Preparation method of graphene oxide composite film with self-supporting sponge-like hole structure

Hydrophilic carbon nanofibers were prepared by electrospinning and combined with dopamine hydrochloride to form a graphene oxide composite film with a self-supporting sponge pore structure, which solved the problem of insufficient permeability and bending performance of graphene oxide films and achieved high efficiency oil-water separation effect.

CN118949708AActive Publication Date: 2024-11-15NANTONG UNIV

Patent Information

Application Number
CN202411010517.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Graphene oxide films have poor permeability and poor bending performance in the field of water treatment, and cannot be effectively applied in the field of oil-water separation.

Method used

Hydrophilic carbon nanofibers were prepared by electrospinning, and a graphene oxide composite film with self-supporting sponge pore structure was formed by vacuum suction filtration and high-temperature calcination. Dopamine hydrochloride was used as a binder to enhance the bending resistance of the film. Performance and permeability.

Benefits of technology

The bending resistance and water permeability of the graphene oxide composite film are improved, and the self-supported oil-water separation effect is achieved, and it is easy to operate, environmentally friendly and pollution-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949708A_ABST
    Figure CN118949708A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: preparing silicon-doped carbon nanofibers, preparing a graphene oxide / silicon-doped carbon nanofiber dispersion liquid, carrying out vacuum filtration to form a film, drying the film at room temperature to form the film, and carrying out high-temperature calcination in an air atmosphere to remove a mixed cellulose substrate film, so as to obtain the self-supporting sponge-like-hole-structure graphene oxide composite film. The silicon-doped carbon nanofiber / graphene oxide composite film is easy to operate, low in cost, efficient, free of additional modification chemical reagents, environmentally friendly and free of pollution. A carbon nanofiber intercalation layer is inserted into graphene oxide to form a composite film by adopting vacuum filtration, and a self-polymerization effect is adopted, so that the combination of the carbon nanofiber / graphene oxide film is tighter, the mechanical property of the composite film is enhanced, a sponge-like hole structure is formed, and the water channel and permeation flux of the graphene oxide composite film are increased; the carbon nanofiber / graphene oxide composite film can be self-supported through high-temperature calcination, and a thought is provided for preparing the self-supporting graphene oxide film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil-water separation membrane preparation, and specifically relates to a method for preparing a self-supporting sponge-like pore structured graphene oxide composite film. Background Art

[0002] Currently, there are several methods for wastewater purification, such as adsorption combustion, membrane separation and photocatalytic degradation. Among them, membrane separation has been proven to be one of the most promising methods for effectively treating wastewater due to its advantages of high efficiency, no secondary pollution and easy operation. Graphene oxide (GO) is a two-dimensional sheet formed by oxidation and exfoliation of graphite materials. It has oxygen-containing functional groups on the basal surface and the edge, so it is hydrophilic and has high chemical activity. The stacked pure GO membrane traditionally made by a simple solution filtration method has a smooth and dense laminated structure, but it is not directly suitable for water separation because GO nanosheets are extremely hydrophilic and easy to break; and the channels of GO-based membranes are usually too narrow to achieve high permeation flux. Therefore, how to improve the shortcomings of GO-based membranes in the field of water treatment so that they can be effectively applied in the field of oily wastewater treatment is one of the keys to the research of graphene oxide membranes in the field of water treatment.

[0003] In recent years, in order to achieve efficient separation of GO-based membranes, researchers have done some research on how to couple GO-based membranes with nanomaterials to synergistically regulate the channel structure of water transmission and enhance the stability of the membrane. The document "SWCNT-intercalated GO ultrathin films for ultrafast separation of molecules. J. Master. Chem. A, 2015, 36649-6654" reported that a single-walled carbon nanotube intercalated GO-based film was prepared by vacuum filtration to achieve fast water transmission. However, although the GO membrane intercalated with nanomaterials reported in the above document can improve the permeation flux of pure GO membrane, over time, the GO on the membrane surface may be lost, resulting in a decrease in membrane performance, and the above membrane is actually not stable enough to be reused. The document "One-step preparation of GO / SiO2 membrane for highly efficient separation of oil-in-water emulsion, Journal of Membrane Science, 2018, 0376-7388" reported the preparation of GO / SiO2 membrane by vacuum filtration. 2 However, the GO / SiO composite membranes reported in the above literature 2 SiO in the film 2The dispersion process will have problems with uniformity, which will affect the stability of the composite film and the spacing between GO layers, thus affecting the GO / SiO 2 In addition, the composite membrane is a non-self-supporting membrane, and the separation process relies on the mixed cellulose substrate membrane, which is not conducive to the separation of GO / SiO 2 further promotion and application.

[0004] Self-supporting GO is of great significance for oil-water separation. Foreign patent KR1020230084575A discloses a method for preparing a self-supporting graphene oxide or reduced graphene oxide (rGO) film. The method is carried out by depositing an aqueous dispersion containing GO or rGO on a flat substrate of a polymer film that is soluble in an organic solvent and insoluble in water, and finally pickling the polymer film with an organic solvent to dissolve the polymer film to obtain a self-supporting GO film. However, the preparation method of this patent is complicated and dangerous to operate, and polymer molecules will be adsorbed during the dissolution of the polymer film. The use of organic solvents and acids will cause pollution. The mechanical properties of the GO membrane are poor and it is difficult to apply to the field of oil-water separation. Therefore, it is of great significance to develop a self-supporting GO membrane with good mechanical properties and separation properties and apply it to the field of oil-water separation. Summary of the invention

[0005] Technical issues solved:

[0006] In response to the technical problems in the prior art such as poor permeability and poor bending performance of graphene oxide films, the present application provides a method for preparing a self-supporting graphene oxide composite film with a sponge-like pore structure, so as to prepare a self-supporting graphene oxide film with a bending-resistant and sponge-like pore structure.

[0007] Technical solution:

[0008] To achieve the above objectives, this application is implemented through the following technical solutions:

[0009] A method for preparing a self-supporting sponge-like pore structured graphene oxide composite film comprises the following steps:

[0010] The first step: preparing hydrophilic carbon nanofibers;

[0011] Step 2: preparing graphene oxide / carbon nanofiber short fibers / dopamine hydrochloride dispersion;

[0012] Step 3: vacuum filtration and drying at room temperature to form a film;

[0013] The fourth step is to remove the filter membrane: remove the base membrane by high-temperature calcination in an air atmosphere to obtain a self-supporting graphene oxide composite film.

[0014] Furthermore, the first step of preparing silicon-doped carbon nanofibers is an electrospinning method, and the specific steps are:

[0015] S1: Using polyacrylonitrile as spinning polymer, tetraethyl orthosilicate liquid or silicon dioxide as silicon source, wherein the amount of tetraethyl orthosilicate or silicon dioxide nanoparticles added is 15-30% of the mass of polyacrylonitrile; adding the silicon source and spinning polymer into a solvent containing a catalyst, wherein the catalyst is glacial acetic acid, and the amount of glacial acetic acid added is 0.01-6.25% of the volume of the solvent; electrospinning is performed in a multi-nozzle electrospinning machine using non-woven fabric as a receiving substrate; the electrospinning process parameters are: spinning voltage 25kV, injection speed 1mL / h, receiving distance 20cm, ambient temperature 25±3℃, ambient humidity 50±5%, to prepare the required raw materials for nanofiber membranes;

[0016] S2: Cut the nanofiber membrane into pieces and put them into a blender for high-speed blending at a speed of 8000-15000 r / min for 20 min to obtain nano short fibers, wherein the length of the nano short fibers is 30-100 μm; then put the nano short fibers into an oven to completely dry them, put the dried nano short fibers into a glass container, and finally put them into a blast oven and heat them to 240°C at 5°C / min, keep them warm for 120 min, take them out, and naturally cool them to room temperature to obtain nano short fibers after pre-oxidation heat treatment;

[0017] S3, carbonization treatment: the nano short fibers after pre-oxidation heat treatment are placed in a vacuum tube furnace, and the temperature is raised to 800-1000°C at a rate of 5°C / min under the protection of high-purity nitrogen, and maintained for 120 minutes. During this period, the high-purity nitrogen flow rate is 2 ml / min, and the vacuum tube furnace outlet valve is kept half open. After cooling to room temperature, hydrophilic carbon nano short fibers CNF are obtained.

[0018] Furthermore, the preparation method of the graphene oxide / carbon nano short fibers / dopamine hydrochloride dispersion in the second step is:

[0019] Step 1: 0.3 g of dopamine hydrochloride and 0.4 g of Tris were added to 60 ml of aqueous solution at a concentration of 5 mg / ml to prepare a dopamine hydrochloride mixed solution, the pH of which was between 8 and 9;

[0020] Step 2: fix the solid content of graphene oxide and / or hydrophilic carbon nanofibers CNF to 0.5 mg / ml, change the mass ratio of GO and / or CNF and add them to the dopamine hydrochloride mixed solution of step 1 to obtain a suspension, then use an ultrasonic cell stirrer to sonicate for 120 min or use a high-speed disperser to stir the suspension at 10000 rpm for 10 min to obtain a graphene oxide / hydrophilic carbon nanofibers / dopamine hydrochloride dispersion.

[0021] Furthermore, the specific method of the third step is a vacuum filtration film-forming method; specifically, filter paper is placed between a filtration cup and a filter head, and then the dispersion obtained in the second step is poured into the filtration cup, and a circulating water vacuum filtration pump is connected to filter the graphene oxide / hydrophilic carbon nanofiber / dopamine hydrochloride dispersion to obtain a wet graphene oxide / carbon nanofiber / filter paper composite film, and finally the composite film is placed at room temperature for natural drying or dried in a vacuum drying oven at 60°C for 120 minutes to completely dry the composite film; during the drying process, the dopamine remaining in the composite film undergoes self-polymerization to form polydopamine, which plays a bonding role; the filter paper is made of a thermosetting resin substrate, and the membrane pore size is 0.22 to 0.45 μm; the maximum vacuum degree of vacuum filtration is 0.098 MPa.

[0022] Furthermore, in the fourth step, the high-temperature calcination step is to place the graphene oxide / hydrophilic carbon nanofiber / filter paper substrate membrane composite film in a crucible, put it into a muffle furnace and heat it to 300°C at a heating rate of 15°C / min and keep it warm for 10 minutes until the filter paper substrate membrane is completely decomposed, and finally naturally cool it to room temperature to obtain a self-supporting sponge-like pore structure graphene oxide composite film.

[0023] Furthermore, the mass fraction of polyacrylonitrile in S1 is 12 wt % of the total mass of the solution.

[0024] Furthermore, the solvent in S1 is a mixture of one or more of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

[0025] Furthermore, in step 2, the mass ratios of GO and / or CNF are 1:0, 2:1, 1:1, and 2:1, respectively.

[0026] Principle explanation: This patent mainly utilizes GO, which has oxygen-containing functional groups on its base and edge, is hydrophilic, has high chemical activity, and forms a uniform dispersion after high-speed dispersion in water, and can form an oil-water separation membrane under the action of suction filtration. However, the current GO membrane has shortcomings such as poor water flux, i.e., poor permeability, inability to be self-supporting, and poor bending resistance. Therefore, by preparing flexible hydrophilic carbon nanofibers, they can be intercalated between GO sheets under the pressure of vacuum filtration. Furthermore, because CNF and GO cannot form a membrane smoothly by relying solely on suction filtration and have poor mechanical properties, dopamine hydrochloride is used as a binder for the two. The self-polymerization of dopamine enables GO and CNFS to be effectively bonded together. In addition, dopamine also contains hydrophilic groups that will not significantly affect the hydrophilicity of the membrane. Moreover, under the intercalation of CNF, the vertical spacing between GO layers is significantly expanded, making it easier for water to penetrate through the layered membrane structure. Hydrophilic CNFs are hydrophilic, thermally stable, and chemically inert, and combined with GO make the composite membranes ideal for energy-saving oil-water separation technologies such as gravity-driven separation, where CNFs show high reinforcement ability and improve the mechanical properties of the nanocomposite membranes.

[0027] Beneficial effects:

[0028] The present application provides a method for preparing a self-supporting sponge-like pore structured graphene oxide composite film, which has the following beneficial effects compared with the prior art:

[0029] 1. The hydrophilic carbon nanofibers of the present application have flexibility due to the introduction of silicon dioxide into the fibers, and the fibers are intercalated into the graphene oxide film through vacuum filtration and combined with the self-polymerization bonding effect of dopamine to enhance the bending resistance of the hydrophilic carbon nanofiber / graphene oxide composite film;

[0030] 2. The present application forms a sponge-like pore structure by introducing hydrophilic carbon nanofibers between GO sheets, thereby expanding the vertical interlayer nanochannels, thereby improving the water permeability. At the same time, the presence of hydrophilic carbon nanofibers and dopamine also makes the composite film have super-hydrophilic underwater super-oleophobic properties, preventing oil droplets from penetrating through the membrane;

[0031] 3. The hydrophilic carbon nanofiber / graphene oxide composite film can be self-supported by high-temperature calcination, which provides a way to prepare self-supporting graphene oxide film;

[0032] 4. The technology of the present invention is easy to operate, low in cost and highly efficient, does not require the use of additional modified chemical reagents, and is environmentally friendly and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a cross-sectional SEM image of the GO / CNF=1:1 film of the present application, wherein (a) is a 500x image and (b) is a 5kx image;

[0034] Figure 2 The water contact angle measurement graphs of GO / CNF composite films with different ratios of the present application, wherein (a) is the water contact angle measurement graph of pure GO, (b) is the water contact angle measurement graph of the composite film with GO / CNF addition ratio of 2:1, (c) is the water contact angle measurement graph of the composite film with GO / CNF addition ratio of 1:1, and (d) is the water contact angle measurement graph of the composite film with GO / CNF addition ratio of 1:2;

[0035] Figure 3 These are test photos of the bending resistance of the GO / CNF composite film of the present application, wherein (a) is a test photo of the bending resistance of the GO film, and (b) is a test photo of the bending resistance of the GO / CNF=1:1 composite film;

[0036] Figure 4 This is a graph showing the change in pure water flux of different GO / CNF composite films of the present application. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0038] In the following examples, polyacrylonitrile (molecular weight 90,000) used to prepare self-supporting sponge-like pore-structured graphene oxide composite films was purchased from Jiangsu Kunshan Hongyu Plastic Co., Ltd., tetraethyl orthosilicate, silicon dioxide nanoparticles (7-40nm), N,N-dimethylformamide, and glacial acetic acid were all purchased from Shanghai McLean Biochemical Technology Co., Ltd., monolayer graphene oxide was purchased from Suzhou Carbon Feng Technology, dopamine hydrochloride (98%), tris (hydroxymethyl) aminomethane (Tris) and sodium dodecyl sulfate (SDS) were all purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; electrospinning used the HZ-11 multi-nozzle electrospinning machine produced by Qingdao Nuokang Environmental Protection Technology Co., Ltd., and the receiving substrate used a polypropylene spunbond non-woven fabric with a gram weight of 10g / m2; the contact angle test used the SDC-350 contact angle measuring instrument of Kunshan Shengding Industrial Intelligent Technology Co., Ltd., When testing the water contact angle, the graphene oxide composite film is first stretched flat with a tension clamp and fixed on a horizontal test table. A 3μL ultrapure water droplet is transferred to the membrane surface using a microsyringe. After the water droplet morphology is stable, a contact angle photo is taken and measured, and the average value is taken for at least 5 measurements. When measuring the dynamic wetting time of the droplet on the membrane surface, a high-speed camera is used to shoot the wetting process of the droplet at a speed of 200 frames / second, and then the complete wetting time is calculated based on the time required for the droplet contact angle in the photographed picture to become 0°. The oily wastewater purification performance of the membrane material is evaluated by using petroleum ether as an oil pollutant template. Petroleum ether and SDS / deionized water are mixed in a volume ratio of 1:99 and the resulting oil-water mixture is emulsified for 5 minutes using a high-speed disperser at 5000rpm, wherein the concentration of SDS in water is 100ppm, and a water-in-oil emulsified oil-water mixture is prepared. The oil-water separation performance test process of the membrane material is as follows: first, the separation membrane is placed in a commercially available filtration device, and the water-in-oil emulsified oil-water mixture is added into the funnel of the filtration device and the liquid level is maintained at 10 cm. The volume V of the filtrate collected within a unit time t (t = 1 min) is measured, and the membrane separation flux is calculated using the formula P = V / St, where S is the effective working area of ​​the separation membrane; subsequently, the total organic carbon (TOC) value C0 of the oil-water mixture before separation and the TOC value C1 of the filtrate after separation are tested using a total organic carbon analyzer, and the membrane separation efficiency is calculated using the formula: E = (C0-C1) / C0.

[0039] Embodiment 1:

[0040] A method for preparing a self-supporting sponge-like pore structured graphene oxide composite film comprises the following steps:

[0041] The first step is to prepare hydrophilic carbon nanofibers:

[0042] S1: Polyacrylonitrile is used as the spinning polymer, tetraethyl orthosilicate is used as the silicon source, N,N-dimethylformamide is used as the spinning solvent, the mass fraction of polyacrylonitrile is 12% (3.6g), and the amount of tetraethyl orthosilicate added is 30% (1.08g) of the mass of polyacrylonitrile; at room temperature, tetraethyl orthosilicate is first added to N,N-dimethylformamide (26.4g) containing glacial acetic acid (volume fraction of 6.25%) and magnetically stirred for 30min, and then polyacrylonitrile is added, and the spinning solution is obtained after sufficient stirring; then, electrospinning is carried out in a multi-nozzle electrospinning machine with non-woven fabric as the receiving substrate, the spinning voltage is 25kV, the injection speed is 1mL / h, the receiving distance is 20cm, the ambient temperature is 25±3℃, and the ambient humidity is 50±5%, to prepare the required raw materials for the nanofiber membrane;

[0043] S2: Cut the nanofiber membrane into pieces and put them into a blender for high-speed (12000r / min) blending for 20min to obtain nano short fibers; then put the nano short fibers into an oven to completely dry them, put the dried nano short fibers into a glass container, then put them into a blast oven and heat them to 240°C at 5°C / min, keep them warm for 120min, take them out, and naturally cool them to room temperature to obtain pre-oxidized nano short fibers;

[0044] S3: Carbonization treatment: The nano-short fibers after pre-oxidation heat treatment are placed in a vacuum tube furnace, and the temperature is raised to 1000°C at a rate of 5°C / min under the protection of high-purity nitrogen, and maintained for 120 minutes. During this period, the high-purity nitrogen flow rate is 2 ml / min, and the vacuum tube furnace outlet valve is kept half open. After cooling to room temperature, hydrophilic carbon nano-short fibers (CNF) are obtained.

[0045] The second step is to prepare graphene oxide / carbon nanofiber / dopamine hydrochloride dispersion:

[0046] Step 1: add 0.3g dopamine hydrochloride and 0.4g Tris to 60ml aqueous solution at a concentration of 5mg / ml to prepare a dopamine hydrochloride mixed solution, the pH of which is between 8-9;

[0047] Step 2: The solid content of graphene oxide / hydrophilic carbon nanofibers is fixed at 0.5 mg / ml, and the solid content ratio is GO:CNF=2:1, that is, 0.02 g GO and 0.01 g CNF are added to the mixed solution of step 1, and then the suspension is stirred at 10000 rpm for 20 min using a high-speed disperser to obtain a graphene oxide / carbon nanofiber / dopamine hydrochloride dispersion;

[0048] The third step is vacuum filtration and drying to form a film; specifically, filter paper is placed between the filtration cup and the filter head, and then the dispersion obtained in the second step is poured into the filtration cup, and a circulating water vacuum filtration pump is connected to filter the graphene oxide / hydrophilic carbon nanofiber / dopamine hydrochloride dispersion to obtain a wet graphene oxide / carbon nanofiber / filter paper composite film, and finally the composite film is placed in a room temperature environment to dry naturally to completely dry the composite film;

[0049] Step 4: Place the graphene oxide / hydrophilic carbon nanofiber composite film in a crucible, put it in a muffle furnace and heat it to 300°C at a heating rate of 15°C / min and keep it warm for 10 minutes until the filter paper base film is completely decomposed, and finally cool it naturally to room temperature to obtain a self-supporting sponge-like pore structure graphene oxide film.

[0050] A self-supporting graphene oxide composite film with a sponge-like pore structure is prepared by the above method.

[0051] Embodiment 2:

[0052] A method for preparing a self-supporting sponge-like pore structured graphene oxide composite film comprises the following steps:

[0053] The first step is to prepare silicon-doped carbon nanofibers:

[0054] S1: Polyacrylonitrile is used as the spinning polymer, tetraethyl orthosilicate is used as the silicon source, N,N-dimethylformamide is used as the spinning solvent, the mass fraction of polyacrylonitrile is 12% (3.6 g), and the amount of tetraethyl orthosilicate added is 30% (1.08 g) of the mass of polyacrylonitrile; at room temperature, tetraethyl orthosilicate is first added to N,N-dimethylformamide (26.4 g) containing glacial acetic acid (volume fraction of 6.25%) and magnetically stirred for 30 minutes, and then polyacrylonitrile is added, and the spinning solution is obtained after sufficient stirring; then, electrospinning is carried out in a multi-nozzle electrospinning machine using non-woven fabric as the receiving substrate, the spinning voltage is 25 kV, the injection speed is 1 mL / h, the receiving distance is 20 cm, the ambient temperature is 25±3°C, and the ambient humidity is 50±5%, and a nanofiber membrane with uniform thickness is prepared;

[0055] S2: Cut the nanofiber membrane into pieces and put them into a blender for high-speed (12000r / min) blending for 20min to obtain nano short fibers; then put the nano short fibers into an oven to completely dry them, put the dried nano short fibers into a glass container, then put them into a blast oven and heat them to 240°C at 5°C / min, keep them warm for 120min, take them out, and naturally cool them to room temperature to obtain pre-oxidized nano short fibers;

[0056] S3: Carbonization treatment: The nano-short fibers after pre-oxidation heat treatment are placed in a vacuum tube furnace, and the temperature is raised to 1000°C at a rate of 5°C / min under the protection of high-purity nitrogen, and maintained for 120 minutes. During this period, the high-purity nitrogen flow rate is 2 ml / min, and the vacuum tube furnace outlet valve is kept half open. After cooling to room temperature, hydrophilic carbon nano-short fibers (CNF) are obtained.

[0057] The second step is to prepare a graphene oxide / carbon nanofiber short fiber / dopamine hydrochloride dispersion;

[0058] Step 1: add 0.3g dopamine hydrochloride and 0.4g Tris to 60ml aqueous solution at a concentration of 5mg / ml to prepare a dopamine hydrochloride mixed solution, the pH of which is between 8-9;

[0059] Step 2: The solid content of graphene oxide / hydrophilic carbon nanofibers is fixed at 0.5 mg / ml, and the solid content ratio is GO:CNF=1:1, that is, 0.015 g GO and 0.015 g CNF are added to the mixed solution of step 1, and then the suspension is stirred at 10000 rpm for 20 min using a high-speed disperser to obtain a graphene oxide / carbon nanofiber / dopamine hydrochloride dispersion;

[0060] The third step is vacuum filtration and drying to form a film; specifically, filter paper is placed between the filtration cup and the filter head, and then the dispersion obtained in the second step is poured into the filtration cup, and a circulating water vacuum filtration pump is connected to filter the graphene oxide / hydrophilic carbon nanofiber / dopamine hydrochloride dispersion to obtain a wet graphene oxide / carbon nanofiber / filter paper composite film, and finally the composite film is placed in a room temperature environment to dry naturally to completely dry the composite film;

[0061] Step 4: Place the graphene oxide / hydrophilic carbon nanofiber composite film in a crucible, put it in a muffle furnace and heat it to 300°C at a heating rate of 15°C / min and keep it warm for 10 minutes until the filter paper base film is completely decomposed, and finally cool it naturally to room temperature to obtain a self-supporting sponge-like pore structure graphene oxide film.

[0062] A self-supporting sponge-like pore structured graphene oxide composite film is prepared by the above method.

[0063] Embodiment 3:

[0064] A method for preparing a self-supporting sponge-like pore structured graphene oxide composite film comprises the following steps:

[0065] The first step is to prepare silicon-doped carbon nanofibers:

[0066] S1: Polyacrylonitrile is used as the spinning polymer, tetraethyl orthosilicate is used as the silicon source, N,N-dimethylformamide is used as the spinning solvent, the mass fraction of polyacrylonitrile is 12% (3.6 g), and the amount of tetraethyl orthosilicate added is 30% (1.08 g) of the mass of polyacrylonitrile; at room temperature, tetraethyl orthosilicate is first added to N,N-dimethylformamide (26.4 g) containing glacial acetic acid (volume fraction of 6.25%) and magnetically stirred for 30 minutes, and then polyacrylonitrile is added, and the spinning solution is obtained after sufficient stirring; then, electrospinning is carried out in a multi-nozzle electrospinning machine using non-woven fabric as the receiving substrate, the spinning voltage is 25 kV, the injection speed is 1 mL / h, the receiving distance is 20 cm, the ambient temperature is 25±3°C, and the ambient humidity is 50±5%, and a nanofiber membrane with uniform thickness is prepared;

[0067] S2: Cut the nanofiber membrane into pieces and put them into a blender for high-speed (12000r / min) blending for 20min to obtain nano short fibers; then put the nano short fibers into an oven to completely dry them, put the dried nano short fibers into a glass container, then put them into a blast oven and heat them to 240°C at 5°C / min, keep them warm for 120min, take them out, and naturally cool them to room temperature to obtain pre-oxidized nano short fibers;

[0068] S3: Carbonization treatment: The nano-short fibers after pre-oxidation heat treatment are placed in a vacuum tube furnace, and the temperature is raised to 1000°C at a rate of 5°C / min under the protection of high-purity nitrogen, and maintained for 120 minutes. During this period, the high-purity nitrogen flow rate is 2 ml / min, and the vacuum tube furnace outlet valve is kept half open. After cooling to room temperature, hydrophilic carbon nano-short fibers (CNF) are obtained.

[0069] The second step is to prepare graphene oxide / carbon nanofiber / dopamine hydrochloride dispersion:

[0070] Step 1: add 0.3g dopamine hydrochloride and 0.4g Tris to 60ml aqueous solution at a concentration of 5mg / ml to prepare a dopamine hydrochloride mixed solution, the pH of which is between 8-9;

[0071] Step 2: The solid content of graphene oxide / hydrophilic carbon nanofibers is fixed at 0.5 mg / ml, and the solid content ratio is GO:CNF=1:2, that is, 0.01 g GO and 0.02 g CNF are added to the mixed solution of step 1, and then the suspension is stirred at 10000 rpm for 20 min using a high-speed disperser to obtain a graphene oxide / carbon nanofiber / dopamine hydrochloride dispersion;

[0072] The third step is vacuum filtration and drying to form a film; specifically, filter paper is placed between the filtration cup and the filter head, and then the dispersion obtained in the second step is poured into the filtration cup, and a circulating water vacuum filtration pump is connected to filter the graphene oxide / hydrophilic carbon nanofiber / dopamine hydrochloride dispersion to obtain a wet graphene oxide / carbon nanofiber / filter paper composite film, and finally the composite film is placed in a room temperature environment to dry naturally to completely dry the composite film;

[0073] Step 4: Place the graphene oxide / hydrophilic carbon nanofiber composite film in a crucible, put it in a muffle furnace and heat it to 300°C at a heating rate of 15°C / min and keep it warm for 10 minutes until the filter paper base film is completely decomposed, and finally cool it naturally to room temperature to obtain a self-supporting sponge-like pore structure graphene oxide film.

[0074] A self-supporting sponge-like pore structured graphene oxide composite film is prepared by the above method.

[0075] Embodiment 4:

[0076] A method for preparing a self-supporting sponge-like pore structured graphene oxide composite film, the steps being different from those of Example 1 in that hydrophilic carbon nanofibers do not need to be prepared, and in step 2, 0.3 g GO is added instead, i.e., GO / CNF=1:0, and the remaining steps are the same.

[0077] The structure and oil-water selective wettability of the self-supporting sponge-like pore-structured graphene oxide composite film prepared in the above examples were evaluated. Figure 1 As shown in the figure, the graphene oxide composite film with hydrophilic carbon nanofibers presents an obvious sponge-like pore structure, and obvious carbon nanofibers can be seen in the composite film. Figure 2 As shown, a 3 μL water droplet can quickly wet the surface of the graphene oxide composite film prepared in all embodiments, and the static water contact angle of all composite films can be 0°, which is comparable to that of pure GO film ( Figure 2 In a), it can be seen that the addition of hydrophilic carbon nanofibers significantly increases the wetting time of water droplets ( Figure 2 b, c, d). Figure 3 As shown in the figure, the pure GO membrane has obvious creases after bending, which affects the subsequent use of the membrane ( Figure 3 a); after adding carbon nanofibers ( Figure 3b), the composite film does not change after bending, indicating that the addition of carbon nanofibers improves the bending resistance of the graphene oxide composite film. In addition, the oil-water separation performance test of the membrane material shows that the water flux of the obtained graphene oxide composite film gradually increases with the addition of hydrophilic carbon nanofibers, indicating that the carbon nanofibers effectively expand the water transport channel of graphene oxide and increase the water permeability; and under the condition of an additional 10kPa pressure, the separation efficiency of the oil-water mixture containing surfactant in water-in-oil type can reach more than 96%, and the water flux can reach up to 2000Lm -2 h -1 above.

[0078] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing a self-supporting sponge-like pore structure graphene oxide composite film, characterized in that: The specific steps include: The first step: preparing hydrophilic carbon nanofibers; Step 2: preparing graphene oxide / carbon nanofiber short fibers / dopamine hydrochloride dispersion; Step 3: vacuum filtration and drying at room temperature to form a film; The fourth step is to remove the filter membrane: remove the base membrane by high-temperature calcination in an air atmosphere to obtain a self-supporting graphene oxide composite film.

2. The method for preparing the self-supporting graphene oxide composite film according to claim 1, characterized in that: The first step of preparing hydrophilic carbon nanofibers is an electrospinning method, and the specific steps are: S1: Using polyacrylonitrile as spinning polymer, tetraethyl orthosilicate liquid or silicon dioxide as silicon source, wherein the amount of tetraethyl orthosilicate or silicon dioxide nanoparticles added is 15-30% of the mass of polyacrylonitrile; adding the silicon source and spinning polymer into a solvent containing a catalyst, wherein the catalyst is glacial acetic acid, and the amount of glacial acetic acid added is 0.01-6.25% of the volume of the solvent; electrospinning is performed in a multi-nozzle electrospinning machine using non-woven fabric as a receiving substrate; the electrospinning process parameters are: spinning voltage 25kV, injection speed 1mL / h, receiving distance 20cm, ambient temperature 25±3℃, ambient humidity 50±5%, to prepare the required raw materials for nanofiber membranes; S2: Cut the nanofiber membrane into pieces and put them into a blender for high-speed blending at a speed of 8000-15000 r / min for 20 min to obtain nano short fibers, wherein the length of the nano short fibers is 30-100 μm; Then, the nano short fibers were placed in an oven to be completely dried, and the dried nano short fibers were placed in a glass container, and finally placed in a blast oven and heated to 240°C at 5°C / min. After being kept warm for 120 minutes, they were taken out and naturally cooled to room temperature to obtain nano short fibers after pre-oxidation heat treatment. S3, carbonization treatment: the nano short fibers after pre-oxidation heat treatment are placed in a vacuum tube furnace and heated to 400 °C under the protection of high-purity nitrogen. The temperature was raised to 800-1000°C at 5°C / min and maintained for 120min, during which the high-purity nitrogen flow rate was 2ml / min and the outlet valve of the vacuum tube furnace was kept half-open. After cooling to room temperature, hydrophilic carbon nanofibers CNF were obtained.

3. The method for preparing the self-supporting sponge-like pore structure graphene oxide composite film according to claim 1, characterized in that: The preparation method of the graphene oxide / carbon nano short fibers / dopamine hydrochloride dispersion in the second step is: Step 1: 0.3 g of dopamine hydrochloride and 0.4 g of Tris were added to 60 ml of aqueous solution at a concentration of 5 mg / ml to prepare a dopamine hydrochloride mixed solution, the pH of which was between 8 and 9; Step 2: fix the solid content of graphene oxide and / or hydrophilic carbon nanofibers CNF to 0.5 mg / ml, change the mass ratio of GO and / or CNF and add them to the dopamine hydrochloride mixed solution of step 1 to obtain a suspension, then use an ultrasonic cell stirrer to sonicate for 120 min or use a high-speed disperser to stir the suspension at 10000 rpm for 10 min to obtain a graphene oxide / hydrophilic carbon nanofibers / dopamine hydrochloride dispersion.

4. The method for preparing the self-supporting sponge-like pore structure graphene oxide composite film according to claim 1, characterized in that: The specific method of the third step is a vacuum filtration film-forming method; specifically, filter paper is placed between a filtration cup and a filter head, and then the dispersion obtained in the second step is poured into the filtration cup, and a circulating water vacuum filtration pump is connected to filter the graphene oxide / hydrophilic carbon nanofiber / dopamine hydrochloride dispersion to obtain a wet graphene oxide / carbon nanofiber / filter paper composite film, and finally the composite film is placed in a room temperature environment for natural drying or dried in a vacuum drying oven at 60°C for 120 minutes to completely dry the composite film; during the drying process, the dopamine remaining in the composite film undergoes self-polymerization to form polydopamine, which plays a bonding role; the filter paper is made of a thermosetting resin substrate, and the membrane pore size is 0.22 to 0.45 μm; the maximum vacuum degree of vacuum filtration is 0.098 MPa.

5. The method for preparing the self-supporting sponge-like pore structure graphene oxide composite film according to claim 1, characterized in that: In the fourth step, the high-temperature calcination step is to place the graphene oxide / hydrophilic carbon nanofiber / filter paper substrate membrane composite film in a crucible, put it into a muffle furnace and heat it to 300°C at a heating rate of 15°C / min and keep it warm for 10 minutes until the filter paper substrate membrane is completely decomposed, and finally naturally cool it to room temperature to obtain a self-supporting sponge-like pore structure graphene oxide composite film.

6. The method for preparing the self-supporting sponge-like pore structure graphene oxide composite film according to claim 2, characterized in that: The mass fraction of polyacrylonitrile in S1 is 12 wt % of the total mass of the solution.

7. The method for preparing the self-supporting sponge-like pore structure graphene oxide composite film according to claim 2, characterized in that: The solvent in S1 is a mixture of one or more of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.

8. The method for preparing the self-supporting sponge-like pore structure graphene oxide composite film according to claim 3, characterized in that: In step 2, the mass ratios of GO and / or CNF are 1:0, 2:1, 1:1, and 2:1, respectively.

Citation Information

Patent Citations

  • Super-hydrophilic and underwater super-oleophobic carbon nanofiber membrane and preparation method thereof

    CN114749039A

  • Graphene oxide self-supporting composite membrane as well as preparation method and application thereof

    CN117919959A

  • Method of preparing composite films having poly(dopamine) treated graphene oxide-poly(vinylalcohol) and humidity sensing method using the same

    KR1020150121793A

Cited By

  • Aramid 1414-based aerogel membrane material for separating oily sewage as well as preparation method and application of aramid 1414-based aerogel membrane material

    CN122273343A