Method for treating high-concentration salt-containing organic wastewater

Through the combination of the modified exchange membrane and the electroless plating solution, the problems of salt ion effect and inorganic salt composition in high-salt organic wastewater treatment are solved, and the long life of efficient organic matter extraction and ion exchange membrane is achieved, meeting the sewage treatment standards.

CN118954840AActive Publication Date: 2024-11-15JIANGSU TONGYONG ENVIRONMENTAL GRP CO LTD

Patent Information

Application Number
CN202411216015.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-15
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The prior art ignores the effects of salt ion effect and solute correlation on solution water molecules when treating high-salt organic wastewater, and the impact of inorganic salt components on the performance of flocculants is not fully considered, resulting in poor extraction effect and ion exchange. The membrane has a short service life.

Method used

The modified cation and anion exchange membrane were used to treat high-salt organic wastewater by electrodialysis, and the coupling modification of activated CNTs/TiO2-CuO with polyvinyl chloride and polyethersulfone was modified, combined with electroless plating solution to enhance the catalysis of the film and Mechanical strength, optimize the electrodialysis process.

Benefits of technology

It effectively reduces the impact of salt effect on organic matter extraction, improves the extraction efficiency of inorganic salts, extends the service life of the ion exchange membrane, and improves the oxidation catalytic performance of organic matter, meeting the sewage treatment standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005021554510000051
    Figure BDA0005021554510000051
  • Figure BDA0005021554510000052
    Figure BDA0005021554510000052
  • Figure BDA0005021554510000061
    Figure BDA0005021554510000061
Patent Text Reader

Abstract

The invention discloses a method for treating high-concentration salt-containing organic wastewater, belongs to the technical field of wastewater treatment, and is used for solving the technical problem that in the prior art, the separation degree of components in a high-salt organic matter solution and the performance of an ion exchange membrane in an electrodialysis method need to be improved. The method comprises the following steps: pretreating high-salt and high-organic wastewater to obtain a low-salt and low-organic-matter solution, preparing activated CNTs / TiO2-CuO, preparing a modified cation exchange membrane precursor and a modified anion exchange membrane precursor, and plating to obtain a modified cation exchange membrane and a modified anion exchange membrane. Electrodialyzing the low-salt low-organic matter solution to obtain a high-salt solution and dischargeable water; according to the invention, the surface-modified ion exchange membrane is used to improve the catalytic ability of the oxidizing agent to organic matters, chemical plating is used to provide a uniform deposition layer, and finally the purpose of efficient and high-purity treatment of salt-containing organic wastewater is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of industrial wastewater treatment, and in particular to a method for treating high-concentration salt-containing organic wastewater. Background Art

[0002] In industrial production, high-salt organic wastewater contains a large amount of organic matter and salts. Direct discharge or improper treatment can easily cause serious environmental pollution, such as long-term impacts on soil and groundwater. Effective recycling and treatment of high-salt organic wastewater can protect natural resources while recycling high-salt organic wastewater, which is also one of the important aspects of achieving sustainable development.

[0003] Patent application CN2016110952679 discloses a method for treating high-salt organic wastewater. The method repeatedly dehydrates and crystallizes the high-salt organic wastewater to achieve the purpose of separating inorganic salts and organic matter. However, the method ignores the influence of salt ion effect and colligative properties of solute on the crystallization of water molecules in the solution, and the extraction effect of repeated crystallization on inorganic salts needs to be further improved.

[0004] Patent application CN2019110771785 discloses a method for treating high-salt organic wastewater with electrodialysis. The method first uses a flocculant to initially separate organic matter in the high-salt organic wastewater, and then uses the plated ion exchange membrane for electrodialysis. During the electrodialysis, an oxidant is introduced to catalyze the decomposition of residual organic matter in the solution, thereby achieving the purpose of separating inorganic salts and removing organic matter. However, this method ignores the effect of inorganic salt components on the performance of flocculants in precipitating organic matter, does not modify the ion exchange membrane, and cannot guarantee the service life of the ion exchange membrane after plating. In addition, a catalyst that has a strong promoting performance for the oxidation of organic matter by the oxidant is not introduced into the ion exchange membrane, and the catalytic performance of the oxidant on organic matter in the solution is overly optimistically estimated.

[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for treating high-concentration salt-containing organic wastewater to solve the technical defects proposed by the background technology.

[0007] The purpose of the present invention can be achieved by the following technical solution: A method for treating high-concentration salt-containing organic wastewater comprises the following steps:

[0008] S1, pre-treating the high-salt organic solution to obtain a high-salt low-organic solution;

[0009] S2, assembling the modified cation exchange membrane and the modified anion exchange membrane into an electrodialysis device, and using the electrodialysis device to treat the high-salt and low-organic solution to obtain a high-salt solution and dischargeable water;

[0010] The preparation method of the modified cation exchange membrane is as follows: activated CNTs / TiO2-CuO and 10-20wt% polyvinylidene chloride solution are added to a reactor, the temperature of the reactor is increased to 30-40°C, the reactor is kept warm and ultrasonicated for 1-2h, post-processed to obtain modified polyvinylidene chloride, the modified polyvinylidene chloride is coupled and modified to obtain a modified cation exchange membrane precursor, the modified cation exchange membrane precursor is plated with a chemical plating solution, and post-processed to obtain a modified cation exchange membrane;

[0011] The preparation method of the modified anion exchange membrane is as follows: activated CNTs / TiO2-CuO and 10-20wt% polyethersulfone solution are added to a reactor, the temperature of the reactor is increased to 30-40°C, the reactor is kept ultrasonic for 1-2 hours, a composite polyethersulfone membrane is obtained by post-treatment, the composite polyethersulfone membrane is modified to obtain a modified anion exchange membrane precursor, the modified anion exchange membrane precursor is plated with a chemical plating solution, and a modified anion exchange membrane is obtained by post-treatment.

[0012] Furthermore, the pre-processing operation includes the following steps:

[0013] A1. Add high-salt organic solution and deionized water into a reactor and stir for 5-15 minutes at room temperature to obtain a diluted solution;

[0014] A2. Lower the temperature of the reactor containing the diluted solution to 0-5°C, stir for 3-5 hours, and filter to obtain inorganic salt crystals and a low-salt, high-organic matter solution;

[0015] A3. Add the low-salt high-organic matter solution and the extract into a reaction kettle and stir. Stir for 20-30 minutes at room temperature. Allow to stand and separate the liquids to obtain an organic solution and a low-salt low-organic matter solution.

[0016] In step A1, the volume ratio of deionized water to high-salt organic solution is 2:1, and the stirring rate is 120 rpm; in step A3, the extractant is one or more of ethyl acetate, dichloromethane, and ether, the volume ratio of the extractant to the mixed solution is 0.5:1, and the stirring rate is 120 rpm.

[0017] Reaction principle:

[0018] Deionized water is used to dilute the high-salt and high-organic solution. Excessive concentration of salt ions will affect the arrangement of water molecules, making the process of forming large ice crystals more complicated. At the same time, due to the colligative properties of solute molecules, excessive organic solutes will also cause the freezing point of the solution to decrease, making it more difficult to freeze. Due to the low solubility and poor affinity of organic components with salt, water molecules will be excluded during the crystallization process, resulting in the formation of ice crystals that are mainly inorganic components of salt. High concentrations of salt ions will affect the extraction performance of the extractant. Using crystallization to remove some inorganic salt components is more conducive to the extraction of organic matter.

[0019] Further, activated CNTs / TiO2-CuO is prepared by the following steps:

[0020] B1, adding single-walled carbon nanotubes, amide compounds and dichloromethane into a reaction kettle, raising the temperature of the reaction kettle to 40-60° C., keeping the temperature for 6-8 hours, and post-treating to obtain modified carbon nanotubes;

[0021] B2, mixing nano-TiO2, nano-CuO and modified carbon nanotubes in N,N-dimethylformamide to obtain a mixed solution, adding the mixed solution to an ultrasonic device for ultrasonication, the ultrasonic device is set at 60-80°C, the frequency is 40-60kHz, the temperature is kept for ultrasonication for 3-5h, and post-processing is performed to obtain CNTs / TiO2-CuO;

[0022] B3. Add CNTs / TiO2-CuO, silane coupling agent and organic solvent into a reactor and stir. Raise the temperature of the reactor to 40-60°C and keep the reaction for 6-8h. Post-treat to obtain activated CNTs / TiO2-CuO.

[0023] Further, in step B1, the dosage ratio of single-walled carbon nanotubes, amide compounds and dichloromethane is 1g:2g:15mL, the amide compound is one or more of acetamide, benzoyl and cystine, and the post-treatment operation is: suction filtration, placing the filter cake in a drying oven at a temperature of 80°C and vacuum drying until the filter cake has a constant weight, to obtain modified carbon nanotubes;

[0024] In step B2, the dosage ratio of nano-TiO2, nano-CuO, modified carbon nanotubes and N,N-dimethylformamide is 2g:1g:5g:40mL, and the post-treatment operation is: suction filtration, placing the filter cake in a drying oven at a temperature of 80°C and vacuum drying until the filter cake has a constant weight, to obtain CNTs / TiO2-CuO;

[0025] In step B3, the amount ratio of CNTs / TiO2-CuO, organic solvent and silane coupling agent is 1g:20mL:4g, the organic solvent is one or more of toluene, xylene and dichloromethane, the silane coupling agent is 3-aminopropyltriethoxysilane, aminophenyltrimethoxysilane, γ-aminobutyltrimethoxysilane, and one or more of the following: the post-treatment operation is: filtration, placing the filter cake in a drying oven at a temperature of 80°C and vacuum drying until the filter cake is constant weight to obtain activated CNTs / TiO2-CuO.

[0026] Reaction principle: Amidation treatment can introduce carboxyl groups (-COOH) or amine groups (-NH2) to the surface of carbon nanotubes, making them more compatible and enhancing the interfacial compatibility with nano-metal particles. Functionalization of the surface of carbon nanotubes can improve their electrochemical properties, especially in electrocatalytic reactions. Composite materials of metal nanoparticles and functionalized carbon nanotubes can show higher electrical conductivity and electrochemical activity, which helps to improve the efficiency and response speed of catalytic materials.

[0027] Silylation treatment can make the surface of carbon fiber tube have certain anti-biological adhesion properties. Silylation can introduce silicon-containing organic groups to the surface of carbon fiber tube. These groups can effectively combine with the matrix molecules of adsorbed ion exchange membrane, enhance the binding force and stability of the interface, and prevent the loosening or peeling of the interface during use.

[0028] Furthermore, the amount ratio of activated CNTs / TiO2-CuO and 10-20wt% polyvinylidene chloride solution is 1g:10ml, and the ultrasonic frequency is 20-80kHz.

[0029] Further, the coupling modification of the modified polyvinylidene chloride comprises the following steps:

[0030] C1, soaking the modified polyvinylidene chloride in 30-50wt% sulfuric acid solution and 1-5wt% hydrogen peroxide solution at a soaking temperature of 60-80°C, keeping the temperature for reaction for 2-4h, and post-treating to obtain sulfonated polyvinylidene chloride;

[0031] The synthetic reaction formula of sulfonated polyvinylidene chloride is:

[0032]

[0033] The synthetic reaction principle of sulfonated polyvinylidene chloride is as follows: sulfuric acid acts as a catalyst in the reaction. Sulfuric acid is a strong acid that can provide protons for the formation of reaction intermediates. Sulfuric acid first reacts with the vinyl chloride group in the polyvinylidene chloride molecule to form an intermediate sulfate ester compound. Under the action of sulfuric acid, the chlorine atom in the vinyl chloride group is replaced or added with a sulfonic acid group (-SO3H) to form a sulfuric acid sulfonic acid compound. In this process, part of the vinyl chloride group will be converted into a sulfonic acid group. After the reaction, part of the vinyl chloride units in the polyvinylidene chloride chain will be sulfonated by sulfuric acid to form sulfonated polyvinylidene chloride.

[0034] C2, soaking the sulfonated polyvinylidene chloride in a mixed solution consisting of 20-30wt% sodium hydroxide solution and 30-50wt% ammonia solution at a soaking temperature of 30-50° C., keeping the mixture warm for 2-4 hours, post-treating to obtain sulfonated polyvinylidene chloride, dissolving the sulfonated polyvinylidene chloride in ethylene glycol monomethyl ether acetate to prepare a sulfonated polyvinylidene chloride solution;

[0035] The synthetic reaction formula of sulfonated polyvinylidene chloride is:

[0036]

[0037] The reaction principle of sulfonated polyvinylidene chloride solution is as follows: the sulfonic acid group is a strongly acidic functional group. Under strong alkaline conditions, a neutralization reaction will occur. The negative charge on the sulfonic acid group is neutralized by sodium ions to form sodium sulfonate salt (-SO3Na). After the formation of sodium sulfonate, it comes into contact with water and undergoes a replacement reaction to form the corresponding sulfonamide group (-SO3NH2).

[0038] C3, spin coating the sulfonated polyvinylidene chloride solution on the surface of the silanized glass fabric to form a coating with a thickness of 150-200 μm to obtain a coated glass fabric, placing the coated glass fabric in a drying oven at 80° C. for vacuum heat treatment for 1 h to obtain a modified glass fabric;

[0039] C4, immersing the modified glass fabric in a 20-30wt% glutaraldehyde solution at a soaking temperature of 40-50°C, keeping the solution warm for 3-5h, and post-treating to obtain a modified cation exchange membrane precursor.

[0040] The synthetic reaction formula of the modified cation exchange membrane precursor is:

[0041]

[0042] The synthetic reaction principle of the modified cation exchange membrane precursor is: the carbonyl group of acetaldehyde is opened by the nucleophilic attack of the amino group to form an intermediate iminium ion. The glutaraldehyde and the amino compound can undergo a Schiff base reaction. In this reaction, the carbonyl group of the aldehyde undergoes a nucleophilic addition reaction with the amino group. The mechanism is: RCHO+NH2R'→RCH=NR'+H2O, wherein R represents the pentyl group (the carbon chain part of the glutaraldehyde), and R' represents the carbon chain part of the amino compound. The generated product is an intermediate product containing a C=N bond, and this intermediate further reacts into a stable Schiff base.

[0043] Furthermore, in step C1, the modified polyvinylidene chloride, 30-50wt% sulfuric acid solution and 1-5wt% hydrogen peroxide solution are used in a ratio of 1g:4mL:1mL, and the post-treatment operation is: suction filtration, placing the filter cake in a drying oven at 80°C and vacuum drying until the filter cake has a constant weight, to obtain sulfonated polyvinylidene chloride;

[0044] In step C2, the amount ratio of sulfonated polyvinylidene chloride, 0-30wt% sodium hydroxide solution and 30-50wt% ammonia solution is 1g:1mL:4mL, and the post-treatment operation is: suction filtration, placing the filter cake in a drying oven at 80°C and vacuum drying until the filter cake has a constant weight, to obtain sulfonated polyvinylidene chloride;

[0045] Further, in step C3, the silanized glass fabric is prepared by the following steps: a glass fabric with a thickness of 0.05-0.10 mm and a 0.5%-5wt% silane coupling agent solution are placed in a stirring kettle for reaction, the temperature is set to 60-80°C, the heat preservation is 2-3h, the stirring rate is 120rpm, and after the reactor is cooled to room temperature, the silanized glass fabric precursor is taken out, rinsed with cold ethanol at a temperature of 10°C for 3-5 times, and then placed in a drying oven and vacuum baked at 110-120°C for 1-2h to obtain the silanized glass fabric.

[0046] The synthetic reaction formula of silanized glass fabric is:

[0047]

[0048] The synthetic reaction principle of silanized glass fabric is as follows: 3-aminopropyltrimethoxysilane molecules are first hydrolyzed under the action of water, and their methoxy (-OCH3) groups are replaced by water molecules to form hydroxyl (-OH). The hydroxyl (-OH) of silane in the 3-aminopropyltrihydroxysilane produced by hydrolysis forms a silicon-oxygen bond (Si-O-Si) with the hydroxyl (-OH) on the glass surface. The newly formed siloxane bond firmly connects the 3-aminopropyl group to the glass surface.

[0049] Furthermore, It represents the mesh structure of glass fabric. The silane coupling agent is 3-aminopropyltrimethoxysilane, and the structure is

[0050] Furthermore, the silane coupling agent is one or more of 3-aminopropyltrimethoxysilane, aminophenyltrimethoxysilane, and γ-aminobutyltrimethoxysilane, preferably 3-aminopropyltrimethoxysilane, and the ratio of glass fabric to 0.5%-5wt% silane coupling agent is 1g:5mL; in step C4, the ratio of modified glass fabric with a thickness of 0.05-0.10mm and 20-30wt% glutaraldehyde solution is 1g:5mL, and the post-treatment operation is: filtration, placing the filter cake in a drying oven at 80°C and vacuum drying until the filter cake has a constant weight, to obtain a modified cation exchange membrane precursor.

[0051] Furthermore, the activated CNTs / TiO2-CuO and 10-20wt% polyethersulfone solution are used in a ratio of 1g:10ml, and the ultrasonic frequency is 20-80kHz.

[0052] Further, the modification treatment of the composite polyethersulfone membrane includes the following steps:

[0053] D1, soaking the composite polyethersulfone membrane in a mixed solution containing 5-10wt% methyl chloride and 20-30wt% aluminum chloride at a soaking temperature of 50-70°C, keeping the temperature for reaction for 1-3h to obtain an impregnated membrane, and post-treating to obtain a halogenated membrane;

[0054] The synthesis equation of halogenated membrane is:

[0055]

[0056] The synthesis principle of halogenated membrane is as follows: aluminum chloride, as Lewis acid, can form coordination compounds with halogen atoms in benzene rings. This coordination makes the π electron system of benzene rings more electrophilic and more susceptible to electrophilic attack. - ) will attack the activated benzene ring, and AlCl3, as a catalyst, can catalyze the intermediate to remove hydrogen chloride (HCl) at the end of the reaction to produce the final halogenated aromatic compound.

[0057] D2. Soak the halogenated membrane in a 20-30wt% trimethylamine solution at a soaking temperature of 40-60°C and keep the solution warm for 2-4 hours to obtain a quaternary ammonium membrane, which is then post-treated to obtain a modified anion exchange membrane precursor.

[0058] The synthesis equation of modified anion exchange membrane precursor is:

[0059]

[0060] The synthesis principle of the modified anion exchange membrane precursor is as follows: trimethylamine is an electrophilic reagent, and its nitrogen atom carries a lone pair of electrons, so it has a strong nucleophilicity. In the reaction, the nitrogen atom of trimethylamine will attack the chlorine group in the halogenated polyethersulfone molecule, causing the chloride ion to detach from the halogenated polyethersulfone molecule to form a transitional intermediate. This intermediate will then lose a proton to form a trimethylamine salt, and finally a compound with a quaternary ammonium salt group is introduced into the halogenated polyethersulfone molecule.

[0061] Furthermore, in step D1, the amount ratio of composite polyethersulfone, 5-10wt% methyl chloride and 20-30wt% aluminum chloride is 1g:5mL:3mL, and the post-treatment operation is: taking out the impregnated membrane, placing the impregnated membrane in a drying oven at 80°C and vacuum drying until the filter cake is constant weight, to obtain a halogenated membrane; in step D2, the amount ratio of halogenated membrane immersion and 20-30wt% trimethylamine solution is 1g:5mL, and the post-treatment operation is: taking out the quaternized membrane, placing the quaternized membrane in a drying oven at 80°C and vacuum drying until the filter cake is constant weight, to obtain a halogenated membrane modified anion exchange membrane precursor.

[0062] Further, the plating comprises the following steps: placing the membrane substrate in a chemical plating solution, maintaining the temperature at 20-40°C for 1-2 hours, and after the plating is completed, using deionized water to rinse the plated ion exchange membrane to neutrality to obtain a modified ion exchange membrane, wherein the membrane substrate is a modified cation exchange membrane or a modified anion exchange membrane;

[0063] The chemical plating solution is composed of a metal ion source, a reducing agent, a complexing agent, a surfactant, a stabilizer, a buffer and deionized water in a weight ratio of 0.1-5:1-10:2-12:0.001-0.2:0.01-0.1:0.01-0.1:10-60;

[0064] The metal ion source is selected from one or more of nickel chloride, nickel sulfate, zinc chloride, zinc sulfate, chromium chloride, chromium sulfate, and chromic anhydride; the reducing agent is selected from one or more of sodium hypophosphite, formaldehyde, and hydrazine; the complexing agent is selected from one or more of ethylenediaminetetraacetic acid, sodium citrate, sodium pyrophosphate, diethanolamine, triethanolamine, diethylenetriamine pentacarboxylate, polyacrylic acid, citric acid, etc.; the surfactant is selected from one or more of sodium dodecylbenzene sulfonate, sodium n-octyl sulfate, and sodium dodecyl sulfate; the stabilizer is selected from lead nitrate or sodium thiosulfate; and the buffer is selected from boric acid or sodium acetate.

[0065] Reaction principle: Chemical plating can provide a very uniform deposition layer, which can form a uniform and dense film on the surface of the ion exchange membrane. It is suitable for substrates of various sizes and shapes, whether flat or curved, chemical plating can form a continuous and uniform film on these surfaces;

[0066] Reducing agents provide electrons to metal ions in the solution, reducing them to corresponding metal atoms; chelating agents can cooperate with metal ions to usually have a more uniform deposition rate and more uniform surface coverage during the plating process; stabilizers can help maintain a stable concentration of metal ions in the plating solution, prevent them from premature precipitation or excessive reduction, and maintain the uniformity and long-term stability of the plating solution; buffers can optimize the chemical environment of the plating solution, help achieve uniformity and consistency of metal deposition, and stable pH conditions can make the deposition rate of metal ions more controllable, thereby producing a uniform deposition layer with good crystalline properties.

[0067] Furthermore, in step S2, the wastewater treatment includes the following steps: setting the voltage of the electrodialysis equipment to 20-80V, introducing ozone into the ion exchange membrane at a rate of 10L / h, setting the electrodialysis time to 6-7h, taking out the electrodialysis water and the salt solution, repeating the electrodialysis operation 2-3 times, and concentrating them to obtain a high salt solution and dischargeable water.

[0068] Reaction principle: The ions in the wastewater are driven by the electric field, the positive electrode attracts anions, and the negative electrode attracts cations. The ion exchange membrane selectively permeates, so that the inorganic salt components in the wastewater are gathered in the electrode area to obtain dischargeable water and high-salt solution.

[0069] The present invention has the following beneficial effects:

[0070] 1. In the pretreatment process of the high-salt and high-organic solution of the present invention, deionized water is first used to reduce the inorganic salt concentration and organic matter concentration in the solution, effectively reducing the salt effect and solute colligative properties in the system. The influence of the freezing process of the solution is effectively reduced. The organic components are excluded from the water molecules during the crystallization process due to their low solubility and poor affinity with salt, resulting in the formation of ice crystals that are mainly inorganic components of salt. Most of the inorganic salts in the solution system are separated, which effectively reduces the influence of the salt effect on the extraction of organic matter and makes the extraction of organic matter more complete. In the process of preparing activated CNTs / TiO2-CuO, amide compounds are used to modify the surface of single-walled carbon fiber tubes to fix amide groups on the surface of carbon nanotubes, which can provide active sites and help the subsequent coating and stabilization of metal particles. The amide group usually has nitrogen atoms, which can provide additional coordination This coordination effect not only helps the adsorption and fixation of metal ions on the surface of carbon nanotubes, but also reduces the dissolution and migration of metal particles in the environment, and helps the carbon nanotubes to be dispersed and evenly coated on the surface of metal particles, thus ensuring the activity and stability of metal particles in catalysis or other applications; using single-walled carbon nanotubes to coat metal copper particles and metal oxide particles on titanium dioxide with catalytic oxidation can help improve the catalytic performance of the particles and the stability during electrodialysis; using silane coupling agents to modify CNTs / TiO2-CuO can silylate it, which is beneficial to the subsequent stable combination with polyvinylidene chloride and polyether sulfone, so that the ion exchange membrane has the function of catalyzing the oxidation of organic matter; silylation treatment can adjust the surface of carbon fiber tubes, thereby optimizing the surface properties of adsorption ion exchange membranes.

[0071] 2. In the process of preparing the modified ion exchange membrane, the present invention first uses activated CNTs / TiO2-CuO to respectively combine polyvinylidene chloride and polyether sulfone, thereby enriching the function of the ion exchange membrane; in the process of preparing the modified cation exchange membrane, a modified glass fabric is introduced as a base material to enhance the mechanical strength of the cation exchange membrane, wherein the glass fabric is silylated and the modified polyvinylidene chloride is sulfonated so that the two can be combined through glutaraldehyde to form a compact organic structure, so that the mechanical strength of the modified cation exchange membrane is improved while the modified polyvinylidene chloride is not easy to fall off, thereby extending the service life of the modified cation exchange membrane; in the process of preparing the modified anion exchange membrane, formaldehyde is used to introduce a halogen group under acidic conditions to prepare a halomethyl membrane, and then the halomethyl membrane is further quaternized with trimethylamine to generate a positively charged quaternary ammonium salt, thereby further enhancing the selectivity of the ion exchange membrane.

[0072] 3. In the process of plating the modified ion exchange membrane substrate, the present invention uses chemical plating solution to replace the electrochemical plating method. Chemical plating can provide a very uniform deposition layer and can form a uniform and dense film on the surface of the ion exchange membrane. It is suitable for substrates of various sizes and shapes, whether flat or curved. Chemical plating can form a continuous and uniform film on these surfaces; the reducing agent provides electrons to the metal ions in the solution to reduce them to corresponding metal atoms; the chelating agent can cooperate with the metal ions to usually have a more uniform deposition rate and more uniform surface coverage during the plating process; the stabilizer can help maintain a stable concentration of metal ions in the plating solution, prevent them from premature precipitation or over-reduction, and maintain the uniformity and long-term stability of the plating solution; the buffer can optimize the chemical environment of the plating solution, help to achieve uniformity and consistency of metal deposition, and the stable pH condition can make the deposition rate of metal ions more controllable, thereby producing a uniform deposition layer with good crystalline properties. DETAILED DESCRIPTION

[0073] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0074] Example 1

[0075] This embodiment provides a method for treating high-concentration salt-containing organic wastewater, comprising the following steps:

[0076] S1. Pretreatment of wastewater

[0077] The high-salt organic solution and deionized water were mixed in a reaction kettle at a volume ratio of 1:2 and stirred at a stirring rate of 120 rpm for 5 minutes at room temperature to obtain a diluted solution;

[0078] The temperature of the reactor containing the diluted solution was lowered to 5°C, and after being kept at the temperature for 3 hours, the solid-liquid mixture was separated to obtain high-salt ice and low-salt high-organic matter solution;

[0079] The low-salt high-organic matter and dichloromethane were mixed at a volume ratio of 0.5:1 to obtain a mixed solution, which was added to a reactor and stirred at a speed of 120 rpm for 1 hour at room temperature. The mixture was allowed to stand for 20 minutes, and an organic solution and a low-salt low-organic matter solution were collected.

[0080] S2. Preparation of activated CNTs / TiO2-CuO

[0081] Single-walled carbon nanotubes, acetamide and organic solvent were added into a reactor in a ratio of 1 g:2 g:15 mL, the temperature of the reactor was raised to 40°C, the reaction was kept warm for 6 hours, and the filter cake was placed in a drying oven at 80°C and vacuum dried until the filter cake had a constant weight, thereby obtaining modified carbon nanotubes;

[0082] Mix nano-TiO2, nano-CuO and modified carbon nanotubes 2g:1g:5g:40mL in N,N-dimethylformamide to obtain a mixed solution, add the mixed solution to an ultrasonic device for ultrasonication, set the ultrasonic device to 60°C and a frequency of 40kHz, keep the temperature and ultrasonicate for 3h, filter, and place the filter cake in a drying oven at a temperature of 80°C and vacuum dry until the filter cake has a constant weight, thereby obtaining CNTs / TiO2-CuO;

[0083] CNTs / TiO2-CuO, dichloromethane and -aminopropyltriethoxysilane were added into the reactor in a ratio of 1g:20mL:4g and stirred. The temperature of the reactor was raised to 40°C and kept for 6 hours. The filter cake was vacuum dried in a drying oven at 80°C until the filter cake had a constant weight to obtain activated CNTs / TiO2-CuO.

[0084] S3. Preparation of modified cation exchange membrane precursor

[0085] Add activated CNTs / TiO2-CuO and 10 wt% polyvinylidene chloride solution into a reactor at a ratio of 1 g:10 ml, raise the temperature of the reactor to 30°C, set the frequency to 40 kHz, perform ultrasonic treatment for 1 hour, filter, and place the filter cake in a drying oven at 80°C and vacuum dry to constant weight to obtain modified polyvinylidene chloride;

[0086] The modified polyvinylidene chloride is soaked in a 30wt% sulfuric acid solution and a 1wt% hydrogen peroxide solution, wherein the modified polyvinylidene chloride, the 30wt% sulfuric acid solution and the 1wt% hydrogen peroxide solution are used in a ratio of 1g:4mL:1mL, the soaking temperature is 60°C, the temperature is kept for reaction for 2h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain sulfonated polyvinylidene chloride;

[0087] Soaking sulfonated polyvinylidene chloride in 20wt% sodium hydroxide solution and 30wt% ammonia solution, wherein the amount ratio of sulfonated polyvinylidene chloride, 20wt% sodium hydroxide solution and 30wt% ammonia solution is 1g:1mL:4mL, the soaking temperature is 30°C, the temperature is kept for reaction for 2h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain sulfonated polyvinylidene chloride, and the sulfonated polyvinylidene chloride is dissolved in ethylene glycol monomethyl ether acetate to prepare a sulfonated polyvinylidene chloride solution;

[0088] Putting a glass fabric with a thickness of 0.05 mm and a 2.5 wt% silane coupling agent solution into a stirring kettle for reaction, wherein the amount ratio of the glass fabric with a thickness of 0.05 mm and the 2.5 wt% silane coupling agent is 1 g:5 mL, setting the temperature to 60° C., keeping the reaction for 2 h, and stirring at a rate of 120 rpm, after the reactor is cooled to room temperature, taking out the silanized glass fabric precursor, washing it with cold ethanol at a temperature of 10° C. for 3 times, and then placing it in a drying oven and vacuum baking it at 110° C. for 1 h to obtain the silanized glass fabric;

[0089] Spin-coating the sulfonated polyvinylidene chloride solution on the surface of the silanized glass fabric to form a coating with a thickness of 150 μm to obtain a coated glass fabric, placing the coated glass fabric in a drying oven at 80° C. for vacuum heat treatment for 1 h to obtain a modified glass fabric;

[0090] The modified glass fabric was immersed in a 20wt% glutaraldehyde solution, wherein the amount ratio of the modified glass fabric to the 20wt% glutaraldehyde solution was 1g:5mL, the immersion temperature was 40°C, and the reaction was kept warm for 3 hours. The modified glass fabric was taken out and placed in a drying oven at 80°C for vacuum drying to constant weight to obtain a modified cation exchange membrane precursor.

[0091] S4. Preparation of modified anion exchange cation precursor

[0092] Activated CNTs / TiO2-CuO and 10wt% polyethersulfone solution were added into the reactor at a dosage ratio of 1g:10ml, the temperature of the reactor was raised to 30°C, the frequency was 20kHz, the temperature was kept and ultrasonicated for 1h, the frequency was 20kHz, and the filter cake was placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a composite polyethersulfone membrane;

[0093] The composite polyethersulfone membrane is immersed in a mixed solution consisting of 5wt% methyl chloride and 20wt% aluminum chloride, wherein the amount ratio of the composite polyethersulfone, 5wt% methyl chloride and 20wt% aluminum chloride is 1g:5mL:3mL, the immersion temperature is 50°C, the temperature is kept for 1h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a halogenated membrane;

[0094] The halogenated membrane was immersed in a 20 wt % trimethylamine solution, wherein the amount ratio of the halogenated membrane to the 20 wt % trimethylamine solution was 1 g:5 mL, the immersion temperature was 40° C., the reaction was performed for 2 h, and a modified anion exchange membrane precursor was obtained by post-treatment.

[0095] S5. Chemical plating

[0096] Mix nickel chloride, sodium hypophosphite, sodium citrate, sodium dodecylbenzene sulfonate, sodium thiosulfate, sodium acetate and deionized water in a weight ratio of 0.1:1:2:0.001:0.01:0.01:10 to prepare a chemical plating solution;

[0097] The modified cation exchange membrane precursor and the modified anion exchange membrane precursor were placed in a chemical plating solution and plated at 20°C for 1 hour. After the plating was completed, the plated ion exchange membrane was rinsed with deionized water to neutrality to obtain a modified ion exchange membrane.

[0098] S6. Electrodialysis

[0099] Assemble the cation exchange membrane and the anion exchange membrane into the electrodialysis equipment: set the voltage of the electrodialysis equipment to 20V, introduce ozone into the ion exchange membrane at a rate of 10L / h, set the electrodialysis time to 6h, take out the electrodialysis water and the salt solution, repeat the electrodialysis operation twice, and obtain the high salt solution and the dischargeable water after concentration.

[0100] Example 2

[0101] This embodiment provides a method for treating high-concentration salt-containing organic wastewater, comprising the following steps:

[0102] S1. Pretreatment of high-salt and high-organic solution

[0103] The high-salt organic solution and deionized water were mixed in a reaction kettle at a volume ratio of 1:2 and stirred at a stirring rate of 120 rpm for 10 min at room temperature to obtain a diluted solution;

[0104] The temperature of the reactor containing the diluted solution was lowered to 3°C, and after being kept at the temperature for 4 hours, the solid-liquid mixture was separated to obtain high-salt ice and low-salt high-organic matter solution;

[0105] The low-salt high-organic matter and dichloromethane were mixed at a volume ratio of 0.5:1 to obtain a mixed solution, and the mixed solution was added to a reactor and stirred at a speed of 120 rpm. The mixture was stirred at room temperature for 1.5 h, allowed to stand for 20 min, and the organic solution and the low-salt low-organic matter solution were collected.

[0106] S2. Preparation of activated CNTs / TiO2-CuO

[0107] Single-walled carbon nanotubes, acetamide and organic solvent were added into a reactor in a ratio of 1 g:2 g:15 mL and stirred. The temperature of the reactor was raised to 50°C and kept for 7 hours. The filter cake was placed in a drying oven at 80°C and dried under vacuum until the filter cake had a constant weight, thereby obtaining modified carbon nanotubes.

[0108] Mix nano-TiO2, nano-CuO and modified carbon nanotubes 2g:1g:5g:40mL in N,N-dimethylformamide to obtain a mixed solution, add the mixed solution to an ultrasonic device for ultrasonication, set the ultrasonic device to 70°C, the frequency to 50kHz, keep the temperature and ultrasonicate for 4 hours, filter, place the filter cake in a drying oven at 80°C and vacuum dry until the filter cake has a constant weight, and obtain CNTs / TiO2-CuO;

[0109] CNTs / TiO2-CuO, dichloromethane and -aminopropyltriethoxysilane were added into the reactor in a ratio of 1g:20mL:4g and stirred. The temperature of the reactor was raised to 50°C and kept for 7 hours. The filter cake was vacuum dried in a drying oven at 80°C until the filter cake had a constant weight to obtain activated CNTs / TiO2-CuO.

[0110] S3. Preparation of modified cation exchange membrane precursor

[0111] Activated CNTs / TiO2-CuO and 15wt% polyvinylidene chloride solution were added into a reactor at a ratio of 1g:10ml, the temperature of the reactor was raised to 35°C, the frequency was set to 40kHz, the temperature was kept and ultrasonicated for 1.5h, and the filter cake was placed in a drying oven at 80°C and vacuum dried to constant weight to obtain modified polyvinylidene chloride;

[0112] The modified polyvinylidene chloride is soaked in a 40wt% sulfuric acid solution and a 3wt% hydrogen peroxide solution, wherein the modified polyvinylidene chloride, the 40wt% sulfuric acid solution and the 3wt% hydrogen peroxide solution are used in a ratio of 1g:4mL:1mL, the soaking temperature is 70°C, the temperature is kept for reaction for 3h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain sulfonated polyvinylidene chloride;

[0113] Soaking sulfonated polyvinylidene chloride in 25wt% sodium hydroxide solution and 40wt% ammonia solution, wherein the amount ratio of sulfonated polyvinylidene chloride, 25wt% sodium hydroxide solution and 40wt% ammonia solution is 1g:1mL:4mL, the soaking temperature is 40°C, the temperature is kept for reaction for 3h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain sulfonated polyvinylidene chloride, and the sulfonated polyvinylidene chloride is dissolved in ethylene glycol monomethyl ether acetate to prepare a sulfonated polyvinylidene chloride solution;

[0114] Putting a glass fabric with a thickness of 0.10 mm and a 5wt% silane coupling agent solution into a stirring kettle for reaction, wherein the amount ratio of the glass fabric with a thickness of 0.10 mm and the 5wt% silane coupling agent is 1 g:5 mL, setting the temperature to 70°C, keeping the reaction for 3 hours, and stirring at a rate of 120 rpm. After the reactor is cooled to room temperature, taking out the silanized glass fabric precursor, washing it with cold ethanol at a temperature of 10°C for 5 times, and then placing it in a drying oven and vacuum baking it at 120°C for 2 hours to obtain the silanized glass fabric;

[0115] The sulfonated polyvinylidene chloride solution was spin-coated on the surface of the silanized glass fabric to form a coating with a thickness of 200 μm to obtain a coated glass fabric, and the coated glass fabric was placed in a drying oven at 80° C. for vacuum heat treatment for 1 h to obtain a modified glass fabric;

[0116] The modified glass fabric was immersed in a 25wt% glutaraldehyde solution, wherein the amount ratio of the modified glass fabric to the 25wt% glutaraldehyde solution was 1g:5mL, the immersion temperature was 45°C, and the reaction was kept warm for 4 hours. The modified glass fabric was taken out and placed in a drying oven at 80°C for vacuum drying to constant weight to obtain a modified cation exchange membrane precursor.

[0117] S4. Preparation of modified anion exchange cation precursor

[0118] Activated CNTs / TiO2-CuO and 15wt% polyethersulfone solution were added into the reactor at a dosage ratio of 1g:10ml, the temperature of the reactor was raised to 35°C, the frequency was set to 40kHz, the temperature was kept and ultrasonicated for 1h, the frequency was set to 40kHz, and the filter cake was placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a composite polyethersulfone membrane;

[0119] The composite polyethersulfone membrane is immersed in a mixed solution consisting of 8wt% methyl chloride and 25wt% aluminum chloride, wherein the amount ratio of the composite polyethersulfone, 8wt% methyl chloride and 25wt% aluminum chloride is 1g:5mL:3mL, the immersion temperature is 60°C, the temperature is kept for 2h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a halogenated membrane;

[0120] The halogenated membrane was immersed in a 25wt% trimethylamine solution, wherein the ratio of the halogenated membrane to the 25wt% trimethylamine solution was 1g:5mL, the immersion temperature was 50°C, the reaction was kept warm for 3h, and the filter cake was placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a modified anion exchange membrane precursor.

[0121] S5. Chemical plating

[0122] Mix nickel chloride, sodium hypophosphite, sodium citrate, sodium dodecylbenzene sulfonate, sodium thiosulfate, sodium acetate and deionized water in a weight ratio of 3:5:6:0.01:0.05:0.05:30 to prepare a chemical plating solution;

[0123] The modified cation exchange membrane precursor and the modified anion exchange membrane precursor were placed in a chemical plating solution and plated at 30°C for 2 hours. After the plating was completed, the plated ion exchange membrane was rinsed with deionized water to neutrality to obtain a modified ion exchange membrane.

[0124] S6. Electrodialysis

[0125] Assemble the cation exchange membrane and the anion exchange membrane into the electrodialysis equipment: set the voltage of the electrodialysis equipment to 60V, introduce ozone into the ion exchange membrane at a rate of 10L / h, set the electrodialysis time to 6h, take out the electrodialysis water and the salt solution, repeat the electrodialysis operation twice, and obtain the high salt solution and the dischargeable water after concentration.

[0126] Example 3

[0127] This embodiment provides a method for treating high-concentration salt-containing organic wastewater, comprising the following steps:

[0128] S1. Pretreatment of high-salt and high-organic solution

[0129] The high-salt organic solution and deionized water were mixed in a reaction kettle at a volume ratio of 1:2 and stirred at a stirring rate of 120 rpm for 15 minutes at room temperature to obtain a diluted solution;

[0130] The temperature of the reactor containing the diluted solution was lowered to 0°C, and after being kept at the temperature for 5 hours, the solid-liquid mixture was separated to obtain high-salt ice and low-salt high-organic matter solution;

[0131] The low-salt high-organic matter and dichloromethane were mixed in a volume ratio of 0.5:1 to obtain a mixed solution, which was added to a reactor and stirred. The speed was set to 120 rpm, and the mixture was kept warm and stirred for 2 hours. The mixture was allowed to stand for 30 minutes, and the organic solution and the low-salt low-organic matter solution were collected. The high-salt ice was melted and mixed with the low-salt low-organic matter solution to obtain a high-salt low-organic matter solution.

[0132] S2. Preparation of activated CNTs / TiO2-CuO

[0133] Single-walled carbon nanotubes, acetamide and organic solvent were added into a reactor in a ratio of 1 g: 2 g: 15 mL and stirred. The temperature of the reactor was raised to 60°C and kept for 8 hours. The filter cake was placed in a drying oven at 80°C and dried under vacuum until the filter cake had a constant weight, thereby obtaining modified carbon nanotubes.

[0134] Mix nano-TiO2, nano-CuO and modified carbon nanotubes 2g:1g:5g:40mL in N,N-dimethylformamide to obtain a mixed solution, add the mixed solution to an ultrasonic device for ultrasonication, set the ultrasonic device to 80°C, the frequency to 60kHz, keep the temperature and ultrasonicate for 5h, filter, place the filter cake in a drying oven at 80°C and vacuum dry until the filter cake has a constant weight, and obtain CNTs / TiO2-CuO;

[0135] CNTs / TiO2-CuO, dichloromethane and -aminopropyltriethoxysilane were added into the reactor in a ratio of 1g:20mL:4g and stirred. The temperature of the reactor was raised to 60°C and kept for 8h. Activated CNTs / TiO2-CuO was obtained by post-treatment.

[0136] S3. Preparation of modified cation exchange membrane precursor

[0137] Add activated CNTs / TiO2-CuO and 20 wt% polyvinylidene chloride solution into a reactor, raise the temperature of the reactor to 40°C, set the frequency to 80 kHz, keep the temperature and perform ultrasonic treatment for 2 hours, filter, and place the filter cake in a drying oven at 80°C and vacuum dry to constant weight to obtain modified polyvinylidene chloride;

[0138] The modified polyvinylidene chloride is soaked in a 50wt% sulfuric acid solution and a 5wt% hydrogen peroxide solution, wherein the modified polyvinylidene chloride, the 50wt% sulfuric acid solution and the 5wt% hydrogen peroxide solution are used in a ratio of 1g:4mL:1mL, the soaking temperature is 80°C, the temperature is kept for 4h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain sulfonated polyvinylidene chloride;

[0139] Soaking sulfonated polyvinylidene chloride in 30wt% sodium hydroxide solution and 50wt% ammonia solution, wherein the amount ratio of sulfonated polyvinylidene chloride, 30wt% sodium hydroxide solution and 50wt% ammonia solution is 1g:1mL:4mL, the soaking temperature is 50°C, the temperature is kept for 4h, and the filter cake is placed in a drying oven at 80°C and vacuum dried to constant weight to obtain sulfonated polyvinylidene chloride, and the sulfonated polyvinylidene chloride is dissolved in ethylene glycol monomethyl ether acetate to prepare a sulfonated polyvinylidene chloride solution;

[0140] A glass fabric with a thickness of 0.75 mm and a 5 wt% silane coupling agent solution are placed in a stirring kettle for reaction, wherein the glass fabric with a thickness of 0.75 mm and the 5 wt% silane coupling agent are used in a ratio of 1 g:5 mL, the temperature is set to 80° C., the reaction is kept warm for 3 hours, the stirring rate is 120 rpm, and after the reactor is cooled to room temperature, the silanized glass fabric precursor is taken out, rinsed with cold ethanol at a temperature of 10° C. for 5 times, and then placed in a drying oven and vacuum baked at 120° C. for 2 hours to obtain the silanized glass fabric;

[0141] The sulfonated polyvinylidene chloride solution was spin-coated on the surface of the silanized glass fabric to form a coating with a thickness of 175 μm to obtain a coated glass fabric, and the coated glass fabric was placed in a drying oven at 80° C. for vacuum heat treatment for 1 h to obtain a modified glass fabric;

[0142] The modified glass fabric was immersed in a 30wt% glutaraldehyde solution, wherein the amount ratio of the modified glass fabric to the 30wt% glutaraldehyde solution was 1g:5mL, the immersion temperature was 50°C, and the reaction was kept warm for 5h. The modified glass fabric was taken out and placed in a drying oven at 80°C for vacuum drying to constant weight to obtain a modified cation exchange membrane precursor.

[0143] S4. Preparation of modified anion exchange cation precursor

[0144] Activated CNTs / TiO2-CuO and 20wt% polyethersulfone solution were added into the reactor at a dosage ratio of 1g:10ml, the temperature of the reactor was raised to 40°C, the frequency was set to 80kHz, the temperature was kept and ultrasonicated for 2h, and the filter cake was placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a composite polyethersulfone membrane;

[0145] The composite polyethersulfone membrane was immersed in 10wt% methyl chloride and 30wt% aluminum chloride, wherein the amount ratio of the composite polyethersulfone, 10wt% methyl chloride and 30wt% aluminum chloride was 1g:5mL:3mL, the immersion temperature was 70°C, the reaction time was 3h, and the filter cake was placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a halomethylated membrane;

[0146] The halogenated membrane was immersed in a 30 wt% trimethylamine solution, wherein the ratio of the halogenated membrane to the 30 wt% trimethylamine solution was 1 g:5 mL, the immersion temperature was 60°C, the reaction was kept warm for 4 hours, and the filter cake was placed in a drying oven at 80°C and vacuum dried to constant weight to obtain a modified anion exchange membrane precursor.

[0147] S5. Chemical plating

[0148] Mix nickel chloride, sodium hypophosphite, sodium citrate, sodium dodecylbenzene sulfonate, sodium thiosulfate, sodium acetate and deionized water in a weight ratio of 5:10:12:0.2:0.1:0.1:60 to prepare a chemical plating solution;

[0149] The modified cation exchange membrane precursor and the modified anion exchange membrane precursor were placed in a chemical plating solution and plated at 40°C for 2 hours. After the plating was completed, the plated ion exchange membrane was rinsed with deionized water to neutrality to obtain a modified ion exchange membrane.

[0150] S6. Electrodialysis

[0151] The cation exchange membrane and the anion exchange membrane were assembled into an electrodialysis device, the voltage of the electrodialysis device was set to 80 V, ozone was introduced into the ion exchange membrane at a rate of 10 L / h, the electrodialysis time was set to 7 h, and after the electrodialysis water and the salt solution were taken out, the electrodialysis water was repeated for 3 times to obtain a high salt solution and dischargeable water after concentration.

[0152] Comparative Example 1

[0153] The difference between this comparative example and Example 3 is that the high-salt and high-organic matter solution is pretreated by adding 1 g / L of polyaluminium chloride as a flocculant into the wastewater, allowing it to stand for 0.5 h, and filtering it with activated carbon.

[0154] Comparative Example 2

[0155] The difference between this comparative example and Example 3 is that step S2 is omitted, and the use of activated CNTs / TiO2-CuO in the subsequent steps is omitted.

[0156] Comparative Example 3

[0157] The difference between this comparative example and Example 3 is that in step S3, the glass fabric modification process is cancelled and the glass fabric is not used as a matrix for modified cation exchange.

[0158] According to the standard GB 8978-1996 "Comprehensive Standard for Sewage Discharge", the dischargeable water obtained from Examples 1-3 and Comparative Examples 1-2 was tested: after repeated electrodialysis operations were performed on the ion exchange membranes obtained in Example 3 and Comparative Example 3, different batches of dischargeable water were inspected according to the standard GB 8978-1996 "Comprehensive Standard for Sewage Discharge", and the inspection data results are shown in Table 1-2.

[0159] Table 1-Dischargeable water content test data table

[0160]

[0161]

[0162] Table 2-Ion exchange membrane cycle electrodialysis test data table

[0163]

[0164]

[0165] Data Analysis:

[0166] By analyzing the data in Table 1 above, in the method for treating high-concentration salt-containing organic wastewater, by comparing Example 3 with Comparative Example 1, it can be found that, compared with directly using a flocculant for treatment, the pretreatment method of the present invention is more sufficient for separating organic matter;

[0167] By comparing Example 3 with Comparative Example 2, it can be found that using activated CNTs / TiO2-CuO to treat the ion exchange membrane can effectively promote the oxidation of organic matter by the oxidant during the electrodialysis process and thus meet the emission standards;

[0168] Analyzing the data in Table 2 above, the use of silanized glass fabric in the preparation of ion exchange membranes can still effectively separate the components of wastewater after ten electrodialysis treatments.

[0169] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for treating high-concentration saline organic wastewater, characterized in that: The following steps are involved: S1, pre-treating the high-salt organic solution to obtain a low-salt and low-organic solution; S2, assembling the modified cation exchange membrane and the modified anion exchange membrane into an electrodialysis device, and using the electrodialysis device to treat the high-salt and low-organic solution to obtain a high-salt solution and dischargeable water; The preparation method of the modified cation exchange membrane is as follows: activated CNTs / TiO2-CuO and 10-20wt% polyvinylidene chloride solution are added to a reactor and stirred, the temperature of the reactor is increased to 30-40°C, the reactor is kept warm and ultrasonicated for 1-2h, post-processed to obtain modified polyvinylidene chloride, the modified polyvinylidene chloride is coupled and modified to obtain a modified cation exchange membrane precursor, and the modified cation exchange membrane precursor is plated with a chemical plating solution to obtain a modified cation exchange membrane; The preparation method of the modified anion exchange membrane is as follows: activated CNTs / TiO2-CuO and 10-20wt% polyethersulfone solution are added into a reactor and stirred, the temperature of the reactor is increased to 30-40°C, and the reactor is kept warm and ultrasonicated for 1-2h, a composite polyethersulfone membrane is obtained by post-treatment, the composite polyethersulfone membrane is modified to obtain a modified anion exchange membrane precursor, and the modified anion exchange membrane precursor is plated with a chemical plating solution to obtain a modified anion exchange membrane.

2. The method for treating high-concentration saline organic wastewater according to claim 1, characterized in that: In step S1, the pre-processing operation includes the following steps: A1. Add high-salt organic solution and deionized water into a reactor and stir for 5-15 minutes at room temperature to obtain a diluted solution; A2. Lower the temperature of the reactor containing the diluted solution to 0-5°C, stir for 3-5 hours, and filter to obtain inorganic salt crystals and a low-salt, high-organic matter solution; A3. Add the low-salt high-organic matter solution and the extract into a reaction kettle and stir. Stir for 20-30 minutes at room temperature. Allow to stand and separate the liquids to obtain an organic solution and a low-salt low-organic matter solution.

3. The method for treating high-concentration saline organic wastewater according to claim 2, characterized in that: In step A1, the volume ratio of deionized water to high-salt organic solution is 2:1, and the stirring rate is 120 rpm; in step A3, the extractant is one or more of ethyl acetate, dichloromethane, and ether, the volume ratio of the extractant to the mixed solution is 0.5:1, and the stirring rate is 120 rpm.

4. The method for treating high-concentration saline organic wastewater according to claim 1, characterized in that: Activated CNTs / TiO2-CuO was prepared by the following steps: B1, adding single-walled carbon nanotubes, amide compounds and dichloromethane into a reactor, raising the temperature of the reactor to 40-60°C, keeping the temperature for 6-8h, and post-treating to obtain modified carbon nanotubes; B2, mixing nano-TiO2, nano-CuO and modified carbon nanotubes in N,N-dimethylformamide to obtain a mixed solution, adding the mixed solution to an ultrasonic device for ultrasonication, the ultrasonic device is set at 60-80°C, the frequency is 40-60kHz, the temperature is kept for reaction for 3-5h, and post-processing is performed to obtain CNTs / TiO2-CuO; B3. Add CNTs / TiO2-CuO, silane coupling agent and organic solvent into a reactor and stir. Raise the temperature of the reactor to 40-60°C and keep the reaction for 6-8h. Post-treat to obtain activated CNTs / TiO2-CuO.

5. The method for treating high-concentration saline organic wastewater according to claim 1, characterized in that: The amount ratio of activated CNTs / TiO2-CuO and 10-20wt% polyvinylidene chloride solution is 1g:10ml, and the ultrasonic frequency is 20-80kHz; the coupling modification of the modified polyvinylidene chloride includes the following steps: C1, soaking the modified polyvinylidene chloride in a mixed solution consisting of 30-50wt% sulfuric acid solution and 1-5wt% hydrogen peroxide solution, the mixed solution temperature is 60-80°C, and the mixture is soaked for 2-4 hours, and post-processed to obtain sulfonated polyvinylidene chloride; C2, soaking the sulfonated polyvinylidene chloride in a mixed solution consisting of 20-30wt% sodium hydroxide solution and 30-50wt% ammonia solution, the mixed solution temperature is 30-50°C, and the mixture is soaked for 2-4h, post-processed to obtain sulfonated polyvinylidene chloride, and the sulfonated polyvinylidene chloride is dissolved in ethylene glycol monomethyl ether acetate to prepare a sulfonated polyvinylidene chloride solution; C3, spin coating the sulfonated polyvinylidene chloride solution on the surface of the silanized glass fabric to form a coating with a thickness of 150-200 μm to obtain a coated glass fabric, placing the coated glass fabric in a drying oven at 80° C. for vacuum heat treatment for 1 h to obtain a modified glass fabric; C4, immersing the modified glass fabric in a 20-30wt% glutaraldehyde solution at a soaking temperature of 40-50°C, keeping the solution warm for 3-5h, and post-treating to obtain a modified cation exchange membrane precursor.

6. The method for treating high-concentration saline organic wastewater according to claim 5, characterized in that: The silanized glass fabric is prepared by the following steps: a glass fabric with a thickness of 0.05-0.10 mm and a 0.5-5wt% silane coupling agent solution are placed in a stirring kettle and stirred, the temperature of the reaction kettle is increased to 60-80°C, the stirring rate is set to 120rpm, and the reaction is kept warm for 2-3 hours. After the reaction is completed, the reaction kettle is cooled to room temperature, the silanized glass fabric precursor is taken out, rinsed with cold ethanol at a temperature of 10°C for 3-5 times, and then placed in a drying oven and vacuum baked at 110-120°C for 1-2 hours to obtain the silanized glass fabric.

7. The method for treating high-concentration saline organic wastewater according to claim 1, characterized in that: The activated CNTs / TiO2-CuO and 10-20wt% polyethersulfone solution are used in a ratio of 1g:10ml, and the ultrasonic frequency is 20-80kHz; the modification treatment of the composite polyethersulfone membrane includes the following steps: D1, soaking the composite polyethersulfone membrane in 5-10wt% methyl chloride and 20-30wt% aluminum chloride at a temperature of 50-70°C, keeping the temperature for reaction for 1-3h to obtain an impregnated membrane, and post-treating to obtain a halogenated membrane; D2. Soak the halogenated membrane in a 20-30wt% trimethylamine solution at a soaking temperature of 40-60°C, keep the solution warm for 2-4 hours, and post-treat to obtain a modified anion exchange membrane precursor.

8. The method for treating high-concentration saline organic wastewater according to claim 1, characterized in that: The plating includes the following steps: placing the membrane substrate in a chemical plating solution, keeping the plating at a temperature of 20-40°C for 1-2 hours, and after the plating is completed, using deionized water to rinse the plated ion exchange membrane to neutrality to obtain a modified ion exchange membrane, wherein the membrane substrate is a modified cation exchange membrane precursor or a modified anion exchange membrane precursor.

9. The method for treating high-concentration saline organic wastewater according to claim 1, characterized in that: In step S2, the wastewater treatment includes the following steps: setting the voltage of the electrodialysis equipment to 20-80V, introducing ozone into the ion exchange membrane at a rate of 10L / h, setting the electrodialysis time to 6-7h, taking out the electrodialysis water and the salt solution, repeating the electrodialysis operation 2-3 times, and concentrating them to obtain a high salt solution and dischargeable water.

Citation Information

Patent Citations

  • Method for preparing carbon nano tube modified bipolar membrane with anion groups

    CN102580549A

  • Treatment system for sodium bromide wastewater

    CN214141976U

  • Filter

    DE202023105704U1

Cited By

  • Cationic electrodialysis membrane and preparation method thereof

    CN119951332A

  • A cationic electrodialysis membrane and its preparation method

    CN119951332B