Method for preparing zinc oxide by purifying zinc ash through improved acid leaching method

Through the modified acid leaching method, dilute sulfuric acid and polymer flocculant are used to remove impurity iron, combined with ammonium bicarbonate precipitation, control the particle size, and finally calcined to produce high-purity ultrafine nano zinc oxide, which solves the low leaching rate in the wet zinc smelting process and The problem of low purity has achieved efficient recycling of zinc solid waste and the preparation of nano zinc oxide.

CN118954574APending Publication Date: 2024-11-15SHIJIAZHUANG UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411315633.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing wet zinc smelting process, the leaching rate of the acid leaching method is low and the product purity is not high. The high iron content leads to unstable zinc oxide quality, making it difficult to effectively recycle zinc solid waste.

Method used

At a certain temperature, the zinc ash is leaching through dilute sulfuric acid, and the impurity iron is removed through oxidation reaction and polymer flocculant. After the replacement reaction, the refined zinc sulfate solution is obtained. Then, it reacts with ammonium bicarbonate to precipitate to form alkaline zinc carbonate, which passes through surfactivity The agent controls the particle size and finally produces high-purity ultrafine nano zinc oxide through calcination.

Benefits of technology

It significantly improves the leaching rate of zinc and the purity of zinc oxide, improves the crystallization performance and particle size distribution of the product, makes the morphology and particle size of zinc oxide more uniform, and solves the low leaching rate and low purity of traditional acid leaching methods. Problem, providing a high-value utilization method for zinc solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954574A_ABST
    Figure CN118954574A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing zinc oxide by purifying zinc ash through an improved acid leaching method, which comprises the following steps of: preparing zinc oxide by taking waste zinc ash of a zinc smelting plant as a raw material, leaching the zinc ash through sulfuric acid at a certain temperature through an improved traditional acid leaching method to generate a crude zinc sulfate solution, and effectively removing impurity iron through an oxidation reaction by utilizing the coagulation effect of a polymeric flocculant; removing other heavy metal impurities after replacement reaction to obtain a refined zinc sulfate solution, reacting the refined zinc sulfate solution with ammonium bicarbonate under the action of a surfactant to obtain basic zinc carbonate precipitate, controlling the product morphology and particle size through the surfactant, and finally obtaining the high-purity superfine nano zinc oxide through filtering, washing, drying and calcining. And controllable preparation of the morphology and the particle size of the zinc oxide product is realized. According to the method, the zinc ash solid waste is recycled, environmental pollution and resource waste caused by accumulation of solid waste such as zinc-containing waste residues and smoke dust are effectively solved, and meanwhile the dilemma that the zinc ore storage amount supply is insufficient in China is relieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal oxide preparation methods, and in particular to a method for preparing zinc oxide by purifying zinc ash using an improved acid leaching method. Background Art

[0002] Zinc oxide is an important basic chemical raw material, widely used in rubber production, paint additives, enamel products, cables, biomedicine and other fields. With the gradual increase in demand for zinc oxide, my country is facing the dilemma of insufficient supply of zinc ore reserves; and the accumulation and stacking of zinc-containing waste slag, smoke and other solid wastes produced by smelting enterprises have brought environmental pollution and waste of resources. Therefore, the effective recycling and utilization of non-traditional zinc resources is of great significance to alleviate the contradiction between supply and demand and ensure the healthy and sustainable development of the zinc industry.

[0003] There are two main methods for recycling zinc-containing solid waste to prepare zinc oxide: pyrometallurgy and hydrometallurgy. Pyrometallurgy is the process of extracting metallic zinc from zinc oxide materials at high temperature using carbon as a reducing agent. Due to the disadvantages of this method, such as high cost, high energy consumption, unstable product quality, and serious pollution, it has been gradually replaced by hydrometallurgy. The hydrometallurgy is to dissolve the zinc ions in the zinc ash raw material directly into the solution through liquid phase leaching, so as to further refine and process it. Cui Wenguang, Gao Yanlei, Ci Lijie, et al. Research on the technology of producing high-purity zinc oxide from zinc ash direct method [J]. Sintering and Pelletizing, 2020, 45(03): 49. The leaching methods include acid leaching, ammonia leaching, ammonium chloride solution, and solvent extraction, which are relatively mature recycling processes. The amount of zinc-containing solid waste treated by the wet method is smaller than that of the pyrometallurgy, but it has certain advantages, such as strong universality of raw materials and high purity of the obtained products. In addition, extraction technology can be used for further efficient wet purification.

[0004] Hydrometallurgy is divided into alkaline and acid processes according to the different leaching solutions. The alkaline leaching process usually uses caustic soda or ammonium carbonate as the leaching agent, and basic zinc carbonate or activated zinc oxide is the final product. The advantages of the alkaline leaching process are good metal separation and high product purity; the disadvantages are low metal leaching rate (about 85%-90%), and the reprocessing of the ammonia solution involved increases the cost. If necessary, water washing or alkaline washing is required to remove soluble fluorine and chlorine. In addition, zinc ferrite and zinc sulfate are difficult to leach with alkali. The mainstream leaching agent for acid leaching is sulfuric acid or hydrochloric acid, and the leachate is purified by extraction and other processes, and then electrolytic zinc or basic zinc carbonate is produced. The advantages of the acid leaching process are high reaction efficiency and high metal leaching rate (generally greater than 95%), but the iron content of the leachate of this process is relatively high, resulting in problems such as low product purity. Summary of the invention

[0005] In order to improve the leaching rate of hydrometallurgical zinc and the purity of zinc oxide products, the present invention improves the traditional acid leaching process, leaches zinc ash with sulfuric acid at a certain temperature to generate a crude zinc sulfate solution, and effectively removes impurity iron by the coagulation effect of a polymer flocculant through an oxidation reaction, removes other heavy metal impurities after a displacement reaction to obtain a refined zinc sulfate solution, reacts with ammonium bicarbonate under the action of a surfactant to obtain a basic zinc carbonate precipitate, controls the product particle size through a surfactant, and finally obtains high-purity ultrafine nano zinc oxide through filtering, washing, drying and calcining.

[0006] The technical solution of the present invention:

[0007] A method for preparing zinc oxide by purifying zinc ash using an improved acid leaching method, comprising the following steps:

[0008] S1. Zinc ash pretreatment

[0009] S11, acid leaching: add dilute sulfuric acid to the zinc ash, stir evenly, and heat for acid leaching;

[0010] S12, dechlorination: continue stirring under heating conditions to remove chlorine;

[0011] S2. Impurity Removal

[0012] S21, oxidative removal: add H2O2 to the dechlorinated leaching solution to remove Fe 2+ Oxidized to Fe 3+ , then add a high molecular weight flocculant, and adjust the pH to 4-5 with diluted ammonia water, let it stand and then filter it, and retain the filtrate;

[0013] S22, replacement and impurity removal: heating the filtrate, adding zinc powder and stirring, filtering with suction, and the filtrate left by the filtration is the refined zinc sulfate solution;

[0014] S3, zinc precipitation

[0015] Place the refined zinc sulfate solution in a water bath, stir, then add ammonium carbonate and a surfactant, the resulting white precipitate is the precursor basic zinc carbonate, filter and retain the filter cake, wash with distilled water, then wash with anhydrous ethanol 2-3 times, dry to obtain a dry powder;

[0016] S4. Calcination

[0017] The dried powder was calcined in a muffle furnace to obtain zinc oxide.

[0018] Preferably, the zinc ash and dilute sulfuric acid n(H2SO4) in S11: n(Zn 2+ )=0.5-2:1;

[0019] The concentration of dilute sulfuric acid is 1-8 molL -1 ;

[0020] The temperature of heated acid leaching is 30-60℃ and the time is 30-40min.

[0021] Preferably, the heating temperature in S12 is 70-90° C., and the stirring time is continued for 2-2.5 h;

[0022] The spilled chlorine is absorbed by alkaline solution.

[0023] Preferably, the mass ratio of FeSO4: polymer flocculant: H2O2 in the leaching solution in S21 is 1-30:1:700-3000;

[0024] The mass concentration of H2O2 is 30%;

[0025] The mass concentration of diluted ammonia water is 12.5%;

[0026] The standing time is 30-40 minutes.

[0027] Preferably, the polymer flocculant is an organic polymer flocculant, and the organic polymer flocculant includes polyacrylamide;

[0028] Polyacrylamide includes cationic polyacrylamide, anionic polyacrylamide and zwitterionic polyacrylamide. Preferably, the filtrate in S22 is heated to 50-70°C;

[0029] The amount of zinc powder added is 0.06-0.2 parts by mass per part by mass of zinc ash;

[0030] The stirring time is 30-40 minutes.

[0031] Preferably, the temperature of the water bath in S3 is 60-63° C.;

[0032] Ammonium carbonate: in refined zinc sulfate solution, n(NH4HCO3):n(ZnSO4)=2.0-2.25:1;

[0033] The amount of surfactant used is 0-0.08g ml -1 per ml of solution;

[0034] The drying temperature is 100-120℃.

[0035] Preferably, the surfactant includes polyethylene glycol 400, sodium lauryl sulfate, hexadecyltrimethylammonium bromide and polyvinyl pyrrolidone.

[0036] Preferably, the calcination temperature in S4 is 600-750° C., and the calcination time is 3-5 h.

[0037] Preferably, the method comprises the following steps:

[0038] S1. Zinc ash pretreatment

[0039] S11, acid leaching: add 1-3 molL to the zinc ash -1的 Dilute sulfuric acid, stir evenly, 40-60℃, react for 30min;

[0040] S12, dechlorination: continue stirring at 85℃ for 2h to remove chlorine, and absorb the overflowed chlorine with alkali solution; S2, impurity removal

[0041] S21, oxidation removal: add H2O2 to the leaching solution to remove Fe 2+ Oxidized to Fe 3+ , then add polyacrylamide, and adjust the pH to 4-5 with diluted ammonia water, let it stand for 30 minutes, then filter and retain the filtrate;

[0042] S22, replacement and impurity removal: heat the filtrate to 60°C, add zinc powder and stir for 30 minutes; filter with suction, and the remaining filtrate is the refined zinc sulfate solution;

[0043] S3, zinc precipitation

[0044] Place the refined zinc sulfate solution in a water bath at 60°C, stir, then add ammonium carbonate and polyethylene glycol 400, the generated white precipitate is the precursor basic zinc carbonate, filter and retain the filter cake, wash it with distilled water, then wash it with anhydrous ethanol 2-3 times, and dry it at 120°C to obtain a dry powder;

[0045] S4. Calcination

[0046] The dried powder is calcined at 650-750° C. in a muffle furnace to obtain zinc oxide.

[0047] Beneficial effects of the present invention:

[0048] (1) During the acid leaching process, the zinc leaching rate in the zinc ash raw material is significantly affected by the acid leaching temperature and the amount of acid used. When the acid leaching temperature rises from 30 to 50°C, the leaching rate increases from 89.98% to 93.86%; as the temperature continues to rise, the leaching rate decreases significantly, and the most suitable acid leaching temperature is 50°C. When the amount of sulfuric acid changes from n(H2SO4):n(Zn 2+ )=1.15, the zinc leaching rate is the highest, reaching 98.37%.

[0049] (2) In the further impurity removal process, dechlorination of the leachate can improve the crystallization properties of the zinc oxide product and increase the crystal size. 2+ At pH 3.7, it is converted into colloidal Fe(OH)3, and the colloidal flocculation and filtration of the polymer flocculant polyacrylamide are used. The optimized dosage of polyacrylamide is 0.04 g ml -1 (crude leachate).

[0050] (3) The surfactant polyethylene glycol affects the morphology and size of basic zinc carbonate during its growth process, thereby achieving the regulation of the morphology and particle size of zinc oxide products. The dosage of polyethylene glycol 400 is 0-0.08g

[0051] ml -1 Within this range, the morphology of zinc oxide gradually changes from an irregular shape to a sphere with a relatively uniform particle size, and the particle size decreases from 258nm to 59nm.

[0052] The modified acid leaching method proposed in the present invention provides a practical way for high-value utilization of zinc solid waste and preparation of nano zinc oxide products with controllable particle size, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 The XRD patterns of zinc oxide prepared by the present invention with or without dechlorination operation;

[0054] Figure 2 The figure is a curve diagram showing the concentration of iron ions according to the present invention changing with the amount of acrylamide used;

[0055] Figure 3 The XRD spectrum of zinc oxide of the present invention; the dosage of polyethylene glycol 400 is (a) 0, (b) 0.02, (c) 0.04, (d) 0.06, (e) 0.08gml -1 ;

[0056] Figure 4 (a) shows polyethylene glycol 0gml -1 SEM characterization of zinc oxide sample morphology and particle size distribution under different dosages;

[0057] Figure 4(b) shows polyethylene glycol 0.02 g ml -1 SEM characterization of zinc oxide sample morphology and particle size distribution under different dosages;

[0058] Figure 4(c) shows polyethylene glycol 0.04 g ml -1 SEM characterization of zinc oxide sample morphology and particle size distribution under different dosages;

[0059] Figure 4(d) shows polyethylene glycol 0.06 g ml -1 SEM characterization of zinc oxide sample morphology and particle size distribution under different dosages;

[0060] Figure 4(e) shows polyethylene glycol 0.08 g ml -1 SEM characterization of the morphology of zinc oxide samples under different dosages and their particle size distribution. DETAILED DESCRIPTION

[0061] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0062] Embodiment 1

[0063] Acid leaching: Slowly add 141 ml of dilute sulfuric acid (1 mol L -1 ), and stir evenly, react at 50°C for 30 minutes.

[0064] Dechlorination: Continue stirring at 85°C for 2 hours to remove chlorine, and absorb the overflowing gas with alkaline solution.

[0065] Remove impurities

[0066] Oxidation and impurity removal: Add 120gH2O2 to the leaching solution to remove Fe 2+ Oxidized to Fe 3+ , add 0.04g polyacrylamide per milliliter of leaching solution, and adjust the pH to 4-5 with 12.5% ​​(1:1) diluted ammonia water, let it stand for 30 minutes, then filter and retain the filtrate.

[0067] Replacement and impurity removal: Heat the filtrate to 60°C, add 1.2g zinc powder and stir for 30 minutes. Filter by suction, and the remaining filtrate is the refined zinc sulfate solution.

[0068] Zinc precipitation: Place the above refined zinc sulfate solution in a water bath at about 60°C, stir rapidly, and then add 17g of ammonium carbonate and 0.08gmL -1 Polyethylene glycol 400, the generated white precipitate is the precursor basic zinc carbonate, which is filtered to retain the filter cake, which is fully washed with distilled water, then washed with anhydrous ethanol 2-3 times, and dried at 120°C to obtain a dry powder.

[0069] Calcination: The above dried powder was calcined at 750°C in a muffle furnace to obtain zinc oxide.

[0070] In order to improve the quality of zinc oxide products prepared from zinc solid waste, the effects of acid leaching temperature, acid leaching dosage, dechlorination treatment, flocculant dosage, ammonium bicarbonate dosage, polyethylene glycol 400 dosage on zinc oxide products were investigated.

[0071] The following conditional embodiments only change a single condition relative to Example 1, as follows:

[0072] (1) Effect of acid leaching temperature on zinc leaching rate

[0073] When the reaction time is 30min, n(H2SO4):n(Zn 2+)=1.0, the zinc ash was acid-leached in the range of 30~60℃ to explore the effect of temperature on the leaching rate of zinc in the zinc ash. (Note: The zinc ion content in the zinc ash before acid leaching and the zinc ion content in the solution after acid leaching were measured by the xylenol orange method, and the ratio of the latter to the former is the zinc leaching rate; the following determinations of zinc ion content were all measured by the xylenol orange method)

[0074] Table 1 Effect of temperature on zinc leaching rate

[0075]

[0076] It can be seen from Table 1 that the leaching rate of zinc in the raw material shows a volcanic shape with the change of acid leaching temperature. The zinc leaching rate reaches the highest value at a temperature of 50°C. When the temperature is lower than 50°C, the zinc leaching rate increases with the increase of temperature. When the temperature is higher than 50°C, the zinc leaching rate decreases significantly with the increase of temperature.

[0077] (2) Effect of acid dosage on zinc leaching rate

[0078] Under the conditions of acid leaching temperature of 50℃ and reaction time of 30min, the effect of acid dosage on the zinc leaching rate in zinc ash was investigated.

[0079] Table 2 Effect of sulfuric acid dosage on zinc leaching rate

[0080]

[0081] From Table 2, it can be seen that when the reaction time is 30 min and the temperature is 50 ° C, the amount of acid used is n(H2SO4): n(Zn 2+ )=1.15, the zinc leaching rate is the highest, reaching 98.37%.

[0082] (3) No dechlorination operation

[0083] Slowly add 141 ml of dilute sulfuric acid (1 mol / L) to 10 g of zinc ash. -1 ), and stir evenly, react at 50°C for 30 minutes.

[0084] Adding H2O2 to the leaching solution will 2+ Oxidized to Fe 3+ , then add 0.04gmL -1 Polyacrylamide, and adjust pH to 4-5 with diluted ammonia 12.5% ​​(1:1), let stand for 30 minutes and then filter, retain the filtrate. Replacement and impurity removal: heat the filtrate to 60°C, add 1.2g zinc powder and stir for 30 minutes. Filter and obtain refined zinc sulfate solution.

[0085] Place the zinc sulfate solution in a water bath at about 60°C, stir rapidly, and then add 17 g of ammonium carbonate and 0.08 g mL -1 Polyethylene glycol 400, the generated white precipitate is the precursor basic zinc carbonate, which is filtered to retain the filter cake, which is fully washed with distilled water, then washed with anhydrous ethanol 2-3 times, and dried at 120°C to obtain a dry powder.

[0086] The dried powder was calcined at 750° C. in a muffle furnace to obtain zinc oxide.

[0087] The XRD analysis of zinc oxide samples obtained by dechlorination and without dechlorination was compared. Figure 1 .Depend on Figure 1 It can be seen that hexagonal wurtzite ZnO (PDF#75-0576) can be obtained with or without the dechlorination step in the pretreatment. Comparing the two XRD patterns, it is found that the XRD diffraction peak of the zinc oxide sample prepared by dechlorination is sharp and has no impurity peaks; while the XRD diffraction peak of the zinc oxide sample prepared without dechlorination is broad and the grain size is smaller.

[0088] (4) Effect of flocculants

[0089] Oxidation removal (ferrous ion)

[0090] Fe in zinc ash 2+ After acid leaching, a large amount of ferrous ions are present in the leaching solution. In order to further remove ferrous ions, an appropriate amount of H2O2 is added to the leaching solution to remove Fe 2+ Oxidized to Fe 3+ After that, gradually add ammonia water to adjust the pH value of the solution. When pH = 1.7, Fe(OH)3 begins to form, and the reaction is complete when pH = 3.7. Since the particle size of Fe(OH)3 colloid is very fine and easy to filter, in order to improve the filtration efficiency, a polymer flocculant is added before adjusting the pH. Under the flocculation effect, the Fe(OH)3 colloid particles will agglomerate together. After standing and aging for 30 minutes, it is filtered, and the iron removal effect is good.

[0091] In order to optimize the dosage of high molecular weight flocculant polyacrylamide, the dosage of 0-0.05 g was investigated. The initial iron content in zinc ash was determined by spectrophotometry to be about 7.2 × 10 -4 μgml -1 The residual amount of iron in the filtrate after oxidation and impurity removal is as follows: Figure 2 .

[0092] (5) Effect of the dosage of ammonium bicarbonate on the yield

[0093] Add ammonium bicarbonate to the zinc sulfate solution after impurities are removed. Since ammonium bicarbonate undergoes a double hydrolysis reaction, the reaction product combines with zinc ions to eventually form a white precipitate - basic zinc carbonate. The reaction equation is: 6NH4HCO3+3ZnSO4=ZnCO3·2Zn(OH)2·H2O↓+5CO2↑+3(NH4)2SO4. Theoretically, the ratio of ammonium bicarbonate to zinc sulfate is 2:1.

[0094] Table 3 Effect of ammonium bicarbonate dosage on yield

[0095] <![CDATA[n(NH4HCO3):1.902.02.12.152.202.25]]> Yield / % 77.55 91.78 98.30 98.55 98.96 93.88

[0096] Based on the reaction formula n(NH4HCO3):n(ZnSO4)=2:1, the effect of different NH4HCO3 dosages on the yield of zinc oxide was investigated. As shown in Table 3, the dosage of ammonium bicarbonate has a greater impact on the yield, and insufficient or excessive ammonium bicarbonate dosage will reduce the yield.

[0097] Zinc oxide yield calculation

[0098]

[0099] Note: In formula (1), actual zinc oxide output is the actual output mass of zinc oxide corresponding to the unit mass of zinc ash input.

[0100] (6) Effect of the dosage of surfactant polyethylene glycol 400 on the morphology and particle size of zinc oxide

[0101] Polyethylene glycol dosage, from 0 to 0.08 gml -1 In the range of 0, 0.02, 0.04, and 0.06 g mL-1, the effects on the particle size and morphology of ZnO, such as Figure 3 As shown in Figure 4 (a), (b), (c), and (d), (e) is 0.08 g ml -1 .

[0102] like Figure 3 As shown in the figure, the XRD diffraction peak positions and intensities of all samples correspond to the ZnO standard card PDF#75-0576, indicating that all samples are hexagonal wurtzite structure ZnO. Further comparison of the XRD spectra of each sample shows that the sample (a) prepared without adding surfactant has a sharp diffraction peak and a narrow half-height width of the diffraction peak. The half-height width of the diffraction peak of zinc oxide (b), (c), (d), and (e) obtained after using surfactant gradually widens with the increase of the amount of polyethylene glycol 400. According to the Scherrer formula, it can be inferred that the more polyethylene glycol 400 is used, the wider the half-height width of the diffraction peak and the smaller the particle size; the use of surfactant significantly affects the particle size of ZnO.

[0103] As shown in Figure 4(a), the zinc oxide sample without adding surfactant has irregular block and granular morphology, uneven particle size and wide particle size range (100-500nm); as shown in Figure 4(b), the zinc oxide with a small amount of polyethylene glycol 400 added is irregular rectangular, ellipsoid and sphere, and the particle distribution is uneven; as can be seen from Figures 4(c), 4(d) and 4(e), with the increase of the amount of polyethylene glycol 400, the morphology of zinc oxide gradually changes to a more regular spherical shape and forms a beaded shape; the particle size of the zinc oxide sample becomes smaller and smaller, and the particle size distribution range is about 30 to 130nm.

[0104] Embodiment 2

[0105] Acid leaching: Slowly add 90 ml of dilute sulfuric acid (1.5 mol / L) to 10 g of zinc ash. -1 ), and stir evenly, react at 60℃ for 30min.

[0106] Dechlorination: Continue stirring at 85°C for 2 hours to remove chlorine, and absorb the overflowing gas with alkaline solution.

[0107] Remove impurities

[0108] Oxidation and impurity removal: Add 100gH2O2 to the leaching solution to remove Fe 2+ Oxidized to Fe 3+ , add 0.1g sodium alginate to each milliliter of the leaching solution, and adjust the pH to 4-5 with 12.5% ​​diluted ammonia water. After standing for 30 minutes, filter and retain the filtrate.

[0109] Replacement and impurity removal: Heat the filtrate to 60°C, add 2g zinc powder and stir for 30 minutes. Filter by suction, and the remaining filtrate is the refined zinc sulfate solution.

[0110] Zinc precipitation: Place the above refined zinc sulfate solution in a water bath at about 60°C, stir rapidly, and then add 17g of ammonium carbonate and 0.08gmL -1 Hexadecyltrimethylammonium bromide, the generated white precipitate is the precursor basic zinc carbonate, filtered to retain the filter cake, after fully washing with distilled water, then washed with anhydrous ethanol 2-3 times, dried at 120 ° C to obtain dry powder.

[0111] Calcination: The dried powder was calcined at 650°C in a muffle furnace to obtain zinc oxide.

[0112] Embodiment 3

[0113] Acid leaching: Slowly add 80 ml of dilute sulfuric acid (2 mol / L) to 10 g of zinc ash. -1 ), and stir evenly, react at 60℃ for 30min.

[0114] Dechlorination: Continue stirring at 90°C for 2 hours to remove chlorine, and absorb the overflowing gas with alkaline solution.

[0115] Remove impurities

[0116] Oxidation and impurity removal: Add 70gH2O2 to the leaching solution to remove Fe 2+ Oxidized to Fe 3+ , add 0.1g polyacrylamide to each milliliter of the leaching solution, and adjust the pH to 4-5 with 12.5% ​​diluted ammonia water. After standing for 30 minutes, filter and retain the filtrate.

[0117] Replacement and impurity removal: Heat the filtrate to 60°C, add 0.6g zinc powder and stir for 30 minutes. Filter by suction, and the remaining filtrate is the refined zinc sulfate solution.

[0118] Zinc precipitation: Place the above refined zinc sulfate solution in a water bath at about 60°C, stir rapidly, then add 17g ammonium carbonate and 0.1gmL -1 Polyvinyl pyrrolidone, the generated white precipitate is the precursor basic zinc carbonate, which is filtered to retain the filter cake, which is fully washed with distilled water, then washed with anhydrous ethanol 2-3 times, and dried at 120°C to obtain a dry powder.

[0119] Calcination: The above dried powder was calcined at 750°C in a muffle furnace to obtain zinc oxide.

[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing zinc oxide by purifying zinc ash using an improved acid leaching method, characterized in that: The following steps are involved: S1. Zinc ash pretreatment S11, acid leaching: add dilute sulfuric acid to the zinc ash, stir evenly, and heat for acid leaching; S12, dechlorination: continue stirring under heating conditions to remove chlorine; S2. Impurity Removal S21, oxidative removal: add H2O2 to the dechlorinated leaching solution to remove Fe 2+ Oxidized to Fe 3+ , then add a high molecular weight flocculant, and adjust the pH to 4-5 with diluted ammonia water, let it stand and then filter it, and retain the filtrate; S22, replacement and impurity removal: heating the filtrate, adding zinc powder and stirring, filtering with suction, and the filtrate left by the filtration is the refined zinc sulfate solution; S3, zinc precipitation Heat the refined zinc sulfate solution in a water bath, stir, then add ammonium carbonate and a surfactant, the generated white precipitate is the precursor basic zinc carbonate, filter and retain the filter cake, wash with distilled water, then wash with anhydrous ethanol, dry to obtain dry powder; S4. Calcination The dried powder is calcined to obtain zinc oxide.

2. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: Zinc ash and dilute sulfuric acid n(H2SO4) in S11: n(Zn 2+ )=0.5-2:1; The concentration of dilute sulfuric acid is 1-8 molL -1 ; The temperature of heated acid leaching is 30-60℃ and the time is 30-40min.

3. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: In S12, the heating temperature is 70-90°C, and the stirring time is continued for 2-2.5h; The spilled chlorine is absorbed by alkaline solution.

4. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: The mass ratio of FeSO4: polymer flocculant: H2O2 in the leaching solution of S21 is 1-30:1:700-3000; The mass concentration of H2O2 is 30%; The mass concentration of diluted ammonia water is 12.5%; The standing time is 30-40 minutes.

5. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: The polymer flocculant is an organic polymer flocculant, and the organic polymer flocculant includes polyacrylamide; Polyacrylamide includes cationic polyacrylamide, anionic polyacrylamide and zwitterionic polyacrylamide.

6. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: The filtrate in S22 is heated to 50-70°C; The amount of zinc powder added is 0.06-0.2 parts by mass per part by mass of zinc ash; The stirring time is 30-40 minutes.

7. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: The temperature of the water bath in S3 is 60-63°C; Ammonium carbonate: in refined zinc sulfate solution, n(NH4HCO3):n(ZnSO4)=2.0-2.25:1; The amount of surfactant used is 0-0.08g ml per ml of solution -1 ; The drying temperature is 100-120℃.

8. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 7, characterized in that: The surfactant includes polyethylene glycol 400, sodium lauryl sulfate, hexadecyltrimethylammonium bromide and polyvinyl pyrrolidone.

9. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: The calcination temperature in S4 is 600-750°C, and the calcination time is 3-5h.

10. The method for preparing zinc oxide by purifying zinc ash by improved acid leaching method according to claim 1, characterized in that: The following steps are involved: S1. Zinc ash pretreatment S11, acid leaching: add 1-3 molL to the zinc ash -1的 Dilute sulfuric acid, stir evenly, 40-60℃, react for 30min; S12, dechlorination: continue stirring at 85°C for 2h to remove chlorine, and absorb the overflowed chlorine with alkali solution; S2. Impurity Removal S21, oxidation removal: add H2O2 to the leaching solution to remove Fe 2+ Oxidized to Fe 3+ , then add polyacrylamide, and adjust the pH to 4-5 with diluted ammonia water, let it stand for 30 minutes, then filter and retain the filtrate; S22, replacement and impurity removal: heat the filtrate to 60°C, add zinc powder and stir for 30 minutes; filter with suction, and the remaining filtrate is the refined zinc sulfate solution; S3, zinc precipitation Place the refined zinc sulfate solution in a water bath at 60°C, stir, then add ammonium carbonate and polyethylene glycol 400, the generated white precipitate is the precursor basic zinc carbonate, filter and retain the filter cake, wash it with distilled water, then wash it with anhydrous ethanol 2-3 times, and dry it at 120°C to obtain a dry powder; S4. Calcination The dried powder is calcined at 650-750° C. in a muffle furnace to obtain zinc oxide.