Quartz sand purification process

Through the decomposition removal process of quartz sand raw materials, combined with magnetic separation, reselecting, flotation and acid leaching, the problem of impurities not being removed during the purification process of quartz sand in the prior art has been solved, improving the quality of finished products and reducing the environment Pollution ensures the cleanliness and safety of the products.

CN118950237APending Publication Date: 2024-11-15JIANGSU JUNGE ZHICHENG TECH CO LTD

Patent Information

Application Number
CN202410850203.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing quartz sand purification process fails to remove impurities based on the origin of the quartz sand raw materials, resulting in redness, mica and feldspar-containing finished sand, affecting the quality.

Method used

Using processes including raw material scrubbing, crushing, sieving, grinding, dehydration and drying, combined with magnetic separation, reselecting, flotation and acid leaching, comprehensive coverage of quartz stone raw materials in different regions Remove impurities.

Benefits of technology

It effectively improves the processing quality of quartz sand, reduces environmental pollution, and ensures the safety of the product through deionized water cleaning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950237A_ABST
    Figure CN118950237A_ABST
Patent Text Reader

Abstract

The invention discloses a quartz sand purification process, and belongs to the technical field of quartz sand production, and the quartz sand purification process comprises the following steps: S1, raw material scrubbing: feeding a quartz sand raw material into a scrubbing machine, removing thin film iron, bonding and mud impurities on the surface of the quartz sand raw material through the scrubbing machine, and removing the surface of the quartz sand raw material through a quartz sand raw material combination under the mechanical force action of the scrubbing machine; the quartz sand is rubbed into quartz sand raw material monomers; s2, crushing the raw materials; s3, sieving: feeding the crushed quartz sand raw material into sieving equipment, intercepting the large-particle quartz sand raw material after sieving, and feeding the sieved quartz sand raw material into grinding equipment; s4, grinding; s5, impurity removal of the raw materials, wherein the ground quartz sand is subjected to impurity removal operation; and S6, dehydrating and drying. According to the quartz sand impurity removal device, impurity removal can be comprehensively covered, quartz sand can be well subjected to impurity removal operation, and the processing quality of the quartz sand can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of quartz sand production, and in particular relates to a quartz sand purification process. Background Art

[0002] Quartz sand is quartz particles made by crushing quartz stone. Quartz stone is a non-metallic mineral, a silicate mineral that is hard, wear-resistant and chemically stable. The color of quartz sand is milky white or colorless and translucent. Quartz sand is an important industrial mineral raw material, non-chemical hazardous goods, widely used in glass, casting, ceramics and fireproof materials, smelting ferrosilicon, metallurgical flux, metallurgy, construction, chemical industry, plastics, rubber, abrasives, filter materials and other industries.

[0003] During the existing quartz sand purification process, the quartz sand raw materials are not purified according to their origin. As a result, after the quartz sand is processed, the quartz sand will be reddish, contain mica and feldspar, which will affect the quality of the finished sand. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a quartz sand purification process, which has the advantages of comprehensive coverage of impurity removal, better impurity removal operation on quartz sand, and effective improvement of the processing quality of quartz sand. It solves the problem that in the operation process of the existing quartz sand purification process, the quartz sand raw material is not impurity-removed according to the origin of the quartz sand raw material, so that after the quartz sand is processed, the quartz sand will be reddish and contain mica and feldspar, thereby affecting the quality of the finished sand.

[0005] The present invention is achieved in that a quartz sand purification process comprises the following steps:

[0006] S1, raw material scrubbing, the quartz sand raw material is sent to the scrubbing machine, the film iron, bonding, and mud impurities on the surface of the quartz sand raw material are removed by the scrubbing machine, and the quartz sand raw material combination is rubbed into quartz sand raw material monomers under the mechanical force of the scrubbing machine;

[0007] S2, raw material crushing, the cleaned quartz sand raw material is sent to the crusher, during which the scrubbed quartz sand raw material is drained to reduce the surface water content of the quartz sand raw material, and the quartz sand raw material is crushed into particles when the crusher is working;

[0008] S3, screening, sending the crushed quartz sand raw material to the screening equipment, after screening, intercepting the large particles of quartz sand raw material, and the screened quartz sand raw material enters the grinding equipment;

[0009] S4, grinding, grinding the screened quartz sand raw material into quartz sand of different particle sizes according to demand;

[0010] S5, raw material impurity removal, the ground quartz sand is subjected to impurity removal operation;

[0011] S6, dehydration and drying, the quartz sand is sent to the dehydration equipment to remove excess water, and then dried in a dryer and vacuum packed in a purification workshop.

[0012] As a preferred embodiment of the present invention, in S1, during the scrubbing process, the scrubbing drain water is filtered through a filtering device and then continuously used in the scrubbing process.

[0013] As a preferred embodiment of the present invention, the filtering device includes a water pool, a water pump and a filter element, the filter element is installed in the water pool, the water pool is connected to the cleaning pool of the scrubbing machine, the filter element is used to filter the cleaning water entering the water pool, the filter element can separate the water pool into two chambers, and the water pump is used to pump the filtered water into the cleaning pool;

[0014] The filter element comprises a frame and a filter screen, wherein the filter screen is fixedly installed in the frame, and the frame is fixedly installed in the water pool, and the frame can separate the water pool into two chambers.

[0015] After the cleaning water enters the pool, it enters one of the chambers. When entering the other chamber, it is filtered by the filter element to remove impurities in the cleaning water, so that the impurities are retained in one chamber.

[0016] As a preferred embodiment of the present invention, the S5 further includes the following steps:

[0017] S5.1, magnetic separation, to remove magnetic minerals from the mine;

[0018] It should be noted that the magnetic minerals include but are not limited to limonite, hematite, mica, garnet, pyrite and ilmenite;

[0019] S5.2, Gravity separation: When the raw material contains a very small amount of heavy mineral impurities, since they are non-magnetic and have a higher specific gravity than quartz, the spiral chute gravity separation method is used to remove such heavy mineral impurities;

[0020] S5.3, flotation, due to the rounded corners of the geographical environment, when the quartz sand raw material contains a large number of mica minerals and feldspar minerals, the flotation process is used to remove these impurity minerals;

[0021] S5.4, acid leaching. After roasting, water quenching, sorting and strong magnetic separation, most oxides and impurity minerals have been removed, but some oxides and impurity minerals are still in the grain boundaries, microcracks and crystals, which are difficult to remove. Long-term acid leaching is used to remove such impurities.

[0022] As a preferred embodiment of the present invention, the water temperature of the acid leaching in S5.4 is set to 40-60°C.

[0023] As a preferred embodiment of the present invention, the S5.3 further comprises the following steps:

[0024] S5.3.1, flotation of mica, flotation of mica by amine collector;

[0025] S5.3.2, flotation of iron-containing minerals;

[0026] S5.3.3, float the feldspar, and finally adjust the pH with hydrofluoric acid to float the feldspar out.

[0027] As a preferred embodiment of the present invention, after the flotation in S5.3 is completed, the residual flotation agent and impurities on the surface of the quartz sand are washed away with deionized water; after acid leaching, the quartz sand after acid leaching is washed with deionized water to make the surface of the quartz sand neutral.

[0028] As a preferred embodiment of the present invention, the pH value of the flotation mica solution in S5.3.1 is set to 3-4.

[0029] As a preferred embodiment of the present invention, the pH value of the flotation iron-containing mineral solution in S5.3.1 is set to 4-5.

[0030] As a preferred embodiment of the present invention, the particle size of the quartz sand raw material after being crushed by the crusher in S2 is set to 5-15 mm, and the particle size of the quartz sand after being ground in S4 is set to 10-40 μm.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The present invention can effectively remove impurities in the quartz sand raw material through scrubbing, screening and impurity removal operations, and can effectively improve the processing quality of quartz sand.

[0033] 2. The present invention can collect the water discharged from the scrubbing machine by using a filtering device. After entering the pool, the water entering the pool is filtered through a filter screen, and when discharged, the harm to the surrounding environment and the water environment can be reduced. At the same time, after filtering, the filtered water can be sent to the cleaning pool through a water pump, which can be recycled and reduced.

[0034] 3. The present invention can ensure the purification effect and reaction rate by maintaining the temperature of the acid leaching solution at 40-60°C.

[0035] 4. The present invention uses the impurity removal process of magnetic separation, gravity separation, flotation and acid leaching. Since the geological and mining environments of quartz raw materials in different regions are different, according to the detection conditions, when removing impurities, one or all of the above-mentioned magnetic separation, gravity separation, flotation and acid leaching impurity removal operations are selected to comprehensively cover the removal of impurities, which can better remove impurities from quartz sand and effectively improve the processing quality of quartz sand.

[0036] 5. The quartz sand washed with deionized water in the present invention can ensure the surface cleanliness while not causing harm to workers who subsequently come into contact with the quartz sand. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 is a schematic block diagram of a process flow provided by an embodiment of the present invention;

[0038] Figure 2 is a schematic block diagram of raw material impurity removal provided by an embodiment of the present invention;

[0039] Figure 3 is a schematic diagram of flotation provided by an embodiment of the present invention;

[0040] Figure 4 It is a schematic diagram of the structure of the filtering device provided in an embodiment of the present invention.

[0041] In the figure: 1. water pool; 2. filter element; 3. frame; 4. filter screen; 5. water pump; 6. cleaning pool. DETAILED DESCRIPTION

[0042] In order to further understand the content, features and effects of the present invention, the following embodiments are given as examples and described in detail with reference to the accompanying drawings.

[0043] The structure of the present invention is described in detail below in conjunction with the accompanying drawings.

[0044] like Figures 1 to 3 As shown, a quartz sand purification process provided by an embodiment of the present invention comprises the following steps:

[0045] S1, raw material scrubbing, the quartz sand raw material is sent to the scrubbing machine, the film iron, bonding, and mud impurities on the surface of the quartz sand raw material are removed by the scrubbing machine, and the quartz sand raw material combination is rubbed into quartz sand raw material monomers under the mechanical force of the scrubbing machine;

[0046] S2, raw material crushing, the cleaned quartz sand raw material is sent to the crusher, during which the scrubbed quartz sand raw material is drained to reduce the surface water content of the quartz sand raw material, and the quartz sand raw material is crushed into particles when the crusher is working;

[0047] S3, screening, sending the crushed quartz sand raw material to the screening equipment, after screening, intercepting the large particles of quartz sand raw material, and the screened quartz sand raw material enters the grinding equipment;

[0048] S4, grinding, grinding the screened quartz sand raw material into quartz sand of different particle sizes according to demand;

[0049] S5, raw material impurity removal, the ground quartz sand is subjected to impurity removal operation;

[0050] S6, dehydration and drying, the quartz sand is sent to the dehydration equipment to remove excess water, and then dried in a dryer and vacuum packed in a purification workshop.

[0051] By adopting the above scheme, impurities in the quartz sand raw material can be effectively removed through scrubbing, screening and impurity removal operations, and the processing quality of the quartz sand can be effectively improved.

[0052] In this embodiment, in S1, during the scrubbing process, the scrubbing discharged water is filtered through a filtering device and then continues to be used in the scrubbing process.

[0053] In this embodiment, the filtering device includes a pool 1, a water pump 5 and a filter 2. The filter 2 is installed in the pool 1. The pool 1 is connected to a cleaning pool 6 of a scrubbing machine. The filter 2 is used to filter the cleaning water entering the pool 1. The filter 2 can separate the pool 1 into two chambers. The water pump 5 is used to pump the filtered water into the cleaning pool.

[0054] The filter element 2 includes a frame 3 and a filter screen 4. The filter screen 4 is fixedly installed in the frame 3. The frame 3 is fixedly installed in the pool 1, and the frame 3 can separate the pool 1 into two chambers.

[0055] After the cleaning water enters the pool 1, it enters one of the chambers. When entering the other chamber, it is filtered by the filter element 2, which can remove impurities in the cleaning water and make the impurities remain in one chamber.

[0056] By adopting the above scheme, the water discharged from the scrubbing machine can be collected through the use of filtering equipment. After entering the pool 1, the water entering the pool 1 is filtered through the filter 4. When discharged, the harm to the surrounding environment and the water environment can be reduced; at the same time, after filtering, the filtered water can be sent to the cleaning pool through the water pump 5, which can be recycled and reduced.

[0057] In this embodiment, S5 further includes the following steps:

[0058] S5.1, magnetic separation, to remove magnetic minerals from the mine;

[0059] It should be noted that the magnetic minerals include but are not limited to limonite, hematite, mica, garnet, pyrite and ilmenite;

[0060] S5.2, Gravity separation: When the raw material contains a very small amount of heavy mineral impurities, since they are non-magnetic and have a higher specific gravity than quartz, the spiral chute gravity separation method is used to remove such heavy mineral impurities;

[0061] S5.3, flotation, due to the rounded corners of the geographical environment, when the quartz sand raw material contains a large number of mica minerals and feldspar minerals, the flotation process is used to remove these impurity minerals;

[0062] S5.4, acid leaching, after roasting, water quenching, sorting, and strong magnetic separation, most oxides and impurity minerals have been removed, but some oxides and impurity minerals are still in the grain boundaries, microcracks and crystals, which are difficult to remove. Long-term acid leaching is used to remove such impurities. The water temperature of the acid leaching is set at 40-60°C;

[0063] It should be noted that during the acid leaching process, when the temperature of the acid leaching solution is maintained at 40-60°C, the purification effect and reaction rate can be guaranteed;

[0064] The S5.3 further comprises the following steps:

[0065] S5.3.1, flotation of mica, flotation of mica by amine collector;

[0066] S5.3.2, flotation of iron-containing minerals;

[0067] S5.3.3, float feldspar, and finally adjust the pH with hydrofluoric acid to float out the feldspar;

[0068] The pH value of the flotation mica solution in S5.3.1 is set to 3-4;

[0069] The pH value of the flotation iron-containing mineral solution in S5.3.1 is set to 4-5.

[0070] By adopting the above scheme, through the impurity removal process of magnetic separation, gravity separation, flotation and acid leaching, due to the different geological and mining environments of quartz raw materials in different regions, according to the detection conditions, when removing impurities, one or all of the above magnetic separation, gravity separation, flotation and acid leaching impurity removal operations are selected, which can better remove impurities from quartz sand and effectively improve the processing quality of quartz sand.

[0071] In this embodiment, after the flotation in S5.3 is completed, the residual flotation agent and impurities on the surface of the quartz sand are washed away with deionized water; after acid leaching, the acid-leached quartz sand is washed with deionized water to make the surface of the quartz sand neutral.

[0072] By adopting the above scheme, the quartz sand washed with deionized water can ensure the surface cleanliness while not causing harm to the workers who subsequently come into contact with the quartz sand.

[0073] In this embodiment, the particle size of the quartz sand raw material after being crushed by the crusher in S2 is set to 5-15 mm, and the particle size of the quartz sand after being ground in S4 is set to 10-40 μm.

[0074] By adopting the above scheme, the particle size after crushing can facilitate subsequent processing, and the quartz sand can be ground to 10-40μm according to demand, which can meet the needs of different customers.

[0075] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0076] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A quartz sand purification process, characterized in that , including the following steps: S1, raw material scrubbing, the quartz sand raw material is sent to the scrubbing machine, the film iron, bonding, and mud impurities on the surface of the quartz sand raw material are removed by the scrubbing machine, and the quartz sand raw material combination is rubbed into quartz sand raw material monomers under the mechanical force of the scrubbing machine; S2, raw material crushing, the cleaned quartz sand raw material is sent to the crusher, during which the scrubbed quartz sand raw material is drained to reduce the surface water content of the quartz sand raw material, and the quartz sand raw material is crushed into particles when the crusher is working; S3, screening, sending the crushed quartz sand raw material to the screening equipment, after screening, intercepting the large particles of quartz sand raw material, and the screened quartz sand raw material enters the grinding equipment; S4, grinding, grinding the screened quartz sand raw material into quartz sand of different particle sizes according to demand; S5, raw material impurity removal, the ground quartz sand is subjected to impurity removal operation; S6, dehydration and drying, the quartz sand is sent to the dehydration equipment to remove excess water, and then dried in a dryer and vacuum packed in a purification workshop.

2. A quartz sand purification process as claimed in claim 1, characterized in that: In S1, during the scrubbing process, the scrubbing drain water is filtered through a filtering device and then is continuously used in the scrubbing process.

3. A quartz sand purification process as claimed in claim 2, characterized in that: The filtering device comprises a water pool (1), a water pump (5) and a filter element (2), wherein the filter element (2) is installed in the water pool (1), the water pool (1) is connected to a cleaning pool of a scrubbing machine, the filter element (2) is used to filter the cleaning water entering the water pool (1), the filter element (2) can separate the water pool (1) into two chambers, and the water pump (5) is used to pump the filtered water into the cleaning pool; The filter element (2) comprises a frame (3) and a filter screen (4); the filter screen (4) is fixedly installed in the frame (3); the frame (3) is fixedly installed in the pool (1); and the frame (3) is capable of dividing the pool (1) into two chambers. After the cleaning water enters the pool (1), it enters one of the chambers. When entering the other chamber, it is filtered by the filter element (2), thereby removing impurities in the cleaning water and causing the impurities to remain in one chamber.

4. A quartz sand purification process as claimed in claim 1, characterized in that: The S5 also includes the following steps: S5.1, magnetic separation, to remove magnetic minerals from the mine; It should be noted that the magnetic minerals include but are not limited to limonite, hematite, mica, garnet, pyrite and ilmenite; S5.2, Gravity separation: When the raw material contains a very small amount of heavy mineral impurities, since they are non-magnetic and have a higher specific gravity than quartz, the spiral chute gravity separation method is used to remove such heavy mineral impurities; S5.3, Flotation: Due to geographical reasons, when the quartz sand raw material contains a large number of mica minerals and feldspar minerals, the flotation process is used to remove these impurity minerals; S5.4, acid leaching. After roasting, water quenching, sorting and strong magnetic separation, most oxides and impurity minerals have been removed, but some oxides and impurity minerals are still in the grain boundaries, microcracks and crystals, which are difficult to remove. Long-term acid leaching is used to remove such impurities.

5. A quartz sand purification process as claimed in claim 4, characterized in that: The water temperature of the acid leaching in S5.4 is set to 40-60°C.

6. A quartz sand purification process as claimed in claim 4, characterized in that: The S5.3 further comprises the following steps: S5.3.1, flotation of mica, flotation of mica by amine collector; S5.3.2, flotation of iron-containing minerals; S5.3.3, float the feldspar, and finally adjust the pH with hydrofluoric acid to float the feldspar out.

7. A quartz sand purification process as claimed in claim 4, characterized in that: After the flotation in S5.3 is completed, the residual flotation agent and impurities on the surface of the quartz sand are washed away with deionized water; after acid leaching, the quartz sand after acid leaching is washed with deionized water to make the surface of the quartz sand neutral.

8. A quartz sand purification process as claimed in claim 6, characterized in that: The pH value of the flotation mica solution in S5.3.1 is set to 3-4.

9. A quartz sand purification process as claimed in claim 6, characterized in that: The pH value of the flotation iron-containing mineral solution in S5.3.1 is set to 4-5.

10. A quartz sand purification process as claimed in claim 1, characterized in that: The particle size of the quartz sand raw material after being crushed by the crusher in S2 is set to 5-15mm; The particle size of the ground quartz sand in S4 is set to 10-40 μm.

Citation Information

Patent Citations

  • Impurity removal process for quartz sand

    CN102189037A

  • Beneficiation method for producing quartz and feldspar by using river and lake sands

    CN102824961A

  • Cleaning water circulation system of camel hair cleaning machine

    CN218491889U

Cited By

  • Method for grinding, washing and purifying quartz sand by utilizing energy-gathered electrode

    CN120157135A

  • Method for preparing high-purity quartz sand by taking weakly magnetic mineral-containing quartzite as raw material

    CN120243248A