Composite nitralloy ball block, preparation method and application of composite nitralloy ball block in steel

By preparing composite nitrogen alloy ball blocks, the problems of difficulty in melting and uneven composition of the original nitrogen alloy blocks in the molten steel are solved, and the uniform distribution and efficient microalloyation of the nitrogen alloy in the molten steel are achieved, thus improving the steel quality enhancement effect and application stability.

CN118951003APending Publication Date: 2024-11-15ANHUI ZHONGYUAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411299893.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing nitrogen alloy native block structure is dense, which makes it difficult to melt in molten steel, uneven composition, poor dissolution speed, affects the steel reinforcement effect, and poor use stability and controllability.

Method used

The composite nitride alloy balls are used to make the balls by mixing nitride with adhesive, which optimizes the uniformity of structure and composition, increases the bonding strength, reduces the floating phenomenon, and is evenly distributed in the molten steel.

Benefits of technology

It improves the uniform distribution and use effect of nitrogen alloy balls in molten steel, improves the microalloyation efficiency of steel, reduces raw material losses, improves the application environment, and improves cost-effectiveness and melting rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951003A_ABST
    Figure CN118951003A_ABST
Patent Text Reader

Abstract

The invention discloses a composite nitroalloy ball block, a preparation method and application in steel, and belongs to the technical field of nitroalloy materials. The composite nitride alloy ball block is prepared by mixing a first substance and a second substance, and the first substance is granular and / or powdery and comprises 93-98 wt% of nitride with the particle size smaller than 10 mm; the second substance contains 2-7wt% of an adhesive and water, and the viscosity value of the adhesive is more than or equal to 10mPa. S; the composite nitride alloy ball block is in the shape of one or more of a sphere, an ellipse, a prism, a regular cube, a long cube, a polygon and a hemisphere. The average particle size of the composite nitride alloy ball block is 1-65 mm; the specific gravity of the composite nitride alloy ball block is 1.1-6.7 g / cm < 3 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nitrided alloy materials, and more specifically, relates to a composite nitrided alloy ball block, a preparation method and application in steel. Background Art

[0002] Nitriding alloy is an alloy widely used in the process of steel metallurgy. In actual steel production, in order to improve the strength of steel, it is necessary to add alloys such as ferrovanadium or ferroniobium during the steelmaking process to achieve this effect through microalloying. In order to give full play to the microalloying strengthening effect of vanadium and niobium, it is generally necessary to add an appropriate amount of nitriding alloy during steelmaking to form carbonitrides with the microalloying elements vanadium and niobium, so as to improve the precipitation, solid solution strengthening and precipitation strengthening effects of the microalloying elements. Usually, there are several main methods for microalloying molten steel: 1) adding vanadium-nitrogen alloy and ferroniobium alloy; 2) adding nitriding alloy while adding ferrovanadium alloy; 3) adding nitriding alloy while adding ferroniobium alloy.

[0003] The most common way to add nitrided alloy to molten steel is to first crush different types of nitrided alloy raw blocks into small blocks of a certain particle size (generally in the range of 10-100 mm), then mix one or more crushed nitrided alloy raw blocks together in proportion, and add them to the molten steel during the steelmaking process. Patent Document 1 Chinese Patent CN106244770A discloses a microalloying reinforcing agent that can be applied to the needs of different microalloyed steel grades and can be made into alloy blocks with a particle size of 5 to 45 mm with vanadium nitride.

[0004] The above alloy blocks inevitably produce the following problems: 1) The structure of the nitrided alloy primary block is dense, and it is difficult for the molten steel to melt through the surface of the nitrided alloy primary block to the inner core part in a short time (2-5 minutes) during the steelmaking process, and the added nitrided alloy cannot be melted through, resulting in a significant reduction in its utilization rate; 2) The nitrided alloy primary block will produce a composition gradient from the outside to the inside during its nitriding process, especially the N element gradient is larger, so after the primary block is broken into small pieces; its various element compositions are uneven, thereby affecting its strengthening effect on steel; 3) The dissolution rates of several nitrided alloy primary blocks added to the molten steel at the same time are quite different, resulting in a large fluctuation in the strengthening effect of the steel; 4) The inherent characteristics of the nitrided alloy primary block result in poor stability and controllability of the molten steel strengthening effect, and a low micro-alloying strengthening target hit rate. Summary of the invention

[0005] 1. Problem to be solved

[0006] In view of the technical problem that the existing nitride alloy primary block has a dense structure and cannot be melted through in a short time, the purpose of the present invention is to provide a composite nitride alloy ball block, optimize the structure and composition uniformity of the nitride alloy primary block, enable the alloy ball blocks to be evenly distributed in the molten steel, thereby improving and stabilizing the use effect of the composite nitride alloy ball block.

[0007] Another object of the present invention is to provide a method for preparing a composite nitride alloy ball block.

[0008] Another object of the present invention is to provide an application of a composite nitride alloy ball block in steel.

[0009] 2. Technical solution

[0010] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0011] The first aspect of the present invention provides a composite nitride alloy ball block, which is formed by mixing a first substance and a second substance. The first substance is in the form of particles and / or powder, and contains 93-98% by weight of nitride with a particle size less than 10 mm (the ratio and type of the nitride are not limited and can be mixed in any proportion), optimizing the structure and uniformity of the composition of the nitride alloy primary block; the second substance contains 2-7% by weight of a binder and water (water is added additionally), and the viscosity of the binder is ≥10 mPa.s, which ensures the bonding strength of the ball block and is not easy to crush.

[0012] The shape of the ball block is one or more of a sphere, an ellipse, a prism, a cube, a rectangular cube, a polygon, a hemisphere, and an irregular ball block. The specific gravity of the composite nitride alloy ball block is 1.1-6.7 g / cm 3 When in use, the alloy ball is placed at the bottom of the ladle, or added with the steel flow. The ball uses the impact force of the molten steel to make the alloy ball evenly distributed in the molten steel, and the larger specific gravity reduces the floating phenomenon;

[0013] The average particle size of the ball block is 1-65 mm, which is smaller than that of the original block, has a larger contact area with the molten steel, and is more conducive to melting.

[0014] According to any embodiment of the first aspect of the present invention, the binder is one or more of molasses, starch, polyvinyl alcohol, dextrin, cellulose polymer, white mud, clay, bentonite, cement, and water glass.

[0015] According to any embodiment of the first aspect of the present invention, the nitride is one or more of vanadium nitride, silicon nitride, titanium nitride, niobium nitride, silicon iron nitride, silicon manganese nitride, and chromium nitride.

[0016] According to any embodiment of the first aspect of the present invention, the composite nitride alloy pellets are produced by different types of pelletizing machines and / or block making machines.

[0017] According to any embodiment of the first aspect of the present invention, it also contains 0-10 wt% of a defoamer, wherein the defoamer is CaF 2 , a type of soda ash.

[0018] The second aspect of the present invention provides a method for preparing the composite nitride alloy ball block described in the first aspect, comprising the steps of: mixing a nitride with a particle size less than 10 mm and a binder; the nitride is selected from one or more of vanadium nitride, silicon nitride, titanium nitride, niobium nitride, silicon iron nitride, silicon manganese nitride, and chromium nitride, and the size of the crushed nitride is 0 to 10 mm, that is, less than 10 mm, because they cannot be compressed; molding in the absence of a binder, and mixing evenly with the binder to form a ball block.

[0019] According to any embodiment of the second aspect of the present invention, the nitride comprises vanadium nitride, and the phase of the vanadium nitride comprises VN phase, V 2 N phase and V 3 N phase; wherein the VN phase accounts for 65-90% by weight, V 2 N and V 3 The sum of the two phases N accounts for 10-35% by weight.

[0020] According to any embodiment of the second aspect of the present invention, the proportion of the VN phase is 80% by weight, and the V 2 N and V 3 The total weight of the two phases is 20%.

[0021] According to any embodiment of the second aspect of the present invention, the nitride comprises silicon nitride, and the phase of the silicon nitride comprises α-Si 3 N 4 and β-Si 3 N 4 Phase, the α-Si 3 N 4 The proportion of the phase is 79-96% by weight, β-Si 3 N 4 The proportion of the phase is 4-21% by weight.

[0022] According to any embodiment of the second aspect of the present invention, the nitride alloy ball block is composed of nitride powder and particles in different proportions, wherein the powder with a particle size less than 0.01 mm accounts for less than 6%, the powder with a particle size of 0.01 mm-0.04 mm accounts for less than or equal to 27%, the powder with a particle size of 0.04 mm-10 mm accounts for greater than or equal to 67%, and the total proportion is calculated as 100%, and all of them can be powder (80 mesh-400 mesh) pressed balls.

[0023] The third aspect of the present invention provides an application of the composite nitride alloy ball block described in the first aspect, or the composite nitride alloy ball block obtained by the preparation method described in the second aspect in steel. The application of the composite nitride alloy ball block of the present invention in steel includes but is not limited to high chromium cast iron, high-strength strip steel, non-quenched and tempered steel, high-strength H-shaped steel, high-speed tool steel, high-strength pipeline steel, V-grade threaded steel, HRB500 (E) high-strength earthquake-resistant steel, HRB400 (E) steel, HRB600 steel and Q620D steel.

[0024] 3. Beneficial effects

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The composite nitride alloy ball block of the present invention may contain 93-98 weight % of at least one nitride with a particle size of less than 10 mm, and 2-7 weight % of a binder and water. The nitride and the binder are mixed to form a ball block, which can not only optimize the structure and uniformity of the composition of the nitride alloy raw block, but also enable the alloy ball block to be evenly distributed in the molten steel, thereby improving and stabilizing the use effect of the composite nitride alloy ball block;

[0027] (2) The composite nitride alloy ball block of the present invention contains a defoaming agent, which can solve the problem that some single nitride alloy primary blocks (such as SiN, SiFeN, SiMnN) generate a large amount of smoke and foam slag during the application process, and effectively improve the application environment;

[0028] (3) The composite nitride alloy pellet of the present invention adjusts the proportion of at least one nitride to make the pellet, which can accurately achieve the required element composition and improve the cost-effectiveness of the steel microalloying efficiency;

[0029] (4) The composite nitride alloy ball of the present invention, wherein the phase of silicon nitride comprises α-Si 3 N 4 and β-Si 3 N 4 Phase, the α-Si 3 N 4 The proportion of the phase is 79-96% by weight, β-Si 3 N 4The proportion of the phase is 4-21% by weight; analysis found that α-Si 3 N 4 The whisker surface is smooth, with a large number of defects and a large number of branched whiskers; β-Si 3 N 4 The surface of the whiskers is smooth, basically defect-free, and has few bifurcated whiskers, which makes the alloy material have better crushing performance. It not only improves the crushing efficiency, but also reduces the proportion of powder and reduces the loss of raw materials, but also avoids dust on site and improves environmental quality.

[0030] (5) The preparation method of the present invention improves the process steps of nitriding the alloy, for example, the cooling rate is controlled to be 3-5°C / s during the cooling process, so that the phases of vanadium nitride precipitated inside the nitrided alloy block include VN phase, V 2 N phase and V 3 N phase; wherein the VN phase accounts for 65-90% by weight, V 2 N and V 3 The sum of the two phases of N accounts for 10-35% by weight, and further, the alloy block of the material has good crushing performance;

[0031] (6) Compared with the prior art in which the cored wire must be added at a refining station using a special wire feeder, which makes the operation inconvenient, the composite nitride alloy ball block of the present invention can be added anytime and anywhere during the entire microalloying process according to the process and working conditions, is not affected by the process station, and is convenient and quick to use. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.

[0033] Figure 1 This is a physical picture of the composite nitride alloy ball block of Example 1 of the present invention;

[0034] Figure 2 This is a physical picture of the composite nitride alloy ball block of Example 2 of the present invention;

[0035] Figure 3 This is a physical picture of the composite nitride alloy ball block of Example 3 of the present invention;

[0036] Figure 4 This is a physical picture of the composite nitride alloy ball block of Example 4 of the present invention;

[0037] Figure 5 It is a structural schematic diagram of an extrusion die of the present invention;

[0038] Figure 6 It is a schematic diagram of the structure of another extrusion die of the present invention. DETAILED DESCRIPTION

[0039] The present disclosure may be more easily understood by reference to the following description in conjunction with the accompanying drawings and examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or shown herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise stated.

[0040] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.

[0041] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".

[0042] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.

[0043] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.

[0044] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.

[0045] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values ​​can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values ​​stated in the range includes each value within the range.

[0046] The composite nitride alloy ball block of the present invention is a ball block made by mixing a first substance and a second substance, wherein the first substance is in the form of particles and / or powder, and its main component contains 93-98% by weight of nitride with a particle size of less than 10 mm. The nitride alloy ball block is composed of nitride powder and particles in different proportions, wherein the powder with a particle size of less than 0.01 mm accounts for less than 6%, the powder with a particle size of 0.01 mm-0.04 mm accounts for less than or equal to 27%, the powder with a particle size of 0.04 mm-10 mm accounts for greater than or equal to 67%, and the total proportion is calculated as 100%, and all powders (80 mesh-400 mesh) can be pressed into balls.

[0047] The nitride is one or more of vanadium nitride, silicon nitride, titanium nitride, niobium nitride, silicon iron nitride, silicon manganese nitride, and chromium nitride. These nitrides contain N element, and by adding alloy balls into microalloyed steel, the nitrogen element interacts with the microalloying element to form nitride or nitrogen carbide in the form of precipitation reaction in ferrite.

[0048] It should be noted that the nitrides of microalloying elements are more stable than carbides and have a lower tendency to aggregate. Nitrogen addition will maximize the ratio of particle volume fraction to particle size, thereby maximizing the key microstructure of microalloyed steel, namely grain refinement and precipitation strengthening. Nitride particles can increase the austenite grain refinement temperature during heating, prevent grain growth during rolling, delay recrystallization, increase phase transformation ratio, and increase precipitation strengthening.

[0049] In addition, preferably, the nitride includes vanadium nitride and silicon nitride. The alloying element vanadium is mainly present in the form of its carbon and nitride in the matrix and grain boundaries in steel, which plays a role in precipitation strengthening and inhibiting grain growth. The solubility of vanadium in ferrite is much smaller than that in austenite. As the phase change proceeds, under certain thermodynamic and kinetic conditions, the carbon and nitride of vanadium precipitate at the phase boundary. By accelerating cooling in the two-phase region, the grains can be refined, and the precipitation of its carbon and nitride can be controlled. The size and distribution of its precipitate determine the effect of its precipitation strengthening. Since vanadium and nitrogen have a strong affinity, adding a certain amount of nitrogen while adding a certain amount of vanadium can make its strengthening effect more effective.

[0050] The present invention provides a preparation method containing vanadium nitride and silicon nitride, and the steps are:

[0051] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, vanadium-containing slag, ferrosilicon, metallic silicon or ferrotitanium;

[0052] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh;

[0053] Step S3, the raw material fine powders obtained in step S2 are mixed according to 60% silicon element, 15% vanadium element, and 12% titanium element, and then 2% of polyborosiloxane and 7% of graphite carbon reducing agent accounting for the mass fraction of the total raw material fine powder are added, mixed and pressed into blocks at a pressure of 120 MPa using a strong ball press;

[0054] Step S4: Place the compact obtained in step S3 into a pretreatment furnace, heat it to 680°C, and fill the furnace with protective gas (argon-nitrogen mixed gas, wherein the purity of Ar gas is 99%, and the purity of N 2 Purity 98%), pretreated for 5 hours;

[0055] Step S5, placing the pretreated pressed block into a nitriding furnace for nitriding treatment; during the nitriding treatment, nitrogen is introduced at a pressure of 0.2 MPa, the temperature is first raised to 1000°C for 3 hours, then raised to 1200°C for 9 hours, and then further raised to 1350°C for 8 hours, until it is heated to 1600°C for 12 hours;

[0056] Step S6: After the nitriding treatment is completed, the alloy is naturally cooled slowly in the furnace to below 300° C., and then taken out of the furnace and cooled to room temperature to obtain vanadium nitride alloys with a particle size of 3-70 mm.

[0057] Furthermore, the second substance contains 2-7 weight % of adhesive and water. After the adhesive and water are mixed and stirred, the viscosity of the adhesive is ≥10mPa.s, preferably between 10mPa.s and 100mPa.s. The ball forming rate of the present invention is 98%. After testing, the ball is relatively complete after falling from 2 meters, which is sufficient to show that the bonding strength of the ball is relatively high.

[0058] Combination Figures 1 to 4 As shown, the shape of the ball block is one or more of a spherical, elliptical, prism-shaped, cube-shaped, rectangular, polygonal, hemispherical, and irregular ball block, and the specific gravity of the composite nitride alloy ball block is 1.1-6.7g / cm 3 When in use, the alloy ball blocks are placed at the bottom of the ladle, or added with the steel flow. The ball blocks use the impact force of the molten steel to make the alloy ball blocks evenly distributed in the molten steel, and the larger specific gravity reduces the floating phenomenon; the average particle size of the ball blocks is 1-65mm, which is smaller than the particles of the original blocks, has a larger contact area with the molten steel, and is more conducive to melting.

[0059] In some embodiments of the present invention, the ball block can be made into various shapes, preferably spherical, elliptical, prismatic, and polygonal. The composite nitride alloy ball block is produced by different types of ball making machines and / or block making machines. The ball making machine and / or block making machine can use an extrusion die, such as Figure 5 , Figure 6 As shown, the corresponding shape is produced.

[0060] In some embodiments of the present invention, the adhesive is one or more of molasses, starch, polyvinyl alcohol, dextrin, cellulose polymer, soda ash, white mud, clay, bentonite, cement, and water glass. Some of the above adhesives are organic compounds, which will participate in combustion (above 1000°C) during the preparation process and convert into carbon elements; some are inorganic compounds, which will decompose into oxides at high temperatures, such as silicon dioxide, aluminum oxide, etc., especially after water glass is dehydrated to form a network structure, so that the strength of the composite nitride alloy ball block is improved.

[0061] In the steel smelting process, in the carbonization process (carbon-oxygen reaction), adding raw alloy balls will promote the deoxidation reaction, thereby increasing the smoke; in addition, the raw alloy blocks are added to the molten steel, and the N generated by thermal decomposition 2 , N 2 The extended residence time of the gas in the slag can easily cause a large amount of gas to be unable to be quickly discharged from the slag in the furnace in a short period of time, causing the slag in the furnace to foam rapidly and rise sharply, eventually forming splashing foam slag. If a large amount of foam slag is produced and cannot be eliminated in time, even in extreme cases, slag overflow accidents may occur, which may directly lead to the deterioration of the alloying conditions of the molten steel.

[0062] On the basis of the above, the alloy ball block contains 0-10% by weight of defoamer, preferably, the defoamer is 3% CaF 2 .CaF 2 It can reduce the viscosity of slag, lower the melting temperature of slag, and sharply reduce the foaming performance of slag. 2 When the content exceeds 10%, the dethickening and defoaming effects are no longer obvious.

[0063] The preparation method of the composite nitride alloy ball block of the present invention comprises the steps of: mixing nitride with a particle size less than 10 mm and a binder; the nitride is selected from one or more of vanadium nitride, silicon nitride, titanium nitride, niobium nitride, silicon iron nitride, silicon manganese nitride, and chromium nitride, and the size of the crushed and ground nitride is 0 to 10 mm, that is, less than 10 mm, because they cannot be compressed; molding without a binder, and making a ball block after being evenly mixed with the binder.

[0064] The nitride alloy material of the present invention adopts X-ray diffractometer phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined; silicon nitride, vanadium nitride and other nitrides are measured respectively, wherein the diffraction peaks of silicon nitride and vanadium nitride appear in the RXD diagram, thereby determining that the alloy block contains vanadium nitride and silicon nitride.

[0065] Wherein, the nitride comprises vanadium nitride, and the phase of the vanadium nitride comprises VN phase, V 2 N phase and V 3 N phase; wherein the VN phase accounts for 65-90% by weight, V 2 N and V 3 The sum of the two phases is 10-35% by weight. Preferably, the VN phase is 80% by weight, and the V 2 N and V 3 The sum of the two phases of N accounts for 20% by weight. 2 N and V 3 There is no set requirement for the mixing ratio between the two phases, and they can be mixed in any ratio.

[0066] It should be noted that the impurity dispersion in the internal structure of the vanadium nitride of the present invention becomes smaller and / or uniform, so that there are a reasonable number of impurity gaps between the vanadium nitride crystals at the microscopic level. Under the action of external force, these parts can be easily broken and crushed, thereby improving the crushing efficiency; in addition, the crystal morphology of the internal vanadium nitride crystals is relatively regular, and the mutual connection method is single, which also makes the morphology of the powder obtained by the final crushing relatively regular and the particle size distribution uniform.

[0067] However, in the prior art, the content of crushed vanadium nitride powder below 0.1 mm reaches 70% (resulting in more than 5% of fine powder less than 0.01 mm), which is not conducive to the preparation of cored wires on the one hand, and on the other hand, due to excessive fine powder, there is a lot of dust on site, resulting in a large loss of vanadium nitride raw materials. According to the final statistics of each batch of production on site, the loss rate of vanadium nitride crushed by the impact crusher reaches about 3%, which is a serious loss and also causes great pollution to the factory environment.

[0068] In addition, the nitride includes silicon nitride. The inventor surprisingly found that the phase of silicon nitride precipitated inside the nitride alloy ball block includes α-Si 3 N 4 and β-Si 3 N 4 Phase, the α-Si 3 N 4 The proportion of the phase is 79-96% by weight, β-Si 3 N 4 The proportion of the phase is 4-21% by weight. 3 N 4 The whisker surface is smooth, with a large number of defects and a large number of branched whiskers; β-Si 3 N 4 The surface of the whiskers is smooth, basically defect-free, and there are few branched whiskers.

[0069] According to the standards: (1) GB / T 20567-2020 "Vanadium Nitrogen Alloy"; (2) GB / T 24583.1-2019 "Vanadium Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder", the specific contents of silicon nitride, vanadium nitride and other nitrides are obtained.

[0070] [Application in steel] The alloy ball block can be used in steel, especially special steel; the application includes using the multi-element nitrided alloy material to smelt high-strength steel, H-shaped steel, and high-chromium cast iron.

[0071] The application of the composite nitride alloy ball block obtained by the above preparation method in steel, the application of the composite nitride alloy ball block of the present invention in steel, includes but is not limited to high chromium cast iron, high-strength strip steel, non-quenched and tempered steel, high-strength H-shaped steel, high-speed tool steel, high-strength pipeline steel, V-grade threaded steel, HRB500 (E) high-strength earthquake-resistant steel, HRB400 (E) steel, HRB600 steel and Q620D steel.

[0072] The data comparison is shown in the following table:

[0073]

[0074] The results of Comparative Example 1 and Comparative Example 2 are compared with those of Examples 1-4. The nitride alloy raw block is added into the molten steel, and the N generated by thermal decomposition is 2 , N 2 The gas in the molten slag drives the molten slag in the furnace to foam rapidly and rise sharply, forming splashing foam slag. However, there is basically no splashing foam slag in Examples 1-4.

[0075] After testing, the phase of silicon nitride obtained in Example 1 includes α-Si 3 N 4 and β-Si 3 N 4 Phase, the α-Si 3 N 4 The proportion of the phase is 90% by weight, β-Si 3 N 4 The proportion of the phase was 10% by weight.

[0076] The VN phase accounts for 70% by weight, V 2 N and V 3 The sum of the two phases of N accounts for 30% by weight. 2 N and V 3 There is no set requirement for the mixing ratio between the two phases, and they can be mixed in any ratio.

[0077] Example 2 The phase of silicon nitride obtained includes α-Si 3 N 4 and β-Si 3 N 4 Phase, the α-Si 3 N 4 The proportion of the phase is 89% by weight, β-Si 3 N 4 The proportion of the phase was 11% by weight.

[0078] The VN phase accounts for 80% by weight, V 2 N and V 3 The sum of the two phases of N accounts for 20% by weight. 2 N and V 3 There is no set requirement for the mixing ratio between the two phases, and they can be mixed in any ratio.

[0079] Example 3 The phase of silicon nitride obtained includes α-Si 3 N 4 and β-Si3 N 4 Phase, the α-Si 3 N 4 The proportion of the phase is 85% by weight, β-Si 3 N 4 The proportion of the phase is 15% by weight.

[0080] The VN phase accounts for 75% by weight, V 2 N and V 3 The sum of the two phases of N accounts for 25% by weight. 2 N and V 3 There is no set requirement for the mixing ratio between the two phases, and they can be mixed in any ratio.

[0081] The composite nitride alloy ball block of the present invention has at least the following effects:

[0082] 1) Adjusting the proportion of at least one nitride to make a ball block can accurately achieve the required element composition and improve the cost-effectiveness of steel microalloying efficiency; it is known from field use that the alloy ball blocks can be evenly distributed in the molten steel, thereby improving and stabilizing the use effect of the composite nitride alloy ball blocks;

[0083] 2) The nitride alloy ball can be adjusted to achieve the appropriate specific gravity (specific gravity 1.1-6.7g / cm 3 ) and porosity (7-46%), increasing melting speed and melting rate by 20-30%;

[0084] 3) The nitride alloy ball can be adjusted to reach a suitable melting point (e.g. ferrosilicon nitride, 1430-1560°C), and the melting speed and melting rate of the nitride alloy in molten steel can be regulated and stabilized;

[0085] 4) By selecting the extrusion die (such as Figure 5 and Figure 6 The shape and size (quality) of the balls can be adapted to a wide range of different application processes and working conditions by controlling the ball-making pressure (the strong ball press presses the balls at a pressure greater than 110Mpa).

[0086] 5) After the ball blocks are made, they are crushed to increase the surface area and surface roughness of the material, increase the contact surface and penetration of the molten steel, and are conducive to improving the melting speed and melting rate.

[0087] The advantages of the alloy ball block of the present invention are:

[0088] 1. Improve the melting rate and recovery rate of alloy elements in molten steel; 2. Improve the strengthening efficiency and stability of molten steel; 3. Adapt to different steel grades and different microalloying processes; 4. Improve the cost-effectiveness of application and significantly reduce the application cost.

[0089] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.

Claims

1. A composite nitride alloy ball block, which is made by mixing a first substance and a second substance into a ball block, characterized in that: The first substance is in the form of granules and / or powders, and contains 93-98% by weight of nitrides with a particle size of less than 10 mm; the second substance contains 2-7% by weight of a binder and water, and the viscosity of the binder is ≥10 mPa.s; The shape of the composite nitride alloy ball block is one or more of spherical, elliptical, prism-shaped, cube-shaped, rectangular, polygonal, and hemispherical; The average particle size of the composite nitride alloy ball block is 1-65 mm; the specific gravity of the composite nitride alloy ball block is 1.1-6.7 g / cm 3 .

2. The composite nitride alloy ball block according to claim 1, characterized in that: The adhesive is one or more of molasses, starch, polyvinyl alcohol, dextrin, cellulose polymer, white mud, clay, bentonite, cement and water glass.

3. The composite nitride alloy ball block according to claim 1, characterized in that: The nitride is one or more of vanadium nitride, silicon nitride, titanium nitride, niobium nitride, silicon iron nitride, silicon manganese nitride, and chromium nitride.

4. The composite nitride alloy ball block according to claim 1, characterized in that: The composite nitride alloy ball blocks are produced and formed by different types of ball making machines and / or block making machines.

5. The composite nitride alloy ball block according to claim 1, characterized in that: It also contains 0-10% by weight of a defoamer, which is one of CaF2 and soda ash.

6. A method for preparing the composite nitride alloy ball block according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing nitride with a particle size less than 10 mm and a binder; the nitride is selected from one or more of vanadium nitride, silicon nitride, titanium nitride, niobium nitride, silicon iron nitride, silicon manganese nitride and chromium nitride, and the size of the crushed and ground nitride is 0 to 10 mm.

7. The method for preparing the composite nitride alloy ball block according to claim 6, characterized in that: The nitride comprises vanadium nitride, and the phases of the vanadium nitride comprise VN phase, V2N phase and V3N phase; wherein the VN phase accounts for 65-90% by weight, and the sum of the V2N and V3N phases accounts for 10-35% by weight.

8. The method for preparing the composite nitride alloy ball block according to claim 7, characterized in that: The VN phase accounts for 80% by weight, and the sum of the V2N and V3N phases accounts for 20% by weight.

9. The method for preparing the composite nitride alloy ball block according to claim 8, characterized in that: The nitride includes silicon nitride, and the phases of the silicon nitride include α-Si3N4 and β-Si3N4 phases. The α-Si3N4 phase accounts for 79-96% by weight, and the β-Si3N4 phase accounts for 4-21% by weight.

10. The method for preparing the composite nitride alloy ball block according to claim 9, characterized in that: The nitride alloy ball block is composed of nitride powder and particles in different proportions, among which powder with a particle size less than 0.01mm accounts for less than 6%, 0.01mm-0.04mm accounts for less than or equal to 27%, 0.04mm-10mm accounts for greater than or equal to 67%, and the total proportion is calculated as 100%.

11. An application of the composite nitride alloy ball block according to any one of claims 1 to 5, or the composite nitride alloy ball block obtained by the preparation method according to any one of claims 6 to 10 in steel, wherein the application of the composite nitride alloy ball block in steel includes but is not limited to high chromium cast iron, high strength strip steel, non-quenched and tempered steel, high strength H-shaped steel, high speed tool steel, high strength pipeline steel, V-grade threaded steel, HRB500 (E) high strength earthquake-resistant steel, HRB400 (E) steel, HRB600 steel and Q620D steel.