Oxidation-resistant and high-temperature-resistant soldering tin bar and preparation method thereof

By setting flux filling holes in the solder strip, the problem that flux cannot be mixed with the tin liquid in time in the prior art is solved, and the flux content and solder stability in the tin liquid are achieved, and the solder strength is improved.

CN118951471AInactive Publication Date: 2024-11-15SHENZHEN GREEN QIANTIAN TIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198629.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing solder strips that are oxidative and high temperature resistant, flux cannot be mixed with the tin liquid in time during the melting process, resulting in changes in the flux content in the tin liquid. External flux is required to improve the soldering quality and affect the soldering stability.

Method used

A solder strip is designed, whose body consists of a pure tin layer and a nickel tin layer. The outer wall of the nickel tin layer is plated with a gold plating layer. A first filling hole and a second filling hole are provided, and flux is filled therein so that the flux is Always maintain a certain proportion during the melting process to ensure the uniformity and stability of the flux in the tin melt.

Benefits of technology

By setting flux filling holes in the solder strip, we ensure that the flux is fully mixed with the tin liquid during the melting process, avoiding the need for external flux addition, and improving soldering stability and solder strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951471A_ABST
    Figure CN118951471A_ABST
Patent Text Reader

Abstract

The invention discloses an antioxidant and high-temperature-resistant soldering tin bar and a preparation method thereof.The antioxidant and high-temperature-resistant soldering tin bar comprises a soldering tin bar body, the soldering tin bar body comprises a pure tin layer and a nickel tin layer, the pure tin layer is located in the nickel tin layer, and the outer wall of the nickel tin layer is plated with a gold plating layer; the soldering tin bar body is mainly composed of the pure tin layer and the nickel tin layer, the gold plating layer is plated on the outer wall of the nickel tin layer, the oxidation resistance of the surface of the soldering tin bar body is improved through the gold plating layer, in addition, the first filling holes are formed in the pure tin layer, the second filling holes are formed between the pure tin layer and the nickel tin layer, and the oxidation resistance of the surface of the soldering tin bar body is improved. The first filling hole and the second filling hole are both filled with soldering flux, when the soldering tin bar body is melted, the proportion of the soldering flux in molten tin is always kept to a certain proportion from the beginning of melting to the end of melting, and the content of the soldering flux in the molten tin cannot change along with increase of use data of the soldering tin bar body. The soldering stability of the soldering tin bar body is improved to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solder bars, and in particular relates to an oxidation-resistant and high-temperature-resistant solder bar and a preparation method thereof. Background Art

[0002] Solder bar is a product used for circuit board welding. Solder bar is divided into two types: lead tin bar and lead-free tin bar. Both lead tin bar and lead-free tin bar have the characteristics of wettability, good fluidity and easy tinning. The solder joints after welding with solder bar are bright, full and free of cold solder joints. They are often used in wave soldering.

[0003] After searching, the Chinese patent document application number is 202110005417.7, which discloses an antioxidant and high-temperature resistant solder bar. The antioxidant and high-temperature resistant solder bar is made by disassembling the integral structure of the traditional solder bar, and a tin antioxidant reduction powder box and a flux filling cavity are arranged inside the solder bar. The tin antioxidant reduction powder box and the flux can be filled into the interior of the solder bar, so that when the solder bar is melted, the tin antioxidant reduction powder and the flux will provide antioxidant protection for the molten tin, thereby ensuring the timeliness and effectiveness of antioxidant protection.

[0004] However, the above solder bar still has the following defects:

[0005] The flux filling cavity in the above-mentioned solder bar is located at the top of the U-shaped preform, and the tin bar usually melts from the end to the middle during the melting process. When the U-shaped preform that is not in the flux cavity is melted, the flux inside the flux cavity cannot be mixed with the molten tin liquid. Until the flux cavity is melted, the flux in the flux cavity gradually melts into the tin liquid, causing the flux content in the tin liquid to change. As the number of solder bars used increases, the flux content in the tin liquid also changes. In order to improve the welding quality of the welded parts, it is necessary to use external flux to improve the welding quality of the welded parts, which brings inconvenience to the welding of the welded parts. For this reason, we propose an antioxidant and high-temperature resistant solder bar and a preparation method thereof to solve the stability of the flux content in the tin liquid and reduce the probability of welding with the help of external flux addition. Summary of the invention

[0006] The object of the present invention is to provide an oxidation-resistant and high-temperature-resistant solder bar and a preparation method thereof. The solder bar body is mainly composed of a pure tin layer and a nickel-tin alloy layer. By filling a first filling hole and a second filling hole with flux, when the solder bar body is melted, the flux ratio in the molten tin always maintains a certain ratio from the beginning to the end of melting, so that the flux content in the molten tin will not change with the increase of the use data of the solder bar body, so as to solve the problems raised in the above-mentioned background technology.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] An oxidation-resistant and high-temperature-resistant solder bar comprises a solder bar body, wherein the solder bar body comprises a pure tin layer and a nickel-tin alloy layer, wherein the pure tin layer is located inside the nickel-tin alloy layer, and the outer wall of the nickel-tin alloy layer is plated with a gold-plated layer, and a second filling hole is arranged equidistantly between the pure tin layer and the nickel-tin alloy layer, and a first filling hole is opened at the center of the pure tin layer, and the first filling hole and the second filling hole are both filled with solder flux, and the mass ratio of the pure tin layer to the nickel-tin alloy layer is 10:1;

[0009] The nickel-tin alloy layer comprises the following components by mass: 10-15 parts of nickel powder and 85-90 parts of tin powder;

[0010] The soldering flux comprises the following components: 40-50 parts of water solvent, 20-30 parts of zinc chloride, 20-30 parts of ammonium chloride, 8-15 parts of boric acid, 8-15 parts of sodium silicate and 8-15 parts of aluminum silicate.

[0011] Preferably, the nickel-tin alloy layer comprises the following components by mass: 10 parts of nickel powder and 85 parts of tin powder;

[0012] The soldering flux comprises the following components: 40 parts of water solvent, 20 parts of zinc chloride, 20 parts of ammonium chloride, 8 parts of boric acid, 8 parts of sodium silicate and 8 parts of aluminum silicate.

[0013] Preferably, the nickel-tin alloy layer comprises the following components by mass: 12 parts of nickel powder and 87 parts of tin powder;

[0014] The soldering flux comprises the following components: 45 parts of water solvent, 25 parts of zinc chloride, 25 parts of ammonium chloride, 12 parts of boric acid, 12 parts of sodium silicate and 12 parts of aluminum silicate.

[0015] Preferably, the nickel-tin alloy layer comprises the following components by mass: 15 parts of nickel powder and 90 parts of tin;

[0016] The soldering flux comprises the following components: 50 parts of water solvent, 30 parts of zinc chloride, 30 parts of ammonium chloride, 15 parts of boric acid, 15 parts of sodium silicate and 15 parts of aluminum silicate.

[0017] Preferably, the first filling hole comprises a main hole portion and a plurality of protrusions, the plurality of protrusions are distributed at equal angles around the main hole portion, and notches are provided on opposite sides of the protrusions.

[0018] Preferably, the second filling hole is provided with a circular hole, the center of the circular hole is flush with the outer wall of the pure tin layer, and the diameter of the circular hole is less than 0.3 mm.

[0019] Preferably, the second filling hole is configured as a semicircular hole recessed toward the inner side of the pure tin layer, and a plurality of the semicircular holes are located at the edges of the pure tin layer.

[0020] Preferably, the thickness of the gold-plated layer is set to 2-2.5um, and the surface of the nickel-tin layer needs to be micro-etched with 5% sulfuric acid before gold plating, and then washed with water solvent to remove oxides on the surface of the nickel-tin layer.

[0021] Preferably, the aqueous solvent used is a mixture of deionized water and an organic acid, and the mass ratio of the deionized water to the organic acid is 10:1.

[0022] Based on the above-described anti-oxidation and high temperature resistant solder bar, the present invention further provides a method for preparing the anti-oxidation and high temperature resistant solder bar, comprising the following steps:

[0023] S1. Prepare pure tin, nickel powder, tin powder and flux raw materials;

[0024] S2, after melting pure tin, pouring the pure tin melt into a pure tin layer pouring mold, and after the pure tin melt is cooled and demoulded, a pure tin layer is obtained; wherein the pure tin layer pouring mold contains a first draw rod having the same shape as the first filling hole, and the first draw rod is not withdrawn during demoulding;

[0025] S3, after melting the tin powder, adding the nickel powder and stirring evenly to form a nickel-tin mixture, then adding the nickel-tin mixture into a nickel-tin alloy layer casting mold for casting, and demoulding after the nickel-tin mixture is cooled to obtain a primary solder bar; wherein the nickel-tin alloy layer casting mold contains a plurality of second draw rods with the same shape as the second filling hole, and the second draw rods are not drawn out during demoulding;

[0026] S4, placing the solder bar product into a gold electroplating tank for gold plating, and pulling out the first draw rod and the second draw rod on the gold-plated product to obtain a solder bar product containing a first filling hole and a second filling hole;

[0027] S5, filling the first filling hole and the second filling hole with soldering flux, so that the soldering flux covers the first filling hole and the second filling hole, and the preparation of the solder bar is completed after the soldering flux solidifies.

[0028] The anti-oxidation and high temperature resistant solder bar and the preparation method thereof proposed by the present invention have the following advantages compared with the prior art:

[0029] The solder bar body provided by the present invention is mainly composed of a pure tin layer and a nickel-tin alloy layer, and a gold-plated layer is plated on the outer wall of the nickel-tin alloy layer, and the gold-plated layer is used to improve the oxidation resistance of the surface of the solder bar body. In addition, a first filling hole is opened on the pure tin layer, and a plurality of second filling holes are arranged between the pure tin layer and the nickel-tin alloy layer, and the first filling holes and the second filling holes are filled with flux. When the solder bar body is melted, the proportion of the flux in the molten tin always maintains a certain proportion from the beginning to the end of melting, so that the content of the flux in the molten tin will not change with the increase of the use data of the solder bar body, and the stability of the solder bar body welding is improved to a certain extent. The flux provided by the present invention is mainly composed of a water solvent, zinc chloride, ammonium chloride, boric acid, sodium silicate and aluminum silicate, so that the flux can be fully mixed with the molten tin when the solder bar body is melted, and the uniformity of the mixing of the flux and the molten tin is improved to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the structure of the solder bar of the present invention;

[0031] Figure 2 It is a top view schematic diagram of the solder bar of the present invention;

[0032] Figure 3 A flowchart of the preparation of the solder bar of the present invention;

[0033] In the figure: 1, solder bar body; 101, nickel-tin alloy layer; 102, pure tin layer; 2, first filling hole; 201, main hole portion; 202, raised portion; 203, recessed portion; 3, second filling hole. DETAILED DESCRIPTION

[0034] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] The present invention provides Figure 1-2An oxidation-resistant and high-temperature-resistant solder bar shown includes a solder bar body 1, wherein the solder bar body 1 includes a pure tin layer 102 and a nickel-tin alloy layer 101, wherein the pure tin layer 102 is located inside the nickel-tin alloy layer 101, wherein the outer wall of the nickel-tin alloy layer 101 is plated with a gold-plated layer, wherein a second filling hole 3 is arranged equidistantly between the pure tin layer 102 and the nickel-tin alloy layer 101, wherein a first filling hole 2 is opened at the center of the pure tin layer 102, wherein the first filling hole 2 and the second filling hole 3 are both filled with solder flux, and wherein the mass ratio of the pure tin layer 102 to the nickel-tin alloy layer 101 is 10:1;

[0036] When the solder bar body 1 is melted, the proportion of flux in the molten tin always maintains a certain proportion from the beginning to the end of melting, so that the content of flux in the molten tin will not change with the increase of the usage data of the solder bar body 1, which improves the welding stability of the solder bar body 1 to a certain extent. After the solder bar is melted, the gold-plated layer melts into the molten tin. When the weldment contacts the molten tin, it is convenient for the molten tin to wrap around the pin of the weldment, which can improve the bonding force between the molten tin and the pin of the weldment, thereby improving the welding strength of the weldment.

[0037] The first filling hole 2 includes a main hole portion 201 and a plurality of raised portions 202, wherein the plurality of raised portions 202 are distributed at equal angles around the main hole portion 201, and recessed portions 203 are provided on opposite sides of the raised portions 202. The main hole portion 201 and the raised portions 202 form a filling hole with a flower-shaped cross-section, so that the flux is equally distributed at different positions of the solder bar body 1, so as to keep the ratio of the flux to the molten tin consistent during melting.

[0038] The second filling hole 3 is provided with a circular hole, the center of the circular hole is flush with the outer wall of the pure tin layer 102, and the diameter of the circular hole is less than 0.3 mm.

[0039] The second filling hole 3 can also be configured as a semicircular hole recessed toward the inner side of the pure tin layer 102 , and a plurality of the semicircular holes are located around the edges of the pure tin layer 102 .

[0040] The thickness of the gold-plated layer is set to 2-2.5um. Before gold plating, the surface of the nickel-tin layer 101 needs to be micro-etched with sulfuric acid with a concentration of 5%, and then washed with a water solvent to remove the oxide on the surface of the nickel-tin layer 101. The gold-plated layer is used to protect the solder bar body 1 to reduce the oxidation caused by the nickel-tin layer 101 contacting with oxygen in the air, thereby improving the oxidation resistance of the surface of the solder bar body 1. At the same time, due to the high melting point of gold, the high-temperature performance of the solder bar body 1 can also be improved by the gold-plated layer.

[0041] The nickel-tin alloy layer 101 comprises the following components by mass: 10-15 parts of nickel powder and 85-90 parts of tin powder. When preparing the nickel-tin alloy layer 101, the tin powder is melted and then added to the nickel powder and stirred evenly to form a nickel-tin mixed liquid. The nickel-tin mixed liquid is then added to a nickel-tin alloy layer casting mold for casting, and the nickel-tin mixed liquid is demolded after cooling.

[0042] The soldering flux comprises the following ingredients: 40-50 parts of water solvent, 20-30 parts of zinc chloride, 20-30 parts of ammonium chloride, 8-15 parts of boric acid, 8-15 parts of sodium silicate and 8-15 parts of aluminum silicate; the water solvent used is a mixture of deionized water and an organic acid, and the mass ratio of the deionized water to the organic acid is 10:1. The soldering flux mainly consists of the water solvent, zinc chloride, ammonium chloride, boric acid, sodium silicate and aluminum silicate, so that the soldering flux can be fully mixed with the molten tin when the solder bar body is melted, thereby improving the uniformity of the mixing of the soldering flux and the molten tin to a certain extent.

[0043] Among them, zinc chloride is an inorganic compound, a white crystalline powder, which is easily soluble in water. When welding, the zinc chloride solution is used to remove the oxides on the surface of the weldment. It does not damage the metal surface of the weldment during welding. After the water evaporates by heat, the molten salt covers the metal surface, preventing it from oxidizing again, thereby improving its oxidation resistance.

[0044] Ammonium chloride is a colorless crystal or white granular powder. It is a strong electrolyte that dissolves in water to form ammonium ions and chloride ions. When ammonia and hydrogen chloride combine to form ammonium chloride, white smoke is produced and it has no odor. Powdered ammonium chloride is very easy to deliquesce, especially qualified products. The moisture absorption point is generally around 76%. It begins to decompose when heated to 100°C and can be completely decomposed into ammonia and hydrogen chloride gas at 337.8°C. When cooled, it recombines to form extremely small particles of ammonium chloride and appears as thick white smoke. It is not easy to sink and is also very difficult to dissolve in water again.

[0045] Boric acid is an inorganic compound, a white crystalline powder, with a smooth feel and no odor. It can improve the heat resistance of solder bars, increase mechanical strength, and shorten melting time.

[0046] The aqueous solution of sodium silicate is commonly known as water glass. It is a mineral binder and a soluble inorganic silicate. When preparing sodium silicate, liquid sodium hydroxide and quartz sand are mixed in an appropriate proportion and added into an autoclave. The mixture is heated with steam and stirred to react directly to form liquid sodium silicate. The finished sodium silicate is obtained by filtering and concentrating.

[0047] Aluminum silicate is made of hard clay clinker as raw material, and is produced by melting in a resistance or electric arc furnace and blowing into fibers. Aluminum silicate is a kind of aluminum silicate, and its properties are: colorless crystals, with low thermal conductivity, excellent thermal stability and chemical stability, which can improve the high temperature resistance of the solder bar to a certain extent.

[0048] Based on the above-described anti-oxidation and high temperature resistant solder bar, the present invention also provides a method for preparing the anti-oxidation and high temperature resistant solder bar, such as Figure 3 As shown, the following steps are included:

[0049] S1. Prepare pure tin, nickel powder, tin powder and flux raw materials;

[0050] S2, after melting pure tin, pouring the pure tin melt into a pure tin layer pouring mold, and after the pure tin melt is cooled and demoulded, a pure tin layer is obtained; wherein the pure tin layer pouring mold contains a first draw rod having the same shape as the first filling hole, and the first draw rod is not withdrawn during demoulding;

[0051] S3, after melting the tin powder, adding the nickel powder and stirring evenly to form a nickel-tin mixture, then adding the nickel-tin mixture into a nickel-tin alloy layer casting mold for casting, and demoulding after the nickel-tin mixture is cooled to obtain a primary solder bar; wherein the nickel-tin alloy layer casting mold contains a plurality of second draw rods with the same shape as the second filling hole, and the second draw rods are not drawn out during demoulding;

[0052] S4, placing the solder bar product into a gold electroplating tank for gold plating, and pulling out the first draw rod and the second draw rod on the gold-plated product to obtain a solder bar product containing a first filling hole and a second filling hole;

[0053] S5, filling the first filling hole and the second filling hole with soldering flux, so that the soldering flux covers the first filling hole and the second filling hole, and the preparation of the solder bar is completed after the soldering flux solidifies.

[0054] When preparing the solder bar, the pure tin layer 102 is poured from the inside to the outside, then the nickel-tin alloy layer 101 is poured, and finally the gold plating layer is performed. The first filling hole 2 is formed at one time when the pure tin layer 102 is poured, and the second filling hole 3 is also formed at one time when the nickel-tin alloy layer 101 is poured, which reduces the processing steps for preparing the first filling hole 2 and the second filling hole 3, and improves the efficiency of solder bar preparation to a certain extent.

[0055] Example 1

[0056] An oxidation-resistant and high-temperature-resistant solder bar comprises a solder bar body 1, wherein the solder bar body 1 comprises a pure tin layer 102 and a nickel-tin alloy layer 101, wherein the pure tin layer 102 is located inside the nickel-tin alloy layer 101, wherein the outer wall of the nickel-tin alloy layer 101 is plated with a gold-plated layer, wherein a second filling hole 3 is arranged equidistantly between the pure tin layer 102 and the nickel-tin alloy layer 101, wherein a first filling hole 2 is opened at the center of the pure tin layer 102, wherein the first filling hole 2 and the second filling hole 3 are both filled with solder flux, and wherein the mass ratio of the pure tin layer 102 to the nickel-tin alloy layer 101 is 10:1;

[0057] The nickel-tin alloy layer 101 comprises the following components by mass: 10 parts of nickel powder and 85 parts of tin powder;

[0058] The soldering flux comprises the following ingredients: 40 parts of water solvent, 20 parts of zinc chloride, 20 parts of ammonium chloride, 8 parts of boric acid, 8 parts of sodium silicate, and 8 parts of aluminum silicate;

[0059] After preparing the solder bar according to the raw materials provided above, a melting test was performed, and the content of the flux in the molten tin was monitored in real time during the melting process of the solder bar. The test results are as follows:

[0060]

[0061] From the above table, it can be confirmed that the proportion of flux in the molten tin always remains at 10% from the beginning to the end of melting, so that the content of flux in the molten tin will not change with the increase of the usage data of the solder bar body, which ensures the stability of the soldering of the solder bar body to a certain extent.

[0062] Example 2

[0063] An oxidation-resistant and high-temperature-resistant solder bar comprises a solder bar body 1, wherein the solder bar body 1 comprises a pure tin layer 102 and a nickel-tin alloy layer 101, wherein the pure tin layer 102 is located inside the nickel-tin alloy layer 101, wherein the outer wall of the nickel-tin alloy layer 101 is plated with a gold-plated layer, wherein a second filling hole 3 is arranged equidistantly between the pure tin layer 102 and the nickel-tin alloy layer 101, wherein a first filling hole 2 is opened at the center of the pure tin layer 102, wherein the first filling hole 2 and the second filling hole 3 are both filled with solder flux, and wherein the mass ratio of the pure tin layer 102 to the nickel-tin alloy layer 101 is 10:1;

[0064] The nickel-tin alloy layer 101 comprises the following components by mass: 12 parts of nickel powder and 87 parts of tin powder;

[0065] The soldering flux comprises the following components: 45 parts of water solvent, 25 parts of zinc chloride, 25 parts of ammonium chloride, 12 parts of boric acid, 12 parts of sodium silicate and 12 parts of aluminum silicate.

[0066] After preparing the solder bar according to the raw materials provided above, a melting test was performed, and the content of the flux in the molten tin was monitored in real time during the melting process of the solder bar. The test results are as follows:

[0067]

[0068] From the above table, it can be confirmed that the proportion of flux in the molten tin always remains at 10% from the beginning to the end of melting, so that the content of flux in the molten tin will not change with the increase of the usage data of the solder bar body, which ensures the stability of the soldering of the solder bar body to a certain extent.

[0069] Example 3

[0070] An oxidation-resistant and high-temperature-resistant solder bar comprises a solder bar body 1, wherein the solder bar body 1 comprises a pure tin layer 102 and a nickel-tin alloy layer 101, wherein the pure tin layer 102 is located inside the nickel-tin alloy layer 101, wherein the outer wall of the nickel-tin alloy layer 101 is plated with a gold-plated layer, wherein a second filling hole 3 is arranged equidistantly between the pure tin layer 102 and the nickel-tin alloy layer 101, wherein a first filling hole 2 is opened at the center of the pure tin layer 102, wherein the first filling hole 2 and the second filling hole 3 are both filled with solder flux, and wherein the mass ratio of the pure tin layer 102 to the nickel-tin alloy layer 101 is 10:1;

[0071] The nickel-tin alloy layer 101 comprises the following components by mass: 15 parts of nickel powder and 90 parts of tin;

[0072] The soldering flux comprises the following components: 50 parts of water solvent, 30 parts of zinc chloride, 30 parts of ammonium chloride, 15 parts of boric acid, 15 parts of sodium silicate and 15 parts of aluminum silicate.

[0073] After preparing the solder bar according to the raw materials provided above, a melting test was performed, and the content of the flux in the molten tin was monitored in real time during the melting process of the solder bar. The test results are as follows:

[0074]

[0075] From the above table, it can be confirmed that the proportion of flux in the molten tin always remains at 10% from the beginning to the end of melting, so that the content of flux in the molten tin will not change with the increase of the usage data of the solder bar body, which ensures the stability of the soldering of the solder bar body to a certain extent.

[0076] Prior art test confirmation: The solder bar prepared by the prior art (the prior art uses the Chinese patent document application number 202110005417.7, which discloses an antioxidant and high temperature resistant solder bar) was subjected to a melting test, and the content of the flux in the molten tin was monitored in real time during the melting process of the solder bar. The test results are as follows:

[0077]

[0078] From the above table, it can be confirmed that the proportion of flux in the molten tin gradually decreases from the beginning to the end of melting, and external flux must be added during welding to improve the welding quality of the welded parts.

[0079] In summary, the present invention provides an antioxidant and high-temperature resistant solder bar. When the solder bar body 1 melts, the proportion of flux in the molten tin always maintains a certain proportion from the beginning to the end of melting, so that the content of flux in the molten tin will not change with the increase of the usage data of the solder bar body 1, and the stability of the soldering of the solder bar body is improved to a certain extent.

[0080] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An oxidation-resistant and high-temperature-resistant solder bar, comprising a solder bar body, characterized in that: The solder bar body comprises a pure tin layer and a nickel-tin alloy layer, wherein the pure tin layer is located inside the nickel-tin alloy layer; The outer wall of the nickel-tin alloy layer is plated with a gold-plated layer; a second filling hole is arranged at an equal distance between the pure tin layer and the nickel-tin alloy layer; and a first filling hole is opened in the center of the pure tin layer; The first filling hole and the second filling hole are both filled with solder flux, and the mass ratio of the pure tin layer to the nickel-tin alloy layer is 10:1; The nickel-tin alloy layer comprises the following components by mass: 10-15 parts of nickel powder and 85-90 parts of tin powder; The soldering flux comprises the following components: 40-50 parts of water solvent, 20-30 parts of zinc chloride, 20-30 parts of ammonium chloride, 8-15 parts of boric acid, 8-15 parts of sodium silicate and 8-15 parts of aluminum silicate.

2. The anti-oxidation and high temperature resistant solder bar according to claim 1, characterized in that: The nickel-tin alloy layer comprises the following components by mass: 10 parts of nickel powder and 85 parts of tin powder; The soldering flux comprises the following components: 40 parts of water solvent, 20 parts of zinc chloride, 20 parts of ammonium chloride, 8 parts of boric acid, 8 parts of sodium silicate and 8 parts of aluminum silicate.

3. The anti-oxidation and high temperature resistant solder bar according to claim 1, characterized in that: The nickel-tin alloy layer comprises the following components by mass: 12 parts of nickel powder and 87 parts of tin powder; The soldering flux comprises the following components: 45 parts of water solvent, 25 parts of zinc chloride, 25 parts of ammonium chloride, 12 parts of boric acid, 12 parts of sodium silicate and 12 parts of aluminum silicate.

4. The anti-oxidation and high temperature resistant solder bar according to claim 1, characterized in that: The nickel-tin alloy layer comprises the following components by mass: 15 parts of nickel powder and 90 parts of tin; The soldering flux comprises the following components: 50 parts of water solvent, 30 parts of zinc chloride, 30 parts of ammonium chloride, 15 parts of boric acid, 15 parts of sodium silicate and 15 parts of aluminum silicate.

5. The anti-oxidation and high temperature resistant solder bar according to claim 1, characterized in that: The first filling hole comprises a main hole portion and a plurality of protrusions, wherein the plurality of protrusions are distributed around the main hole portion at equal angles, and notches are provided on opposite sides of the protrusions.

6. The anti-oxidation and high temperature resistant solder bar according to claim 5, characterized in that: The second filling hole is provided with a circular hole, the center of the circular hole is flush with the outer wall of the pure tin layer, and the diameter of the circular hole is less than 0.3 mm.

7. The anti-oxidation and high temperature resistant solder bar according to claim 5, characterized in that: The second filling hole is configured as a semicircular hole recessed toward the inner side of the pure tin layer, and a plurality of the semicircular holes are located at the edges of the pure tin layer.

8. The anti-oxidation and high temperature resistant solder bar according to claim 1, characterized in that: The thickness of the gold-plated layer is set to 2-2.5um. Before gold plating, the surface of the nickel-tin layer needs to be micro-etched with 5% sulfuric acid and then washed with water solvent to remove oxides on the surface of the nickel-tin layer.

9. The anti-oxidation and high temperature resistant solder bar according to claim 1, characterized in that: The aqueous solvent used is a mixture of deionized water and an organic acid, and the mass ratio of the deionized water to the organic acid is 10:

1.

10. A method for preparing an oxidation-resistant and high-temperature-resistant solder bar, based on the oxidation-resistant and high-temperature-resistant solder bar according to any one of claims 1 to 9, characterized in that: The steps include: S1. Prepare pure tin, nickel powder, tin powder and flux raw materials; S2, after melting the pure tin, pouring the pure tin melt into a pure tin layer pouring mold, and after the pure tin melt is cooled and demoulded, a pure tin layer is obtained; The pure tin layer casting mold contains a first draw rod with the same shape as the first filling hole, and the first draw rod is not drawn out during demoulding; S3, after melting the tin powder, adding the nickel powder and stirring evenly to form a nickel-tin mixture, then adding the nickel-tin mixture into a nickel-tin layer casting mold for casting, and after the nickel-tin mixture is cooled, demoulding to obtain a primary solder bar; The nickel-tin alloy layer casting mold contains a plurality of second draw rods with the same shape as the second filling holes, and the second draw rods are not drawn out during demoulding; S4, placing the solder bar product into a gold electroplating tank for gold plating, and pulling out the first draw rod and the second draw rod on the gold-plated product to obtain a solder bar product containing a first filling hole and a second filling hole; S5, filling the first filling hole and the second filling hole with soldering flux, so that the soldering flux covers the first filling hole and the second filling hole, and the preparation of the solder bar is completed after the soldering flux solidifies.