Asphalt synergistic molybdenum disulfide modified spherical graphite negative electrode material as well as preparation method and application thereof
Through oxidation treatment and pore-forming agent ball milling technology, the uniform dispersion of molybdenum disulfide in porous carbon materials is ensured, which solves the agglomeration and coating inhomogeneity of the negative electrode materials of lithium-ion batteries, and significantly improves the electrochemical performance and cycle stability. , suitable for industrial production.
Patent Information
- Application Number
- CN202411034054.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Molybdenum disulfide is easy to agglomerate when combined with spherical graphite, difficult to modify porous carbon materials, easy to accumulate and agglomerate when asphalt coating is difficult to completely wet the surface, and difficult to control the uniformity of material coating, which limits the improvement of the electrochemical performance of the negative electrode materials of lithium-ion batteries. .
By oxidizing the spherical graphite, adding pore-forming agent and asphalt ball milling and calcining, forming a porous structure, and molybdenum disulfide is grown in hydrothermal reaction to ensure its uniform dispersion and growth in the porous carbon material.
The uniform dispersion of molybdenum disulfide in graphite is achieved, the electrochemical performance of the material is improved, the specific capacity, cycle stability and fast charging performance are significantly improved, while reducing production costs, which is suitable for industrial production.
Smart Images

Figure CN118954500A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation of new energy materials, and specifically relates to a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, and a preparation method and application thereof. Background Art
[0002] At present, the negative electrode of lithium-ion batteries mainly uses spherical graphite, whose theoretical specific capacity is 372mAh g -1 Due to the limitation of theoretical specific capacity, if the battery energy density is to be further improved, it must be compounded with other high specific capacity materials. Molybdenum disulfide material has a very high theoretical specific capacity (670mAh g -1 ), high conductivity and excellent cycle stability. Compounding it with graphite can provide strong support for the development of high-performance negative electrode materials for lithium-ion batteries in the future. However, molybdenum disulfide is easy to agglomerate, and if it cannot be evenly dispersed, it will have the opposite effect.
[0003] Modification treatment is performed on the surface of spherical graphite, such as introducing porous carbon materials, and then using relevant technologies to grow molybdenum disulfide in the porous carbon materials to achieve effective dispersion of molybdenum disulfide and improve the electrochemical performance of the material. From an industrial perspective, asphalt has the advantages of a wide range of sources and a high carbon yield during pyrolysis. If asphalt is used to coat spherical graphite, the production cost will be greatly reduced. However, due to the conjugation effect of polycyclic aromatic hydrocarbons in asphalt, asphalt is easy to accumulate and agglomerate during pyrolysis, which is not conducive to complete coating on the surface of spherical graphite, let alone forming a porous network structure. In addition, the surface of spherical graphite is highly hydrophobic. Even if it is directly calcined with asphalt, its surface tension is not enough to allow the asphalt to completely infiltrate it. Therefore, the problem of uniformity of material coating has always been difficult to solve.
[0004] When preparing high-performance lithium-ion battery negative electrode materials by combining molybdenum disulfide and spherical graphite, there are problems such as molybdenum disulfide is easy to agglomerate, porous carbon materials are difficult to modify, asphalt coating is easy to stack and agglomerate, the surface is difficult to completely wet, and the uniformity of material coating is difficult to control. It is urgent to find new modification methods and coating technologies to achieve uniform dispersion and efficient utilization of molybdenum disulfide in graphite. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide and its preparation method and application, so as to solve the technical problems of easy agglomeration, uneven coating and limited improvement of electrochemical performance when molybdenum disulfide and spherical graphite are compounded in the negative electrode material of lithium-ion batteries.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention discloses a method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, comprising the following steps:
[0008] S1: oxidizing spherical graphite to obtain a first precursor;
[0009] S2: ball-milling the asphalt, the pore-forming agent and the first precursor obtained in step S1 to obtain a second precursor;
[0010] S3: calcining the second precursor obtained in step S2 to obtain a third precursor;
[0011] S4: immersing the third precursor obtained in step S3 in a mixed aqueous solution of sodium molybdate and thiourea to carry out a hydrothermal reaction, filtering and drying to obtain a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide.
[0012] Preferably, in step S1, the atmosphere of the oxidation treatment is air or oxygen; the temperature of the oxidation treatment is 200-400° C.; and the time of the oxidation treatment is 2-8 hours.
[0013] Preferably, in step S2, the mass ratio of the first precursor: asphalt: pore-forming agent is 100: (5-15): (2-10).
[0014] Preferably, in step S2, the pore-forming agent is at least one of zinc chloride, sodium carbonate and sodium chloride.
[0015] Preferably, in step S2, the rotation speed of the ball mill is 200-500 rpm; the ball-to-material ratio is (10-40):1; and the ball milling time is 0.5-2 h.
[0016] Preferably, in step S3, the calcination temperature is 800-1200° C.; the calcination time is 1-3 hours; and the calcination atmosphere is nitrogen or argon.
[0017] Preferably, in step S4, in the mixed aqueous solution of sodium molybdate and thiourea, the molar ratio of sodium molybdate to thiourea is 1:2; the mass ratio of the third precursor to sodium molybdate is 100:(5-20); and the dosage ratio of the third precursor to the total volume of the solution is 1 g:(5-20) mL.
[0018] Preferably, in step S4, the temperature of the hydrothermal reaction is 160-220° C.; and the time of the hydrothermal reaction is 5-12 h.
[0019] The invention also discloses a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide obtained by the preparation method.
[0020] The invention also discloses the use of the asphalt prepared by the preparation method in conjunction with molybdenum disulfide modified spherical graphite negative electrode material in the preparation of negative electrode materials for lithium ion batteries.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The invention discloses a preparation method of a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide. First, the spherical graphite is oxidized to improve its surface roughness and wettability to asphalt, so that the asphalt can be more evenly coated on the graphite surface. Then, the ball milling method is adopted to make it evenly dispersed with the asphalt, avoiding the uneven coating problem caused by insufficient surface tension of asphalt in the traditional method. By adding a pore-forming agent, it is ensured that a porous carbon material coating is generated on the surface of the spherical graphite during the calcination process. These porous structures not only provide abundant sites for the growth of molybdenum disulfide, but also promote the uniform dispersion of molybdenum disulfide on the graphite surface, effectively preventing the agglomeration of molybdenum disulfide, thereby improving the overall electrochemical performance of the composite material. In order to further improve the performance of spherical graphite, molybdenum disulfide is grown in a porous carbon material by an impregnation process and a hydrothermal method. Molybdenum disulfide grows in a highly conductive porous carbon material, and its high theoretical specific capacity is fully utilized, which complements the spherical graphite and significantly improves the overall capacity of the negative electrode material. At the same time, the porous carbon material and the asphalt coating layer work together to improve the material's electron transfer efficiency and ion diffusion rate, and improve the battery's rate performance and cycle stability. At the same time, the hydrothermal process can also remove functional groups such as hydroxyl and carboxyl generated during the oxidation of spherical graphite, ultimately greatly improving the material's capacity and stability. The asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material obtained by the preparation method disclosed in the present invention can solve the problems of low specific capacity and unstable cycle faced by graphite negative electrodes, and obtain a negative electrode material with high capacity and excellent cycle performance.
[0023] The present invention also discloses a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide prepared by the above-mentioned preparation method, which has high specific capacity and energy density, can store more electrical energy, and thus improve the overall energy density of the battery. The combination of the asphalt coating layer and the porous carbon material provides an additional protective barrier for the graphite negative electrode, effectively reduces the volume change of graphite during the charging and discharging process, and prevents the occurrence of structural damage and pulverization. At the same time, molybdenum disulfide itself also has good structural stability and can maintain a high capacity retention rate in multiple charging and discharging cycles. The introduction of porous carbon materials and molybdenum polysulfide improves the transmission path of lithium ions and improves the ionic conductivity of the material. This enables the battery to absorb and release lithium ions faster, thereby improving the fast charging performance of the battery and meeting the needs of modern electronic devices for fast charging. The asphalt coating helps to stabilize the structure of the negative electrode material, reduces the internal stress changes caused by overcharging or over-discharging, and thus reduces the risk of damage to the battery due to overcharging or over-discharging. This improves the safety performance of the battery and extends the service life of the battery. The asphalt coating can prevent direct contact between the electrolyte and the graphite negative electrode, reduce the co-embedding of the electrolyte on the graphite surface, and thus reduce the irreversible capacity loss of the graphite. This helps to improve the cycle efficiency and energy utilization efficiency of the battery. Asphalt and molybdenum disulfide modified spherical graphite negative electrode materials show significant advantages in specific capacity, cycle stability, fast charging performance, safety performance and cost, providing a new solution for improving the performance of lithium-ion batteries.
[0024] The present invention also discloses the use of asphalt prepared by the above-mentioned preparation method and molybdenum disulfide modified spherical graphite negative electrode material in the preparation of lithium ion battery negative electrode material. The introduction of molybdenum disulfide brings additional specific capacity contribution to the negative electrode material. Its high theoretical specific capacity significantly improves the overall specific capacity of the composite material, thereby improving the energy density of the lithium ion battery. The presence of porous carbon material not only provides more active sites for the embedding and de-embedding of lithium ions, but also shortens the transmission path of lithium ions, further improving the energy density of the battery. The synergistic effect of the asphalt coating layer and the porous carbon material effectively reduces the volume change of the graphite negative electrode during the charging and discharging process, prevents the occurrence of structural damage and pulverization, thereby improving the cycle stability of the battery. The introduction of porous carbon material and molybdenum polysulfide improves the ionic conductivity of the negative electrode material, allowing the battery to absorb and release lithium ions faster, thereby improving the fast charging performance of the battery. During the fast charging process, the negative electrode material is prone to polarization, resulting in a decrease in charging efficiency. The asphalt and molybdenum disulfide modified spherical graphite negative electrode material can effectively reduce the occurrence of polarization and improve the fast charging efficiency. Both molybdenum disulfide and asphalt can maintain good stability at high temperatures, which helps to improve the safety of batteries in high temperature environments. The preparation process of asphalt-modified spherical graphite negative electrode materials with molybdenum disulfide is relatively simple and easy, suitable for large-scale industrial production, and helps to improve production efficiency and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The composite material 0.2A g was prepared in Example 1 of the present invention -1 Cycle performance diagram of
[0026] Figure 2 The composite material 0.3A g was prepared in Example 2 of the present invention. -1 Cycle performance diagram. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0028] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0029] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0030] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0031] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0032] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0033] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0034] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0035] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0036] The invention discloses a method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, comprising the following steps:
[0037] The spherical graphite is subjected to oxidation treatment in an oxidizing atmosphere to obtain a first precursor;
[0038] The first precursor, asphalt and pore-forming agent are mixed by ball milling to obtain a second precursor;
[0039] calcining the second precursor at a set temperature and atmosphere to obtain a third precursor;
[0040] The third precursor is immersed in a mixed aqueous solution of sodium molybdate and thiourea to carry out a hydrothermal reaction, and the product is filtered and dried to obtain a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide.
[0041] Preferably, the pre-oxidation atmosphere of graphite is air or oxygen, the pre-oxidation temperature is 200-400°C, and the pre-oxidation time is 2-8h;
[0042] Preferably, the mass ratio of the first precursor, asphalt and pore-forming agent is 100:(5-15):(2-10);
[0043] Preferably, the pore-forming agent is at least one of zinc chloride, sodium carbonate and sodium chloride;
[0044] Preferably, the ball milling speed is between 200 and 500 rpm, the ball-to-material ratio is (10-40):1, and the ball milling time is 0.5-2 h;
[0045] Preferably, the calcination temperature is 800-1200°C, the time is 1-3h, and the calcination atmosphere is nitrogen or argon;
[0046] Preferably, the molar ratio of sodium molybdate to thiourea is 1:2, the mass ratio of spherical graphite to sodium molybdate is 100:(5-20), and the mass volume ratio of spherical graphite to the total volume of the solution is 1 g:(5-20) mL;
[0047] Preferably, the hydrothermal reaction temperature is 160-220°C and the hydrothermal time is 5-12h;
[0048] The final composite material is mainly used in the negative electrode of lithium-ion batteries.
[0049] The present invention also discloses a spherical graphite negative electrode material prepared by the above-mentioned preparation method in cooperation with molybdenum disulfide. -1 At a current density of 1.34 W, the initial specific capacity is 589 mAh g -1 , which is much higher than the theoretical specific capacity of traditional spherical graphite negative electrode materials (372mAh g -1 ). This shows that the modification of asphalt and molybdenum disulfide significantly improves the lithium storage capacity of the negative electrode material. The specific capacity is 476 mAh g after 300 cycles. -1 , the capacity retention rate was 80.8%. At a slightly higher current density of 0.3A g -1 The initial specific capacity is 521 mAh g -1 The initial specific capacity remains at 521 mAhg -1 , indicating that the material can maintain high lithium storage performance under different current conditions. The specific capacity is 417 mAh g after 300 cycles. -1 , although the specific capacity retention rate is slightly lower, it still shows good cycle stability. This shows that the modified negative electrode material has a stable structure during multiple charge and discharge processes and can effectively resist volume change and structural damage.
[0050] The present invention also discloses the use of the asphalt synergistic molybdenum disulfide modified spherical graphite negative electrode material prepared by the above-mentioned preparation method in the preparation of lithium-ion battery negative electrode materials. The introduction of molybdenum disulfide brings additional specific capacity contribution to the negative electrode material. The presence of porous carbon material not only provides more active sites for the embedding and de-embedding of lithium ions, but also shortens the transmission path of lithium ions, further improving the energy density of the battery. The synergistic effect of the asphalt coating layer and the porous carbon material effectively reduces the volume change of the graphite negative electrode during the charging and discharging process, prevents the occurrence of structural damage and pulverization, thereby improving the cycle stability of the battery. The preparation process of the asphalt synergistic molybdenum disulfide modified spherical graphite negative electrode material is relatively simple and easy, suitable for large-scale industrial production, and helps to improve production efficiency and reduce production costs.
[0051] Example 1
[0052] A method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, comprising the following steps:
[0053] 100g of spherical graphite was oxidized in air at 200°C for 8h, then put into a ball mill together with 5g of asphalt and 10g of zinc chloride, and ball milled at 500rpm for 0.5h at a ball-to-material ratio of 10:1. The obtained product was calcined at 800°C for 1h under nitrogen. Then, the obtained powder was immersed in a mixed solution of sodium molybdate and thiourea, wherein the mass of sodium molybdate was 5g, the molar ratio of sodium molybdate to thiourea was 1:2, and the total volume of the solution was 500ml. It was hydrothermally treated at 160°C for 12h, and the obtained material was filtered, washed with water, and dried to obtain asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material.
[0054] See also Figure 1 The composite material 0.2Ag prepared in Example 1 of the present invention -1 Cycle performance diagram; As can be seen from the figure, the negative electrode material prepared in Example 1 is coated on copper foil to prepare the negative electrode, using PP as the separator and 1 mol / L LiPF 6 (The solvent is a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) as the electrolyte and lithium sheets to assemble button cells for electrochemical performance testing, 0.2A g -1 The first specific capacity is 589 mAh g -1 The specific capacity is 476 mAh g after 300 cycles. -1 .
[0055] Example 2
[0056] A method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, comprising the following steps:
[0057] 100g of spherical graphite was oxidized in air at 400°C for 2h, then put into a ball mill together with 15g of asphalt and 2g of sodium carbonate, and ball milled at 200rpm for 2h at a ball-to-material ratio of 40:1. The obtained product was calcined at 1200°C for 3h under argon. Then, the obtained powder was immersed in a mixed solution of sodium molybdate and thiourea, wherein the mass of sodium molybdate was 20g, the molar ratio of sodium molybdate to thiourea was 1:2, and the total volume of the solution was 2000ml. It was hydrothermally treated at 220°C for 5h, and the obtained material was filtered, washed with water, and dried to obtain asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material.
[0058] See also Figure 2 The composite material 0.3Ag prepared in Example 2 of the present invention -1 Cycle performance diagram; As can be seen from the figure, the negative electrode material prepared in Example 2 is coated on copper foil to prepare the negative electrode, using PP as the separator and 1 mol / L LiPF 6 (The solvent is a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) as the electrolyte and lithium sheets to assemble button cells for electrochemical performance testing, 0.3A g -1 The initial specific capacity is 521 mAh g -1 The specific capacity is 417 mAh g after 300 cycles. -1 .
[0059] Example 3
[0060] A method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, comprising the following steps:
[0061] 100g of spherical graphite was oxidized in oxygen at 250°C for 8h, then put into a ball mill together with 10g of asphalt and 5g of sodium chloride, and ball milled at 300rpm for 1h at a ball-to-material ratio of 20:1. The obtained product was calcined at 900°C for 1.5h under nitrogen. Then, the obtained powder was immersed in a mixed solution of sodium molybdate and thiourea, wherein the mass of sodium molybdate was 10g, the molar ratio of sodium molybdate to thiourea was 1:2, and the total volume of the solution was 1000ml. It was hydrothermally treated at 180°C for 12h, and the obtained material was filtered, washed with water, and dried to obtain asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material.
[0062] Example 4
[0063] A method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, comprising the following steps:
[0064] 100g of spherical graphite was oxidized in air at 300°C for 6h, then put into a ball mill together with 12g of asphalt and 8g of zinc chloride, and ball milled at 400rpm for 1.5h at a ball-to-material ratio of 30:1. The obtained product was calcined at 1000°C for 2h under argon. Then, the obtained powder was immersed in a mixed solution of sodium molybdate and thiourea, wherein the mass of sodium molybdate was 15g, the molar ratio of sodium molybdate to thiourea was 1:2, and the total volume of the solution was 1500ml. It was hydrothermally treated at 200°C for 10h, and the obtained material was filtered, washed with water, and dried to obtain asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material.
[0065] Example 5
[0066] A method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, comprising the following steps:
[0067] 100g of spherical graphite was oxidized at 350°C in air for 4h, then put into a ball mill together with 14g of asphalt and 10g of sodium carbonate, and ball milled at 500rpm for 2h at a ball-to-material ratio of 40:1. The obtained product was calcined at 1100°C for 2.5h under nitrogen. Then, the obtained powder was immersed in a mixed solution of sodium molybdate and thiourea, wherein the mass of sodium molybdate was 20g, the molar ratio of sodium molybdate to thiourea was 1:2, and the total volume of the solution was 2000ml. It was hydrothermally treated at 220°C for 8h, and the obtained material was filtered, washed with water, and dried to obtain asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material.
[0068] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide, characterized in that: The following steps are involved: S1: oxidizing spherical graphite to obtain a first precursor; S2: ball-milling the asphalt, the pore-forming agent and the first precursor obtained in step S1 to obtain a second precursor; S3: calcining the second precursor obtained in step S2 to obtain a third precursor; S4: immersing the third precursor obtained in step S3 in a mixed aqueous solution of sodium molybdate and thiourea to carry out a hydrothermal reaction, filtering and drying to obtain a spherical graphite negative electrode material modified by asphalt and molybdenum disulfide.
2. The method for preparing the asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material according to claim 1, characterized in that: In step S1, the atmosphere of the oxidation treatment is air or oxygen; the temperature of the oxidation treatment is 200-400° C.; and the time of the oxidation treatment is 2-8 hours.
3. The method for preparing the asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material according to claim 1, characterized in that: In step S2, the mass ratio of the first precursor: asphalt: pore-forming agent is 100: (5-15): (2-10).
4. The method for preparing the asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material according to claim 1, characterized in that: In step S2, the pore-forming agent is at least one of zinc chloride, sodium carbonate and sodium chloride.
5. The method for preparing the asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material according to claim 1, characterized in that: In step S2, the rotation speed of the ball mill is 200-500 rpm; the ball-to-material ratio is (10-40):1; and the ball milling time is 0.5-2h.
6. The method for preparing the asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material according to claim 1, characterized in that: In step S3, the calcination temperature is 800-1200° C.; the calcination time is 1-3 hours; and the calcination atmosphere is nitrogen or argon.
7. The method for preparing the asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material according to claim 1, characterized in that: In step S4, in the mixed aqueous solution of sodium molybdate and thiourea, the molar ratio of sodium molybdate to thiourea is 1:2; the mass ratio of the third precursor to sodium molybdate is 100:(5-20); and the dosage ratio of the third precursor to the total volume of the solution is 1 g:(5-20) mL.
8. The method for preparing the asphalt-coordinated molybdenum disulfide-modified spherical graphite negative electrode material according to claim 1, characterized in that: In step S4, the temperature of the hydrothermal reaction is 160-220° C.; the time of the hydrothermal reaction is 5-12 hours.
9. The asphalt-modified spherical graphite negative electrode material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the asphalt prepared by the preparation method according to any one of claims 1 to 8 in conjunction with molybdenum disulfide modified spherical graphite negative electrode material in the preparation of lithium ion battery negative electrode materials.
Citation Information
Patent Citations
Torispherical cathode material for lithium ion battery and preparation method thereof
CN101916844A
Graphite-coated MoS2 composite negative electrode material, preparation method thereof and sulfide solid-state battery
CN118398783A
Lithium-ion battery negative electrode material, preparation method therefor, and lithium-ion battery
WO2013029212A1
High-capacity highly stable silicon-carbon negative electrode material and preparation method therefor