Porous shell structure Co3O4-SnO2 in-plane heterojunction, preparation method and application of porous shell structure Co3O4-SnO2 in-plane heterojunction as hydrogen sensor
Synthesis of the in-plane heterojunction of the porous shell structure Co3O4-SnO2 through the template method, solving the problems of low sensitivity and high working temperature of the hydrogen sensor, achieving high sensitivity and low power consumption hydrogen detection, and excellent material stability and selectivity , suitable for hydrogen sensor applications.
Patent Information
- Application Number
- CN202411158725.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
AI Technical Summary
Existing hydrogen sensors have the disadvantages of low sensitivity, high operating temperature and poor stability, making it difficult to detect high sensitivity, low power consumption and excellent selectivity of hydrogen.
The multi-shell structure SnO2 precursor was prepared by the template method to synthesize the in-plane heterojunction of the porous shell structure Co3O4-SnO2 through hydrothermal reaction of different carbon sources and tin compounds, and calcined under high temperature conditions to form in-plane heterojunction of Co3O4-SnO2 The junction is used to form the same two-dimensional in-plane structure of Co3O4 and SnO2 by using Galvanic replacement reaction, increasing the grain boundary contact interface and coordination unsaturation site.
实现了在170°C下对50ppm氢气的高灵敏度检测(响应值8.63),降低了工作温度,提高了材料的稳定性和选择性,并降低了制备成本,适合产业化应用。
Smart Images

Figure CN118954582A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic porous material synthesis, and specifically relates to a porous shell structure Co3O4-SnO2 in-plane heterojunction, a preparation method and application in hydrogen sensors. Background Art
[0002] The rapid depletion of fossil fuel resources has attracted attention for the next generation of green fuels. Alternative fuels such as biofuels, biodiesel, and hydrogen (H 2) It is a trend for researchers to meet this demand. With the advancement of hydrogen production and storage technologies such as fuel cells, hydrogen has become one of the best alternatives to fossil fuels with its highest calorific value and zero carbon emissions during combustion. However, one of the biggest dangers of hydrogen fuel is that H2 will spontaneously ignite even at very low concentrations (above 4%) in the atmosphere, which increases the risk of explosion and danger to humans. In addition, hydrogen flames are completely invisible to the naked eye, thus increasing the danger in unfortunate situations. Therefore, considering safety issues, early, accurate, highly selective and highly sensitive detection of hydrogen gas is imperative. In order to mitigate these adverse effects, various sensors for detecting H2 have been developed. Most of them are based on metal oxides (such as SnO2, TiO2, ZnO, WO3, etc.) because of their high sensitivity. However, this sensitivity can only be achieved at higher operating temperatures (>200°C), which raises safety issues because H2 becomes more flammable at high temperatures. According to literature reports, porous shell structure materials are conducive to the diffusion of gas molecules, but the hydrogen sensors prepared therefrom still have disadvantages such as high operating temperature, poor stability and low sensitivity. Therefore, it is necessary to develop a hydrogen sensor with low operating temperature, high sensitivity, low cost and stability.
[0003] CN 110082406 A discloses a xylene gas sensor based on SnO2-Co3O4 heterojunction nanostructure sensitive material and its preparation method, belonging to the technical field of semiconductor oxide gas sensors. The sensor is composed of a ceramic tube substrate with two parallel, annular and mutually independent gold electrodes on the outer surface, a SnO2-Co3O4 heterojunction nanostructure sensitive material coated on the outer surface of the ceramic tube and the gold electrodes, and a nickel-chromium alloy heating wire placed in the ceramic tube; the sensor based on the SnO2-Co3O4 heterojunction nanostructure sensitive material shows excellent sensitivity (101.9-100ppm) and a low detection limit (0.05ppm) to xylene.
[0004] CN 109085210 A relates to an np heterogeneous core-shell structure gas-sensitive material and a preparation method, and specifically relates to a Co3O4@SnO2 core-shell structure gas-sensitive material with a p-type nano Co3O4 as a core and an n-type nano SnO2 as a shell and a preparation method. The gas-sensitive material of the invention avoids the depletion of interface electrons caused by direct exposure of the p-type Co3O4 layer to the air, and on the other hand, improves the band structure of the gas-sensitive material by using the n-type SnO2 of the shell layer, so as to improve the sensitivity and selectivity of the gas-sensitive material to a specific gas.
[0005] However, most of the SnO2-Co3O4 heterojunctions reported so far are out-of-plane heterojunctions, that is, the two components are not in the same two-dimensional plane, while the SnO2-Co3O4 heterojunction of the present invention is an in-plane heterostructure, and its two heterogeneous components are in the same plane. Therefore, more lattice stress and coordination unsaturated sites are generated at the grain boundary contact interface of the two components compared with the traditional out-of-plane heterostructure, and this site becomes an active site for the gas sensing process, providing an active site for activating the target hydrogen and oxygen. This novel structure helps to improve the operating temperature and sensitivity of oxide-type semiconductor hydrogen sensors. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a porous shell structure Co3O4-SnO2 in-plane heterojunction with high sensitivity, low power consumption and excellent selectivity to hydrogen, as well as a preparation method and application in hydrogen sensors in view of the shortcomings of hydrogen sensors such as low sensitivity, high operating temperature and poor stability.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions: The porous shell structure Co3O4-SnO2 in-plane heterojunction of the present invention is synthesized by a template method strategy, and Co3O4 and SnO2 in the porous shell structure are uniformly distributed in the two-dimensional plane of each shell to form a two-dimensional planar heterostructure.
[0008] The present invention also provides a method for preparing a porous shell structure Co3O4-SnO2 in-plane heterojunction: first, different carbon sources are dissolved in water and stirred until transparent and clear; then, the mixture is placed in a reactor for hydrothermal reaction, and the mixed solution after the reaction is centrifugally dried to obtain composite carbon spheres, and the tin compound and the carbon spheres are dissolved in an organic solvent solution, and ultrasonic stirring is performed until they are completely dispersed to obtain a mixed solution, and the mixed solution is stirred and aged at room temperature, and then centrifugally dried and calcined in air at high temperature to obtain a multi-shell structure SnO2 precursor; the prepared multi-shell structure SnO2 precursor and the cobalt compound are dissolved in an organic solvent, and ultrasonic stirring is performed until they are completely dispersed, and then centrifugally dried, and calcined in air to obtain a porous shell structure Co3O4-SnO2 in-plane heterojunction. Specifically, the following steps are included: (1) Preparation of composite carbon spheres: Dissolve different carbon sources in water, stir until transparent and clear, place in a reactor for hydrothermal reaction, and centrifuge and dry the mixed solution after the reaction to obtain composite carbon spheres; (2) Preparation of multi-shell SnO2 precursor: dissolving a tin compound in an organic solvent solution, adding composite carbon spheres, and ultrasonically stirring until completely dispersed to obtain a mixed solution. Stirring and aging the mixed solution at room temperature, centrifugally drying, and calcining in air to obtain a multi-shell SnO2 precursor. (3) Preparation of a porous shell structure Co3O4-SnO2 in-plane heterojunction: dissolving the multi-shell structure SnO2 precursor and the cobalt compound obtained in step (2) in an organic solvent, ultrasonically dissolving and stirring, centrifugally drying, and calcining in air under high temperature conditions to obtain a porous shell structure Co3O4-SnO2 in-plane heterojunction; Furthermore, the carbon source in step (1) is at least two of sucrose, fructose, glucose, lactose, tannic acid, dopamine, and corn starch, and the concentration is 0.1 g / mL to 0.5 g / mL.
[0009] Furthermore, the hydrothermal reaction temperature in step (1) is 160-200° C., and the reaction time is 1-5 h.
[0010] Furthermore, the tin compound in step (2) is one or more of SnCl2, SnSO4, SnCl4 or Sn(NO3)2, the mass ratio of the tin compound to the carbon sphere is 1:5~1:20, and the aging time is 0.5-3h.
[0011] Furthermore, in the step (3), the mass ratio of the multi-shell SnO2 precursor to the cobalt compound is 1:0.1 to 1:0.3; the cobalt compound is one or more of CoCl2, CoSO4, Co(NO3)2, and cobalt acetylacetonate; and the total concentration of the multi-shell SnO2 precursor and the cobalt compound in the mixed solution B is 0.1 g / mL to 0.22 g / mL.
[0012] Furthermore, in step (2) and step (3), the calcination temperature is 400-600° C., the heating rate is 1° C. / min to 5° C. / min, and the calcination time is 1-2 h.
[0013] Furthermore, the organic solvent in step (2) and step (3) is one or more of ethanol, propanol, glycerol and tetrahydrofuran.
[0014] Furthermore, in the steps (1) to (3), the drying temperature is 60-80° C. and the drying time is 4-6 h.
[0015] Furthermore, in the steps (1) to (3), the drying temperature is 60-80° C. and the drying time is 4-6 h.
[0016] The present invention also provides the application of the porous shell structure Co3O4-SnO2 in-plane heterojunction as a gas sensor in a high-sensitivity hydrogen sensor. When the operating temperature is 170°C, the porous shell structure Co3O4 / SnO2 ball as a gas sensor has good selectivity for hydrogen and the sensitivity to 50ppm hydrogen reaches 8.63.
[0017] The key to the innovation of the present invention is to prepare a multi-carbon source composite SnO2 multi-shell structure and successfully construct a Co3O4-SnO2 in-plane heterojunction. There are many hydrogen sensors prepared from porous shell structure materials, but their preparation methods are cumbersome, the operating temperature is high, the stability is poor and the sensitivity is low. The SnO2-Co3O4 heterojunction of the present invention is an in-plane heterostructure, and its two heterogeneous components are in the same plane. Therefore, more lattice stress and coordination unsaturated sites are generated at the grain boundary contact interface of the two components compared to the traditional out-of-plane heterostructure. This site becomes an active site for the gas sensing process and provides an active site for activating the target hydrogen and oxygen. This novel structure helps to improve the operating temperature and sensitivity of oxide-type semiconductor hydrogen sensors.
[0018] The beneficial effects of the present invention are as follows: the present invention synthesizes carbon balls composited with multiple carbon sources, utilizes the different adsorption forces of different carbon sources on the tin source precursor, and finally forms a multi-shell structure SnO2 in the controlled calcination stage. And based on the Galvanic replacement reaction, according to the difference in the redox potential of different metal ions in the solution, an ion replacement reaction is carried out under specific conditions to synthesize the Co3O4-SnO2 in-plane heterogeneous structure. Since the structure is synthesized by an in-situ replacement process, the two components Co3O4 and SnO2 are in the same two-dimensional in-plane structure. Compared with the traditional out-of-plane heterogeneous structure, the structure has more surface coordinated unsaturated atoms and grain boundaries, and has more active sites, so it is beneficial to improve the sensitivity and selectivity to hydrogen; the sensitivity to 50ppm hydrogen at a working temperature of 170°C reaches 8.63, which is lower than the working temperature of the existing hydrogen sensor. The method of the present invention has innovative synthesis, high yield, low preparation cost; the morphology and size of the material are uniform; the response to hydrogen is fast, and it is easy to realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1This is the XRD diagram of the porous shell structure Co3O4-SnO2 in-plane heterojunction prepared in Example 8.
[0021] Figure 2 This is a scanning electron microscope (SEM) image of the porous shell structure Co3O4-SnO2 in-plane heterojunction prepared in Example 8.
[0022] Figure 3 It is the response value of the porous shell structure Co3O4-SnO2 in-plane heterojunction prepared in Example 8 to 50ppm hydrogen at 110-230°C.
[0023] Figure 4 This is a long-term stability test of the porous shell structure Co3O4-SnO2 in-plane heterojunction prepared in Example 8 to 50ppm hydrogen within 30 days. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention, and those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention.
[0025] Example 1 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Take 6 g of glucose and 9 g of sucrose and dissolve them in 40 ml of water. Stir for 10 min until the solution becomes transparent and clear to obtain a mixed solution. Place the solution in a 100 ml reactor and perform a hydrothermal reaction at 160 °C for 2 h. Centrifuge the mixed solution after the reaction and dry the obtained product at 60 °C for 4 h to obtain composite carbon spheres.
[0026] (2) Dissolve 1 g SnCl2 and 5 g composite carbon spheres in 100 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 2 h, then centrifuge and dry at 60 °C for 4 h. Then calcine at 500 °C in a muffle furnace for 1 h at a heating rate of 1 °C / min to obtain a multi-shell SnO2 precursor.
[0027] (3) Dissolve 1 g of the multi-shell SnO2 precursor prepared in step (2) and 0.3 g of CoSO4 in 12 ml of ethanol, stir ultrasonically until completely dispersed, and then centrifuge and dry at 60°C for 4 h. Calcinate at 500°C in a muffle furnace for 1 h at a heating rate of 1°C / min to obtain a porous shell structure Co3O4-SnO2 in-plane heterojunction.
[0028] Example 2 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Take 8 g of glucose and 8 g of sucrose and dissolve them in 40 ml of water. Stir for 10 min until the solution becomes transparent and clear to obtain a mixed solution. Place the solution in a 100 ml reactor for hydrothermal reaction at 180 °C for 2 h. Centrifuge the mixed solution after the reaction and dry the obtained product at 60 °C for 4 h to obtain composite carbon spheres.
[0029] (2) Dissolve 1 g SnCl4 and 10 g composite carbon spheres in 100 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 2 h, then centrifuge and dry at 60 °C for 4 h. Then calcine at 500 °C in a muffle furnace for 1 h at a heating rate of 1 °C / min to obtain a multi-shell structured SnO2 precursor.
[0030] (3) Dissolve 1 g of the multi-shell SnO2 precursor prepared in step (2) and 0.2 g of CoSO4 in 10 ml of propanol, stir ultrasonically until completely dispersed, and then centrifuge and dry at 60°C for 4 h. Calcinate at 500°C in a muffle furnace for 1 h at a heating rate of 1°C / min to obtain a porous shell structure Co3O4-SnO2 in-plane heterojunction.
[0031] Example 3 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Take 6 g of glucose and 10 g of sucrose and dissolve them in 60 ml of water. Stir for 10 min until the solution becomes transparent and clear to obtain a mixed solution. Place the solution in a 100 ml reactor and perform a hydrothermal reaction at 160 °C for 2 h. Centrifuge the mixed solution after the reaction and dry the obtained product at 60 °C for 4 h to obtain composite carbon spheres.
[0032] (2) Dissolve 2 g Sn(NO3)2 and 10 g composite carbon spheres in 200 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 2 h, then centrifuge and dry at 60 °C for 4 h. Then calcine at 500 °C in a muffle furnace for 1 h at a heating rate of 1 °C / min to obtain a multi-shell SnO2 precursor.
[0033] (3) 1.8 g of the multi-shell structured SnO2 precursor prepared in step (2) and 0.5 g of Co(NO3)2 were dissolved in 20 ml of ethanol, ultrasonically stirred until completely dispersed, and then centrifuged and dried at 60°C for 4 h. The mixture was calcined in a muffle furnace at 500°C for 1 h at a heating rate of 1°C / min to obtain a porous shell structured Co3O4-SnO2 in-plane heterojunction.
[0034] Example 4 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Take 8 g of lactose and 10 g of fructose and dissolve them in 60 ml of water. Stir for 10 min until the mixture becomes transparent and clear to obtain a mixed solution. Place the solution in a 100 ml reactor and perform a hydrothermal reaction at 200 °C for 1 h. After the reaction, centrifuge the mixed solution and dry the obtained product at 60 °C for 4 h to obtain composite carbon spheres.
[0035] (2) Dissolve 2 g SnCl2 and 30 g composite carbon spheres in 200 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 1 h, then centrifuge and dry at 60 °C for 4 h. Then calcine at 500 °C in a muffle furnace for 1 h at a heating rate of 1 °C / min to obtain a multi-shell structured SnO2 precursor.
[0036] (3) 1.95 g of the multi-shell structured SnO2 precursor obtained in step (2) and 0.6 g of CoSO4 were dissolved in 25 ml of ethanol, ultrasonically stirred until completely dispersed, and then centrifuged and dried at 60 °C for 4 h. The mixture was calcined in a muffle furnace at 500 °C for 1 h at a heating rate of 1 °C / min to obtain a porous shell structured Co3O4-SnO2 in-plane heterojunction.
[0037] Example 5 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Dissolve 10 g of lactose and 6 g of glucose in 60 ml of water and stir for 10 min until the solution becomes transparent and clear to obtain a mixed solution. Place the solution in a 100 ml reactor and perform a hydrothermal reaction at 200 °C for 2 h. Centrifuge the mixed solution after the reaction and dry the obtained product at 60 °C for 4 h to obtain composite carbon spheres.
[0038] (2) Dissolve 1.5 g SnCl4 and 25 g composite carbon spheres in 150 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 1 h, then centrifuge and dry at 60 °C for 4 h, and then calcine at 500 °C in a muffle furnace for 1 h at a heating rate of 1 °C / min to obtain a multi-shell structured SnO2 precursor.
[0039] (3) 1.2 g of the multi-shell structured SnO2 precursor prepared in step (2) and 0.36 g of CoSO4 were dissolved in 15 ml of ethanol, ultrasonically stirred until completely dispersed, and then centrifuged and dried at 60 °C for 4 h. The mixture was calcined in a muffle furnace at 500 °C for 1 h at a heating rate of 1 °C / min to obtain a porous shell structured Co3O4-SnO2 in-plane heterojunction.
[0040] Example 6 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Take 7g of lactose and 8g of fructose and dissolve them in 60ml of water. Stir for 10min until the mixture becomes transparent and clear to obtain a mixed solution. Place the solution in a 100ml reactor and perform a hydrothermal reaction at 200℃ for 2h. Centrifuge the mixed solution after the reaction and dry the obtained product at 60℃ for 4h to obtain composite carbon spheres.
[0041] (2) Dissolve 1.5 g Sn(NO3)2 and 7.5 g composite carbon spheres in 150 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 2 h, then centrifuge and dry at 60 °C for 4 h. Then calcine at 500 °C in a muffle furnace for 1 h at a heating rate of 2 °C / min to obtain a multi-shell SnO2 precursor.
[0042] (3) 1.2 g of the multi-shell SnO2 precursor prepared in step (2) and 0.32 g of Co(NO3)2 were dissolved in 15 ml of ethanol, ultrasonically stirred until completely dispersed, and then centrifuged and dried at 60°C for 4 h. The mixture was calcined in a muffle furnace at 500°C for 1 h at a heating rate of 1°C / min to obtain a porous shell structure Co3O4-SnO2 in-plane heterojunction.
[0043] Example 7 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Take 5 g of glucose, 5 g of fructose and 5 g of lactose and dissolve them in 60 ml of water. Stir for 10 min until the solution becomes transparent and clear to obtain a mixed solution. Place the solution in a 100 ml reactor and perform hydrothermal reaction at 200 °C for 2 h. Centrifuge the mixed solution after the reaction and dry the obtained product at 60 °C for 4 h to obtain composite carbon spheres.
[0044] (2) Dissolve 2 g SnCl2 and 10 g composite carbon spheres in 200 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 1 h, then centrifuge and dry at 60 °C for 4 h. Then calcine in a muffle furnace at 450 °C for 2 h with a heating rate of 2 °C / min to obtain a multi-shell structured SnO2 precursor.
[0045] (3) 1.8 g of the multi-shell SnO2 precursor prepared in step (2) and 0.4 g of Co(NO3)2 were dissolved in 20 ml of ethanol, ultrasonically stirred until completely dispersed, and then centrifuged and dried at 60°C for 4 h. The mixture was calcined in a muffle furnace at 500°C for 1 h at a heating rate of 1°C / min to obtain a porous shell structure Co3O4-SnO2 in-plane heterojunction.
[0046] Example 8 The preparation method of the porous shell structure Co3O4-SnO2 in-plane heterojunction of this embodiment is as follows: (1) Dissolve 10 g of glucose and 5 g of sucrose in 60 ml of water and stir for 10 min until the solution becomes transparent and clear to obtain a mixed solution. Place the solution in a 100 ml reactor and perform a hydrothermal reaction at 200 °C for 2 h. Centrifuge the mixed solution after the reaction and dry the obtained product at 60 °C for 4 h to obtain composite carbon spheres.
[0047] (2) Dissolve 2 g SnCl4 and 10 g composite carbon spheres in 200 ml ethanol and stir ultrasonically until completely dispersed to obtain a mixed solution. Stir and age the mixed solution at room temperature for 2 h, then centrifuge and dry at 60 °C for 4 h, and calcine at 500 °C in a muffle furnace for 2 h at a heating rate of 5 °C / min to obtain a multi-shell structured SnO2 precursor.
[0048] (3) 1.9 g of the multi-shell structured SnO2 precursor prepared in step (2) and 0.6 g of CoSO4 were dissolved in 20 ml of propanol and ultrasonically stirred until completely dispersed. The mixture was then centrifuged and dried at 60°C for 4 h. The mixture was calcined in a muffle furnace at 500°C for 1 h at a heating rate of 1°C / min to obtain a porous shell structured Co3O4-SnO2 in-plane heterojunction.
[0049] Figure 1 The XRD spectrum of the porous shell structure Co3O4-SnO2 in-plane heterojunction obtained in this example, the product is a composite of Co3O4 and SnO2; Figure 2 This is the SEM photo of the material, where the obvious Co3O4-SnO2 porous shell structure can be observed; Figure 3 The response value of the porous shell structure Co3O4-SnO2 in-plane heterojunction obtained in this embodiment to 50ppm hydrogen at 110-230℃. It can be seen that at 170℃, the response value is 8.63; Figure 4 The long-term stability test of the porous shell structure Co3O4-SnO2 in-plane heterojunction obtained in this embodiment within 30 days showed that the response value did not change significantly, indicating that the sensor prepared with the porous shell structure Co3O4-SnO2 in-plane heterojunction material has good stability.
[0050] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A porous shell structure Co3O4-SnO2 in-plane heterojunction, characterized by: In the porous shell structure, Co3O4 and SnO2 are uniformly distributed in the two-dimensional plane of each shell to form a two-dimensional planar heterogeneous structure.
2. The method for preparing the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 1, characterized in that: The following steps are involved: (1) Preparation of composite carbon spheres: Dissolve different carbon sources in water, stir until transparent and clear, place in a reactor for hydrothermal reaction, and centrifuge and dry the mixed solution after the reaction to obtain composite carbon spheres; (2) Preparation of a multi-shell SnO2 precursor: dissolving a tin compound in an organic solvent, adding composite carbon spheres, and ultrasonically stirring until completely dispersed to obtain a mixed solution A. Stirring and aging the mixed solution A at room temperature, centrifugally drying, and calcining in air to obtain a multi-shell SnO2 precursor; (3) Preparation of a porous shell structure Co3O4-SnO2 in-plane heterojunction: The multi-shell structure SnO2 precursor and the cobalt compound prepared in step (2) are dissolved in an organic solvent, ultrasonically dissolved and stirred to obtain a mixed solution B, and after centrifugal drying, the mixed solution is calcined in air under high temperature conditions to obtain a porous shell structure Co3O4-SnO2 in-plane heterojunction.
3. The method for preparing the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 2, characterized in that: The carbon source in step (1) is at least two of sucrose, fructose, glucose, lactose, tannic acid, dopamine, and corn starch, and the concentration is 0.1 g / mL to 0.5 g / mL.
4. The method for preparing the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 2, characterized in that: The hydrothermal reaction temperature in step (1) is 160-200° C., and the reaction time is 1-5 h.
5. The method for preparing the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 2, characterized in that: In step (2) and step (3), the organic solvent is one or more of ethanol, propanol, glycerol and tetrahydrofuran.
6. The method for preparing the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 2, characterized in that: The tin compound in step (2) is one or more of SnCl2, SnSO4, SnCl4 or Sn(NO3)2, the mass ratio of the tin compound to the carbon sphere is 1:5~1:20, and the aging time is 0.5-3h.
7. The method for preparing the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 2, characterized in that: In the step (3), the mass ratio of the multi-shell SnO2 precursor to the cobalt compound is 1:0.1 to 1:0.3; the cobalt compound is one or more of CoCl2, CoSO4, Co(NO3)2, and cobalt acetylacetonate; and the total concentration of the multi-shell SnO2 precursor and the cobalt compound in the mixed solution B is 0.1 g / mL to 0.22 g / mL.
8. The method for preparing the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 2, characterized in that: In the step (2) and the step (3), the calcination temperature is 400-600°C, the heating rate is 1°C / min to 5°C / min, and the calcination time is 1-2h.
9. Application of the porous shell structure Co3O4-SnO2 in-plane heterojunction according to claim 1 as a gas sensor in a high-sensitivity hydrogen sensor.
10. The use according to claim 9, characterized in that: When the operating temperature is 170°C, the porous shell structure Co3O4-SnO2 in-plane heterojunction as a gas sensor has good selectivity for hydrogen and the sensitivity to 50ppm hydrogen reaches 8.63.
Citation Information
Cited By
Rare earth monatomic doped Pd / WO3 material as well as preparation method and application thereof
CN120294080A