a sodium hydroxide solution with a mass percentage concentration of 4% for alkaline immersion for 8 hours to prepare an alkaline-immersed mammalian tissue; then the mammalian tissue after alkaline immersion is placed in a hydrochloric acid solution with a mass percentage concentration of 1% for acid immersion for 24 hours to obtain a decellularized matrix.

[0127] (3) Freeze-drying: The decellularized matrix prepared in step (2) is freeze-dried. The freeze-drying conditions include: a freeze-drying temperature of -45°C and a freeze-drying time of 30 h. The freeze-dried decellularized matrix is ​​prepared and cut into pieces with a width of 1.5 cm and a length of 20 cm.

[0128] (4) Cross-linking: The freeze-dried decellularized matrix prepared in step (3) is immersed in a glutaraldehyde solution having a mass percentage concentration of 2% to allow the freeze-dried decellularized matrix to be cross-linked with the glutaraldehyde cross-linking agent. The immersion time is 10 hours to prepare a decellularized matrix band.

[0129] (5) The decellularized matrix band of step (4) is cleaned 4 times with injection water, and then the cleaned decellularized matrix band is packaged and sterilized by irradiation with an irradiation dose of 20-25 KGy.

[0130] The performance of the acellular matrix belts prepared in Examples 1 to 3 and Comparative Example 1 was tested, and the test results are shown in Table 1 below.

[0131] Table 1 Test results of acellular matrix band performance

[0132]

[0133] The acellular matrix band used for vaginal relaxation needs to have a large maximum tensile force and a high elongation at break, and has a strong pulling and maintaining effect and elasticity on the relaxed vaginal muscle layer and soft tissue. According to different degrees of vaginal relaxation, the maximum force and elongation at break are in the range of 30~120N and 130%~300%, respectively. It can be seen from Table 1 that the maximum tensile force of the acellular matrix prepared in Example 1 to Example 3 and Comparative Example 1 is 52N, 48N, 86N and 80N, respectively, and the elongation at break is 160%, 193%, 132% and 82%, respectively. Bands with different elasticity that meet clinical needs can be prepared by different weaving methods.

[0134] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0135] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of this application. Therefore, the protection scope of the patent of this application shall be subject to the attached claims.

Claims

1. A method for preparing an acellular matrix belt, It is characterized in that The steps include: Providing a decellularized matrix of mammalian tissue, and freeze-drying the decellularized matrix to prepare a freeze-dried decellularized matrix; preparing the freeze-dried decellularized matrix into wire; Weaving the wires to prepare a prefabricated strap; as well as The prefabricated band is cross-linked with a cross-linking agent to prepare an acellular matrix band.

2. The method for preparing the acellular matrix belt according to claim 1, It is characterized in that The freeze-drying conditions meet one or more of the following conditions: freeze-drying temperature is -30°C to -50°C, and freeze-drying time is 24 h to 48 h; and / or, the processing method of preparing the freeze-dried decellularized matrix into wires includes one or more of cutting and forming, filament twisting, and mechanical stretching; And / or, the diameter of the wire is 0.1 mm to 3 mm; And / or, the weaving method includes one or more of hexagonal weaving, three-twist weaving, five-twist weaving and plain weaving.

3. The method for preparing the acellular matrix belt according to claim 1, It is characterized in that The step of cross-linking the prefabricated strap with a cross-linking agent comprises: The prefabricated belt is immersed in a solution containing the cross-linking agent.

4. The method for preparing the acellular matrix belt according to claim 3, It is characterized in that The prefabricated strap is immersed in a solution containing the cross-linking agent to meet one or more of the following conditions: (1) The cross-linking agent includes one or more of glutaraldehyde, formaldehyde, butanediol diglycidyl ether and genipin; (2) In the solution containing the cross-linking agent, the mass percentage concentration of the cross-linking agent is 0.1% to 5%; (3) The soaking time is 4h~48h.

5. The method for preparing the acellular matrix belt according to any one of claims 1 to 4, It is characterized in that The steps of preparing the decellularized matrix of mammalian tissue include: placing the mammalian tissue in an alkaline solution for alkaline soaking to prepare an alkaline-soaked mammalian tissue; and The mammalian tissue after alkali soaking is placed in an acidic solution for acid soaking to prepare the decellularized matrix.

6. The method for preparing the acellular matrix belt according to claim 5, It is characterized in that Alkaline soaking meets one or more of the following conditions: (1) The alkali in the alkaline solution includes one or more of sodium hydroxide and potassium hydroxide; (2) The mass percentage concentration of the alkali in the alkaline solution is 0.3% to 10%; (3) The alkali soaking time is 4h~24h; And / or, the acid soaking meets one or more of the following conditions: (1) The acid in the acidic solution includes one or more of hydrochloric acid, lactic acid, citric acid and acetic acid; (2) The mass percentage concentration of the acid in the acidic solution is 1% to 8%; (3) The acid soaking time is 4h~24h.

7. The method for preparing the acellular matrix belt according to any one of claims 1 to 4 and 6, It is characterized in that The tissue site of the mammalian tissue is selected from one or more of skin, pericardium and peritoneum; Optionally, the mammalian tissue originates from one or more of pigs, cows and sheep.

8. The method for preparing the acellular matrix belt according to any one of claims 1 to 4 and 6, It is characterized in that Before the step of preparing the decellularized matrix, the method further includes the following step of pretreating the mammalian tissue: washing the mammalian tissue; and The washed mammalian tissue is freed of fat.

9. An acellular matrix belt, It is characterized in that The method is prepared according to any one of claims 1 to 8.

10. Use of the acellular matrix band according to claim 9 in the preparation of a vaginal tightening biological band product.

Citation Information

Cited By

  • Acellular matrix fiber woven scaffold as well as preparation method and application thereof

    CN121971707A